A kind of Cr-Mo alloy steel resistant to hydrogen embrittlement and preparation method thereof

By adding a specific proportion of microalloy elements such as Se, Cu, Nb, W and RE to Cr-Mo alloy steel and performing tempering treatment to form a nano-scale precipitation phase, the Cr-Mo alloy steel is solved under a high-pressure hydrogen environment. The anti-hydrogen embrittlement problem significantly improves the anti-hydrogen embrittlement and mechanical properties of the material, extends the service life and ensures safety.

CN118814074BActive Publication Date: 2024-11-29UNIV OF SCI & TECH BEIJING
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411295809.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-29
Estimated Expiration
2044-09-18

AI Technical Summary

Technical Problem

Conventional Cr-Mo alloy steels are prone to high-pressure hydrogen embrittlement in high-pressure hydrogen environments, resulting in reduced material toughness, accelerated fatigue crack propagation rate, and reduced critical crack threshold value, affecting the safe use of hydrogen storage and transportation equipment.

Method used

Micro-microphones such as 0.01%~0.1% Se, 0.02%~0.1% Cu, 0.01%~0.04% Nb, 0.3%~1.1% W, and 0.006%~0.009% RE, etc., are added to Cr-Mo alloy steel, such as micro- Alloy elements satisfy the component ratio of 1.3≤Cu/Nb≤2 and 0.5≤Se/Cu≤1.2, and carry out appropriate tempering treatment to form nano-scale precipitation phases to improve grain boundary stability and hydrogen trap density, and enhance resistance. Hydrogen embrittlement properties.

Benefits of technology

It significantly improves the hydrogen embrittlement resistance and mechanical properties of Cr-Mo alloy steel, extends the service life of hydrogen-prone materials, and ensures safety and reliability in high-pressure hydrogen environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118814074B_ABST
    Figure CN118814074B_ABST
Patent Text Reader

Abstract

The present invention relates to a hydrogen embrittlement resistant Cr-Mo alloy steel and a preparation method thereof, and belongs to the technical field of alloy materials. The Cr-Mo alloy steel comprises the following mass percentage components: C, 0.28-0.33%; Si, 0.2-0.35%; Mn, 0.5-0.8%; P≤0.02%; S≤0.01%; Se, 0.01-0.1%; Ni, 0.15-0.25%; Cr, 0.9-1.1%; Mo, 0.17-0.25%; Al, 0.02-0.06%; Cu, 0.02-0.1%; Nb, 0.01-0.04%; W, 0.3-1.1%; RE, 0.006-0.009%; the rest are Fe and impurities; and satisfy 1.3≤Cu / Nb≤2, 0.5≤Se / Cu≤1.2. The present invention obtains a Cr-Mo alloy steel having both strong toughness and excellent hydrogen embrittlement resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy materials, and in particular relates to a hydrogen embrittlement resistant Cr-Mo alloy steel and a preparation method thereof. Background Art

[0002] As a secondary energy with abundant sources, green and low carbon, and wide applications, hydrogen energy has become a strategic emerging industry in my country's energy system. my country has made a comprehensive layout in basic research, applied research, and demonstration applications, covering four links: hydrogen production, storage, transportation, and use. At present, the pressure hydrogen materials used at home and abroad are mainly Cr-Mo steel, 6061 aluminum alloy, and 316L stainless steel. However, due to factors such as cost, process, and specific needs, hydrogen storage containers and long-tube trailers used in domestic hydrogen refueling stations all use Cr-Mo steel. However, conventional Cr-Mo alloy steel materials may suffer from high-pressure hydrogen embrittlement in a high-pressure hydrogen environment, which is mainly manifested in the degradation of mechanical properties such as reduced material toughness, accelerated fatigue crack growth rate, and reduced critical cracking threshold value, which poses a threat to the safe use of high-pressure hydrogen storage and transportation equipment. Safe, energy-saving, and efficient hydrogen transportation construction is an important research direction for the current development of hydrogen energy. The study of material failure behavior in a high-pressure hydrogen environment has important practical significance for ensuring the safety of hydrogen energy transportation.

[0003] Therefore, there is an urgent need to provide a Cr-Mo alloy steel with both strength, toughness and resistance to hydrogen embrittlement and a preparation method thereof, which has important engineering value for improving the service life of hydrogen-exposed materials. Summary of the invention

[0004] In order to solve one or more technical problems existing in the prior art, the present invention provides a hydrogen embrittlement resistant Cr-Mo alloy steel and a preparation method thereof.

[0005] In a first aspect, the present invention provides a hydrogen embrittlement resistant Cr-Mo alloy steel, wherein the hydrogen embrittlement resistant Cr-Mo alloy steel comprises the following components in mass percentage: C, 0.28% to 0.33%; Si, 0.2% to 0.35%; Mn, 0.5% to 0.8%; P≤0.02%; S≤0.01%; Se, 0.01% to 0.1%; Ni, 0.15% to 0.25%; Cr, 0.9% to 1.1%; Mo, 0.17% to 0.25%; Al, 0.02% to 0.06%; Cu, 0.02% to 0.1%; Nb, 0.01% to 0.04%; W, 0.3% to 1.1%; rare earth RE, 0.006% to 0.009%; the rest is Fe and unavoidable impurities;

[0006] And satisfy the following equations (1) and (2):

[0007] 1.3≤Cu / Nb≤2 Formula (1);

[0008] 0.5≤Se / Cu≤1.2 Formula (2);

[0009] In formula (1) and formula (2), each component symbol represents the mass percentage of each component.

[0010] Preferably, the mass percentages of Nb and W components in the hydrogen embrittlement resistant Cr-Mo alloy steel satisfy the following formula (3):

[0011] 0.56%≤4Nb+W≤1.1% Formula (3);

[0012] In formula (3), each component symbol represents the mass percentage of each component.

[0013] Preferably, the rare earth RE is La and Ce, and the mass ratio of La to Ce is (4-6): (4-6).

[0014] Preferably, in the hydrogen embrittlement resistant Cr-Mo alloy steel, the mass percentage of W is 0.5-0.9%.

[0015] Preferably, the yield strength of the hydrogen embrittlement resistant Cr-Mo alloy steel is not less than 666 MPa, the tensile strength is not less than 745 MPa, the room temperature elongation is not less than 14.2%, and the hydrogen embrittlement sensitivity index HEI is not greater than 9.3%.

[0016] In a second aspect, the present invention provides a method for preparing the hydrogen embrittlement resistant Cr-Mo alloy steel according to the first aspect of the present invention, the preparation method comprising the following steps:

[0017] (1) Smelting the raw materials for preparing hydrogen embrittlement resistant Cr-Mo alloy steel in a vacuum induction furnace to obtain a steel ingot;

[0018] (2) After forging, the steel ingot is rolled and tempered in sequence to produce hydrogen embrittlement-resistant Cr-Mo alloy steel.

[0019] Preferably, the initial forging temperature of the forging is 1050°C to 1150°C, and the final forging temperature is 850°C to 900°C.

[0020] Preferably, before the rolling, the steel is preheated to 1050-1150° C. and kept at 1050-1150° C. for 30-90 min.

[0021] Preferably, the starting rolling temperature is 1000°C to 1100°C, and the final rolling temperature is 850°C to 950°C.

[0022] Preferably, the quenching and tempering treatment is first quenching at 850°C to 910°C for 30 to 60 minutes, and then tempering at 670°C to 730°C for 60 to 120 minutes.

[0023] Compared with the prior art, the present invention has at least the following beneficial effects:

[0024] (1) In the hydrogen embrittlement resistant Cr-Mo alloy steel material prepared by the present invention, a variety of micro-alloying elements such as 0.01%~0.1% Se, 0.02%~0.1% Cu, 0.01%~0.04% Nb, 0.3%~1.1% W and 0.006%~0.009% RE are added through composite regulation, and at the same time, 1.3≤Cu / Nb≤2 and 0.5≤Se / Cu≤1.2 are satisfied, which is conducive to obtaining Cr-Mo alloy steel with both strong toughness and excellent hydrogen embrittlement resistance. This has important engineering application value for improving the service life of hydrogen materials, and also lays a good foundation for the development, production and application of a new generation of hydrogen resistant Cr-Mo alloy steel.

[0025] (2) The present invention finds that the addition of Se can form a second phase and improve the stability of the grain boundary, thereby reducing the diffusion rate of hydrogen in the matrix and slowing down the penetration of hydrogen into the material. The addition of Cu can optimize the grain boundary characteristics and adjust the ratio of small-angle grain boundaries to large-angle grain boundaries. On the other hand, it can also form a Cu nano-precipitate phase, which increases the density of deep hydrogen traps and is beneficial to reducing the hydrogen diffusion coefficient. The combination of Se and Cu in an appropriate ratio can further optimize the hydrogen retardation effect while ensuring that the mechanical properties of Cr-Mo alloy steel remain within an ideal range. Controlling their reasonable ratio can effectively improve the hydrogen retardation effect and enhance the stability of the grain boundary, and can make the density of the formed Cu nano-precipitate phase larger, and can effectively avoid the excessive size of the formed hydrogen traps, thereby effectively achieving the desired effect. Improve the hydrogen embrittlement resistance of Cr-Mo alloy steel; in addition, the present invention finds that Cu, Nb and W can all form nano-sized precipitated phases, and the coordinated use of the three can more effectively improve the hydrogen capture efficiency of grain boundaries and hydrogen traps. In order to reasonably control the size of the nano-precipitated phase and effectively ensure the toughness and hydrogen embrittlement resistance of Cr-Mo alloy steel, the contents of the three must be controlled within a reasonable range, especially the element content ratio of Cu and Nb needs to be controlled within 1.3≤Cu / Nb≤2, which is beneficial to significantly improve the hydrogen embrittlement resistance of Cr-Mo alloy steel. In some preferred technical schemes, the element content ratio of Nb and W is more preferably controlled to 0.56%≤4Nb+W≤1.1%, which is beneficial to further improve the hydrogen embrittlement resistance of Cr-Mo alloy steel.

[0026] (3) When preparing hydrogen embrittlement resistant Cr-Mo alloy steel, the present invention preferably performs a suitable quenching and tempering process, which is beneficial to obtaining a large number of dispersed deep hydrogen traps, which is also beneficial to improving the hydrogen embrittlement resistance of the Cr-Mo alloy steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1is the metallographic structure diagram of the hydrogen embrittlement resistant Cr-Mo alloy steel in Example 1 of the present invention;

[0028] Figure 2 It is a transmission electron microscope image of the nano-precipitated phase in the hydrogen embrittlement resistant Cr-Mo alloy steel in Example 1 of the present invention. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In a first aspect, the present invention provides a hydrogen embrittlement resistant Cr-Mo alloy steel (also referred to as hydrogen embrittlement resistant Cr-Mo low alloy steel), wherein the hydrogen embrittlement resistant Cr-Mo alloy steel comprises the following components in percentage by mass: C (carbon), 0.28% to 0.33%; Si (silicon), 0.2% to 0.35%; Mn (manganese), 0.5% to 0.8%; P (phosphorus) ≤ 0.02%; S (sulfur) ≤ 0.01%; Se (selenium), 0.01% to 0.1%; Ni (nickel), 0.15% to 0.25%; Cr (chromium), 0.9% to 1.1%; Mo (molybdenum), 0.17% to 0.25%; Al (aluminum), 0.02% to 0.06%; Cu (copper), 0.02%~0.1%; Nb (niobium), 0.01%~0.04%; W (tungsten), 0.3%~1.1%; rare earth RE, 0.006%~0.009%; the rest is Fe and inevitable impurities; in the present invention, the rare earth RE is, for example, La (lanthanum) and / or Ce (cerium); in the present invention, the sum of the mass percentages of the inevitable impurities in the hydrogen embrittlement resistant Cr-Mo alloy steel is less than 1%; in the present invention, the sum of the mass percentages of each component is 100%; in the present invention, the mass percentages of Se, Cu and Nb components in the hydrogen embrittlement resistant Cr-Mo alloy steel satisfy the following formula (1) and the following formula (2):

[0031] 1.3≤Cu / Nb≤2 Formula (1);

[0032] 0.5≤Se / Cu≤1.2 Formula (2);

[0033] In formula (1) and formula (2), each component symbol represents the mass percentage (mass percentage content) of each component.

[0034] In the hydrogen embrittlement resistant Cr-Mo alloy steel material prepared by the present invention, multiple micro-alloying elements such as 0.01%-0.1% Se, 0.02%-0.1% Cu, 0.01%-0.04% Nb, 0.3%-1.1% W and 0.006%-0.009% RE are added by composite regulation, and 1.3≤Cu / Nb≤2 and 0.5≤Se / Cu≤1.2 are satisfied at the same time, which is conducive to obtaining Cr-Mo alloy steel with both high toughness and excellent hydrogen embrittlement resistance, which has important engineering application value for improving the service life of hydrogen materials, and also lays a good foundation for the development, production and application of a new generation of hydrogen resistant Cr-Mo alloy steel; in the present invention, the addition of Nb can promote the refinement of the microstructure, and can improve the strength and toughness at the same time, And Nb can form NbC nano-precipitation phase, and strengthen the matrix through the precipitation phase, but when the content of Nb exceeds a certain range, it is not conducive to the toughness of the steel. Therefore, the content of Nb in the present invention is controlled at 0.01%~0.04%. The addition of W can increase the content of ferrite and form WC nano-precipitation phase at the same time. However, excessive addition of W element will lead to an increase in dislocation density, which is not conducive to the capture and fixation of hydrogen. Therefore, the content of W in the present invention is controlled at 0.3%~1.1%. The addition of rare earth element RE can modify the inclusions in the steel, reduce the content of inclusions such as MnS and Al2O3 that promote hydrogen cracking, thereby reducing the sensitivity to hydrogen embrittlement. However, too much RE may affect the processing performance. Therefore, the content of RE in the present invention is controlled at 0.006%~0.009%.Particularly, the present invention finds that the addition of Se can form a second phase and improve the stability of the grain boundary, thereby reducing the diffusion rate of hydrogen in the matrix and slowing down the penetration of hydrogen inside the material. The addition of Cu can optimize the grain boundary characteristics and adjust the ratio of small-angle grain boundaries to large-angle grain boundaries on the one hand, and can also form a Cu nano-precipitated phase on the other hand, increasing the density of deep hydrogen traps, which is beneficial to reducing the hydrogen diffusion coefficient. The combination of Se and Cu in an appropriate ratio can further optimize the hydrogen retardation effect, while ensuring that the mechanical properties of the Cr-Mo alloy steel remain within an ideal range. Controlling their reasonable ratio can improve the hydrogen retardation effect and enhance the stability of the grain boundary, and can make the density of the formed Cu nano-precipitated phase larger, and can effectively avoid the excessive size of the formed hydrogen traps, thereby Effectively improve the hydrogen embrittlement resistance of Cr-Mo alloy steel; in addition, the present invention finds that Cu, Nb and W can all form nano-sized precipitated phases, and the coordinated use of the three can more effectively improve the hydrogen capture efficiency of grain boundaries and hydrogen traps. In order to reasonably control the size of the nano-precipitated phase and effectively ensure the toughness and hydrogen embrittlement resistance of Cr-Mo alloy steel, the contents of the three must be controlled within a reasonable range, especially the element content ratio of Cu and Nb needs to be controlled within 1.3≤Cu / Nb≤2, which is beneficial to significantly improve the hydrogen embrittlement resistance of Cr-Mo alloy steel. In some preferred technical schemes, the element content ratio of Nb and W is more preferably controlled to 0.56%≤4Nb+W≤1.1%, which is beneficial to further improve the hydrogen embrittlement resistance of Cr-Mo alloy steel.

[0035] In the present invention, it is very important to reasonably control the contents of Se and Cu and maintain the Se / Cu ratio in the range of 0.5 to 1.2 to improve the hydrogen embrittlement resistance of Cr-Mo alloy steel; by optimizing the grain boundary structure and forming an effective hydrogen trap, Se and Cu can synergistically improve the hydrogen embrittlement resistance and toughness of the material. However, excessive or insufficient Se and Cu, as well as an unreasonable Se / Cu ratio, will destroy this balance, resulting in a decrease in the mechanical properties and hydrogen embrittlement resistance of the material. The present invention finds that if the Se content exceeds 0.1%, excessive Se compounds may be formed on the grain boundaries. The presence of these brittle phases will significantly reduce the ductility and toughness of the material, making it more susceptible to brittle fracture. If the Se content is less than 0.01%, its effect on regulating the grain boundaries is insufficient, and the aggregation and diffusion of hydrogen cannot be effectively reduced, resulting in an insignificant effect on improving the hydrogen embrittlement resistance. If the Cu content exceeds 0.1%, the Se content will not be significantly reduced. When the Se / Cu content is less than 0.1%, excessive Cu nano-precipitates may be formed. Although these precipitates can increase the hydrogen trap density, excessive Cu nano-precipitates may form stress concentration areas at the grain boundaries, reduce the ductility of the material, and increase the risk of brittle fracture. If the Cu content is lower than 0.02%, sufficient Cu nano-precipitates cannot be formed, which will reduce the ability to capture hydrogen and result in an insignificant improvement in hydrogen embrittlement resistance. In addition, if the Se / Cu ratio is greater than 1.2, the Se content is relatively high, while the Cu content is relatively insufficient, the regulation effect of Se will exceed the optimization effect of Cu, resulting in grain boundary embrittlement, and the material's hydrogen embrittlement resistance and toughness will both decrease. If the Se / Cu ratio is less than 0.5, the Cu content is relatively high, while the Se content is relatively insufficient, excessive Cu nano-precipitates will result, grain boundary stress concentration, increased brittleness of the material, and the material's hydrogen embrittlement resistance and toughness will also decrease.

[0036] According to some preferred embodiments, the mass percentages of Nb and W components in the hydrogen embrittlement resistant Cr-Mo alloy steel satisfy the following formula (3):

[0037] 0.56%≤4Nb+W≤1.1% Formula (3);

[0038] In formula (3), each component symbol represents the mass percentage of each component; in the present invention, it is preferred to control the element content ratio of Nb and W to 0.56%≤4Nb+W≤1.1%, which is beneficial to further improve the hydrogen embrittlement resistance of Cr-Mo alloy steel.

[0039] According to some preferred embodiments, the rare earth RE is La and Ce, and the mass ratio of La to Ce is (4-6): (4-6).

[0040] According to some preferred embodiments, in the hydrogen embrittlement resistant Cr-Mo alloy steel, the mass percentage of W is 0.5-0.9%.

[0041] According to some preferred embodiments, the hydrogen embrittlement resistant Cr-Mo alloy steel comprises the following mass percentage components: C, 0.28%~0.33%; Si, 0.2%~0.35%; Mn, 0.5%~0.8%; P≤0.02%; S≤0.01%; Se, 0.02%~0.08%; Ni, 0.15%~0.25%; Cr, 0.9%~1.1%; Mo, 0.17%~0.25%; Al, 0.02%~0.06%; Cu, 0.02%~0.06%; Nb , 0.01%~0.04%; W, 0.5%~0.9%; rare earth RE, 0.006%~0.009%; the rest are Fe and unavoidable impurities; and the mass percentages of Cu and Nb components satisfy 1.3≤Cu / Nb≤2, the mass percentages of Se and Cu components satisfy 0.5≤Se / Cu≤1.2, the mass percentages of Nb and W components satisfy 0.56%≤4Nb+W≤1.1%, the rare earth REs are La and Ce, and the mass fraction ratio of La and Ce is (4~6): (4~6).

[0042] According to some preferred embodiments, the yield strength of the hydrogen embrittlement resistant Cr-Mo alloy steel is not less than 666 MPa, the tensile strength is not less than 745 MPa, the room temperature elongation is not less than 14.2%, and the hydrogen embrittlement sensitivity index HEI (A%) is not greater than 9.3%.

[0043] According to some preferred embodiments, the yield strength of the hydrogen embrittlement resistant Cr-Mo alloy steel is not less than 700 MPa, the tensile strength is not less than 780 MPa, the room temperature elongation is not less than 14.5%, and the hydrogen embrittlement sensitivity index HEI (A%) is not greater than 8.5%.

[0044] According to some preferred embodiments, the metallographic structure of the hydrogen embrittlement resistant Cr-Mo alloy steel is tempered troostite, for example Figure 1 As shown, it includes a ferrite matrix and carbides, wherein the grain size of the ferrite is ≥10 levels. Tempered bainite is an equilibrium structure with relatively small internal stress, and the ferrite grains in the tempered bainite structure are fine, with good toughness and low hardness, and have good resistance to hydrogen embrittlement. When the metallographic structure is not tempered bainite, the hydrogen embrittlement resistance will be reduced. For example, if the metallographic structure is not tempered bainite, but a hard phase structure such as granular bainite, lath bainite or martensite, the dislocation density is large, the internal stress is large, and the hardness is high. Such a structure is very prone to hydrogen embrittlement fracture. In the present invention, the microstructure of the hydrogen embrittlement-resistant Cr-Mo alloy steel contains a large number of dispersedly distributed NbC, WC, and Cu nano-precipitates. For example, Figure 2 As shown, the dispersed nano-precipitated phase can capture fixed hydrogen, thereby reducing the apparent hydrogen concentration and reducing the sensitivity to hydrogen embrittlement.

[0045] In a second aspect, the present invention provides a method for preparing the hydrogen embrittlement resistant Cr-Mo alloy steel according to the first aspect of the present invention, the preparation method comprising the following steps:

[0046] (1) The raw materials for preparing hydrogen embrittlement resistant Cr-Mo alloy steel are smelted in a vacuum induction furnace to obtain a steel ingot; in the present invention, the smelting temperature is not less than 1650° C., preferably, the smelting temperature is 1650-1700° C., and the smelting time is 10-30 min;

[0047] (2) After forging the steel ingot, rolling and tempering treatment are performed in sequence to obtain hydrogen embrittlement resistant Cr-Mo alloy steel; in the present invention, after forging, slow cooling (i.e., furnace cooling) is adopted for cooling, and then the rolling is performed; the hydrogen embrittlement resistant Cr-Mo alloy steel obtained by the present invention is suitable for use in hydrogen energy transportation systems, and specifically, can be used in key equipment of the hydrogen energy transportation system, for example, can be used in hydrogen storage containers and hydrogen transmission pipelines; the present invention does not make specific limitations on the operations such as smelting, forging and rolling, and those skilled in the art can make conventional selections.

[0048] According to some preferred embodiments, the initial forging temperature of the forging is 1050°C to 1150°C, and the final forging temperature is 850°C to 900°C.

[0049] According to some preferred embodiments, before the rolling, the process is preheated to 1050-1150° C. and kept at 1050-1150° C. for 30-90 min.

[0050] According to some preferred embodiments, the starting rolling temperature is 1000°C to 1100°C, and the final rolling temperature is 850°C to 950°C; in the present invention, the pressing amount (pressing rate) of the rolling is, for example, 65% to 70%.

[0051] According to some preferred embodiments, the quenching and tempering treatment is first quenching at 850°C~910°C for 30~60min, and after quenching, the cooling method adopted is water cooling and / or oil cooling, and then tempering at 670°C~730°C for 60~120min. After tempering, the cooling method adopted is air cooling; when preparing hydrogen embrittlement-resistant Cr-Mo alloy steel, the present invention preferably performs a suitable quenching and tempering treatment process, which is beneficial to obtain a large number of dispersed deep hydrogen traps, which is also beneficial to improving the hydrogen embrittlement resistance of Cr-Mo alloy steel; the present invention does not make specific limitations on the slow cooling, water cooling, oil cooling and air cooling, which are conventional technologies in the field. In the present invention, whether the cooling method is slow cooling, water cooling, oil cooling or air cooling, it is cooled to room temperature.

[0052] The present invention will be further described below by way of examples, but the protection scope of the present invention is not limited to these embodiments.

[0053] Example 1

[0054] The present embodiment provides a hydrogen embrittlement resistant Cr-Mo alloy steel, which contains the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.04%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%; Nb, 0.03%; W, 0.5%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=1.33, Se / Cu=1, 4Nb+W=0.62%.

[0055] The metallographic structure diagram of the hydrogen embrittlement resistant Cr-Mo alloy steel of this embodiment is as follows: Figure 1 As shown in FIG. 1 , the metallographic structure of the hydrogen embrittlement resistant Cr-Mo alloy steel is tempered troostite; the transmission electron microscope image of the nano-precipitated phase in the hydrogen embrittlement resistant Cr-Mo alloy steel of this embodiment is as shown in FIG. Figure 2 As shown, NbC, WC, and Cu nano-precipitates are dispersed in the microstructure of the hydrogen embrittlement resistant Cr-Mo alloy steel.

[0056] In this embodiment, the preparation of the hydrogen embrittlement resistant Cr-Mo alloy steel is as follows: the raw materials for preparing the hydrogen embrittlement resistant Cr-Mo alloy steel are added into a vacuum induction furnace according to the above ratio for smelting, and the vacuum is evacuated to 2.5×10 -3 Pa, then fill with argon to 0.04MPa, heat the vacuum induction furnace to 1680℃, keep warm for 20min, then turn off the power to obtain molten steel, and then cool the molten steel to room temperature with the furnace to obtain a steel ingot; after forging the steel ingot, roll and temper treatment are carried out in sequence to obtain hydrogen embrittlement resistant Cr-Mo alloy steel; wherein the initial forging temperature of forging is 1100℃, the final forging temperature is 880℃, and the cooling method is slow cooling; before rolling, preheat to 1100℃ and keep warm at 1100℃ for 60min, the starting rolling temperature of the rolling is 1050℃, the final rolling temperature is 900℃, and the rolling reduction is 70%; the tempering treatment is first quenching at 880℃ for 60min, the cooling method is water cooling, and then tempering at 680℃ for 90min, and the cooling method is air cooling.

[0057] Example 2

[0058] The present embodiment provides a hydrogen embrittlement resistant Cr-Mo alloy steel, which contains the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.04%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%; Nb, 0.03%; W, 0.9%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=1.33, Se / Cu=1, 4Nb+W=1.02%.

[0059] In this embodiment, the preparation of the hydrogen embrittlement resistant Cr-Mo alloy steel is as follows: the raw materials for preparing the hydrogen embrittlement resistant Cr-Mo alloy steel are added into a vacuum induction furnace according to the above ratio for smelting, and the vacuum is evacuated to 2.5×10 -3 Pa, then fill with argon to 0.04MPa, heat the vacuum induction furnace to 1680℃, keep warm for 20min, then turn off the power to obtain molten steel, and then cool the molten steel to room temperature with the furnace to obtain a steel ingot; after forging the steel ingot, roll and temper treatment are carried out in sequence to obtain hydrogen embrittlement resistant Cr-Mo alloy steel; wherein the initial forging temperature of forging is 1100℃, the final forging temperature is 880℃, and the cooling method is slow cooling; before rolling, preheat to 1100℃ and keep warm at 1100℃ for 60min, the starting rolling temperature of the rolling is 1050℃, the final rolling temperature is 900℃, and the rolling reduction is 70%; the tempering treatment is first quenching at 880℃ for 60min, the cooling method is water cooling, and then tempering at 680℃ for 90min, and the cooling method is air cooling.

[0060] Comparative Example 1

[0061] The present comparative example provides a Cr-Mo alloy steel, which contains the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.04%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; Se / Cu=1.

[0062] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0063] Comparative Example 2

[0064] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.04%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%, Nb, 0.04%; W, 1%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=1, Se / Cu=1, 4Nb+W=1.16%.

[0065] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0066] Comparative Example 3

[0067] Comparative Example 3 provides a Cr-Mo alloy steel, which is resistant to hydrogen embrittlement. The Cr-Mo alloy steel contains the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.04%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%; Nb, 0.01%; W, 0.3%; rare earth RE, 0.008%, and the rest is Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=4, Se / Cu=1, 4Nb+W=0.34%.

[0068] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0069] Comparative Example 4

[0070] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.04%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%; Nb, 0.03%; W, 0.5%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 8:2; and Cu / Nb=1.33, Se / Cu=1, 4Nb+W=0.62%.

[0071] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0072] Comparative Example 5

[0073] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.04%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.08%; Nb, 0.03%; W, 0.5%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=2.67, Se / Cu=0.5, 4Nb+W=0.62%.

[0074] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0075] Comparative Example 6

[0076] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.04%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.02%; Nb, 0.03%; W, 0.5%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=0.67, Se / Cu=2,4Nb+W=0.62%.

[0077] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0078] Comparative Example 7

[0079] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.08%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%; Nb, 0.03%; W, 0.5%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=1.33, Se / Cu=2, 4Nb+W=0.62%.

[0080] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0081] Comparative Example 8

[0082] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.01%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%; Nb, 0.03%; W, 0.5%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=1.33, Se / Cu=0.25, 4Nb+W=0.62%.

[0083] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0084] Comparative Example 9

[0085] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.04%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%; Nb, 0.03%; W, 0.5%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=1.33, Se / Cu=1, 4Nb+W=0.62%.

[0086] In this comparative example, the Cr-Mo alloy steel is prepared by adding the raw materials for preparing the Cr-Mo alloy steel into a vacuum induction furnace according to the above ratio for smelting, and evacuating to 2.5×10 -3 Pa, then fill with argon to 0.04MPa, heat the vacuum induction furnace to 1680℃, keep warm for 20min, then turn off the power to obtain molten steel, and then cool the molten steel to room temperature with the furnace to obtain a steel ingot; after forging the steel ingot, roll and temper treatment are carried out in sequence to obtain Cr-Mo alloy steel; wherein the initial forging temperature of forging is 1100℃, the final forging temperature is 880℃, and the cooling method is slow cooling; before rolling, preheat to 1100℃ and keep warm at 1100℃ for 60min, the starting rolling temperature of the rolling is 1050℃, the final rolling temperature is 900℃, and the rolling reduction is 70%; the tempering treatment is first quenching at 880℃ for 60min, the cooling method is water cooling, and then tempering at 680℃ for 150min, and the cooling method is air cooling.

[0087] Comparative Example 10

[0088] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.04%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%; Nb, 0.03%; W, 0.5%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=1.33, Se / Cu=1, 4Nb+W=0.62%.

[0089] In this comparative example, the Cr-Mo alloy steel is prepared by adding the raw materials for preparing the Cr-Mo alloy steel into a vacuum induction furnace according to the above ratio for smelting, and evacuating to 2.5×10 -3Pa, then fill with argon to 0.04MPa, heat the vacuum induction furnace to 1680℃, keep warm for 20min, then turn off the power to obtain molten steel, and then cool the molten steel to room temperature with the furnace to obtain a steel ingot; after forging the steel ingot, roll and temper treatment are carried out in sequence to obtain Cr-Mo alloy steel; wherein the initial forging temperature of forging is 1100℃, the final forging temperature is 880℃, and the cooling method is slow cooling; before rolling, preheat to 1100℃ and keep warm at 1100℃ for 60min, the starting rolling temperature of the rolling is 1050℃, the final rolling temperature is 900℃, and the rolling reduction is 70%; the tempering treatment is first quenching at 880℃ for 90min, the cooling method is water cooling, and then tempering at 680℃ for 90min, and the cooling method is air cooling.

[0090] Comparative Example 11

[0091] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.04%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%; Nb, 0.03%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=1.33, Se / Cu=1, 4Nb+W=0.12%.

[0092] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0093] Comparative Example 12

[0094] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.04%, Nb, 0.03%; W, 0.5%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=1.33, 4Nb+W=0.62%.

[0095] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0096] Comparative Example 13

[0097] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.005%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.01%; Nb, 0.03%; W, 0.5%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=0.33, Se / Cu=0.5, 4Nb+W=0.62%.

[0098] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0099] Comparative Example 14

[0100] The present comparative example provides a Cr-Mo alloy steel, which comprises the following components in mass percentage: C, 0.31%; Si, 0.29%; Mn, 0.61%; P, 0.006%; S, 0.004%; Se, 0.15%; Ni, 0.24%; Cr, 1.1%; Mo, 0.24%; Al, 0.05%; Cu, 0.15%; Nb, 0.03%; W, 0.5%; rare earth RE, 0.008%, and the rest are Fe and unavoidable impurities; wherein the rare earth RE is composed of La and Ce, and the mass ratio of La to Ce is 6:4; and Cu / Nb=5, Se / Cu=1, 4Nb+W=0.62%.

[0101] When preparing the Cr-Mo alloy steel in this comparative example, except for the ratio of each raw material, other parameters and operations are the same as those in Example 1.

[0102] Comparative Example 15

[0103] This comparative example provides a high-strength, high-toughness, hydrogen embrittlement-resistant steel plate (Cr-Mo alloy steel), which contains the following components in mass percentage: C, 0.09%; Si, 0.07%; Mn, 0.9%; Cu, 0.9%; Ni, 2.0%; Cr, 0.4%; Mo, 0.55%; Nb, 0.05%; the rest is Fe and unavoidable impurities.

[0104] In this comparative example, the high-strength, high-toughness, hydrogen embrittlement-resistant steel plate is prepared by adding the raw materials for preparing the high-strength, high-toughness, hydrogen embrittlement-resistant steel plate into a vacuum induction furnace according to the above ratio for smelting, and evacuating to 2.5×10 -3 Pa, then fill with argon to 0.04MPa, heat the vacuum induction furnace to 1680℃, keep warm for 20min, then turn off the power to obtain molten steel, and then cool the molten steel to room temperature with the furnace to obtain a steel ingot; after forging the steel ingot, roll and temper treatment are carried out in sequence to obtain a high-strength, high-toughness, hydrogen embrittlement-resistant steel plate; wherein the initial forging temperature of forging is 1100℃, the final forging temperature is 880℃, and the cooling method is slow cooling; before rolling, preheat to 1100℃ and keep warm at 1100℃ for 60min, the starting rolling temperature of the rolling is 1150℃, the final rolling temperature is 950℃, and the rolling reduction is 70%; the tempering treatment is first quenching at 850℃ for 60min, the cooling method is water cooling, and then tempering at 580℃ for 90min, and the cooling method is air cooling.

[0105] The present invention conducts a room temperature dynamic slow strain rate tensile test on the hydrogen embrittlement resistant Cr-Mo alloy steels prepared in Examples 1 and 2 and the Cr-Mo alloy steels prepared in the comparative examples. During the test, the hydrogen charging solution is an aqueous solution containing 0.2 mol / L NaOH and 0.22 g / L thiourea, and the hydrogen charging current density is 20 mA / cm 2 , the strain rate is 10 -6 s -1 The results of yield strength, tensile strength, room temperature elongation and hydrogen embrittlement sensitivity index are shown in Table 1.

[0106] Table 1

[0107]

[0108] It can be seen from the results in Table 1 that the hydrogen embrittlement resistant Cr-Mo alloy steels prepared in Examples 1 and 2 of the present invention exhibit high toughness (including high yield strength, high tensile strength and high room temperature elongation) in a hydrogen-charged environment and have stronger hydrogen embrittlement resistance. The hydrogen embrittlement resistant Cr-Mo alloy steel material prepared by the present invention is advantageous for obtaining a Cr-Mo alloy steel having both high toughness and excellent hydrogen embrittlement resistance by compositely adding appropriate microalloying elements such as Se, Cu, Nb, W and RE, and simultaneously satisfying 1.3≤Cu / Nb≤2, 0.5≤Se / Cu≤1.2, and 0.56%≤4Nb+W≤1.1%. In the present invention, the addition of an appropriate amount of Se can significantly improve the hydrogen embrittlement resistance of the Cr-Mo alloy steel, and the composite addition of Cu, Nb and W can be used as a strengthening component to produce significant precipitation strengthening, and the dispersedly distributed NbC, WC and Cu nano-scale precipitation phases generated in the matrix can be used as deep hydrogen traps to effectively improve the hydrogen embrittlement resistance of the Cr-Mo alloy steel. The present invention realizes the simultaneous improvement of high strength, high toughness and hydrogen embrittlement resistance of the Cr-Mo alloy steel, while in general, when the strength of the steel increases, the toughness will decrease, and the hydrogen embrittlement resistance will decrease, and it is difficult to improve both at the same time. The present invention solves the problem that the strength and hydrogen embrittlement resistance of the Cr-Mo alloy steel are difficult to coordinate.

[0109] Parts of the present invention that are not described in detail are well known to those skilled in the art.

[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A hydrogen embrittlement resistant Cr-Mo alloy steel, characterized in that: The hydrogen embrittlement resistant Cr-Mo alloy steel comprises the following components in mass percentage: C, 0.28% to 0.33%; Si, 0.2% to 0.35%; Mn, 0.5% to 0.8%; P≤0.02%; S≤0.01%; Se, 0.01% to 0.1%; Ni, 0.15% to 0.25%; Cr, 0.9% to 1.1%; Mo, 0.17% to 0.25%; Al, 0.02% to 0.06%; Cu, 0.02% to 0.1%; Nb, 0.01% to 0.04%; W, 0.3% to 1.1%; rare earth RE, 0.006% to 0.009%; the rest is Fe and unavoidable impurities; And satisfy the following equations (1) and (2): 1.3≤Cu / Nb≤2 Formula (1); 0.5≤Se / Cu≤1.2 Formula (2); In formula (1) and formula (2), each component symbol represents the mass percentage of each component; The mass percentages of Nb and W components in the hydrogen embrittlement resistant Cr-Mo alloy steel satisfy the following formula (3): 0.56%≤4Nb+W≤1.1% Formula (3); In formula (3), each component symbol represents the mass percentage of each component; The yield strength of the hydrogen embrittlement resistant Cr-Mo alloy steel is not less than 666 MPa, the tensile strength is not less than 745 MPa, the room temperature elongation is not less than 14.2%, and the hydrogen embrittlement sensitivity index HEI is not greater than 9.3%.

2. The hydrogen embrittlement resistant Cr-Mo alloy steel according to claim 1, characterized in that: Rare earths RE are La and Ce, and the mass ratio of La to Ce is (4~6): (4~6).

3. The hydrogen embrittlement resistant Cr-Mo alloy steel according to claim 1, characterized in that: In the hydrogen embrittlement resistant Cr-Mo alloy steel, the mass percentage of W is 0.5-0.9%.

4. The method for preparing the hydrogen embrittlement resistant Cr-Mo alloy steel according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: (1) Smelting the raw materials for preparing hydrogen embrittlement resistant Cr-Mo alloy steel in a vacuum induction furnace to obtain a steel ingot; (2) After forging, the steel ingot is rolled and tempered in sequence to produce hydrogen embrittlement-resistant Cr-Mo alloy steel.

5. The preparation method according to claim 4, characterized in that: The initial forging temperature of the forging is 1050°C to 1150°C, and the final forging temperature is 850°C to 900°C.

6. The preparation method according to claim 4, characterized in that: Before the rolling, the steel is preheated to 1050-1150° C. and kept at 1050-1150° C. for 30-90 minutes.

7. The preparation method according to claim 4, characterized in that: The starting rolling temperature of the rolling is 1000°C to 1100°C, and the final rolling temperature is 850°C to 950°C.

8. The preparation method according to claim 4, characterized in that: The quenching and tempering treatment is to first quench at 850°C to 910°C for 30 to 60 minutes, and then temper at 670°C to 730°C for 60 to 120 minutes.

Citation Information

Patent Citations

  • Abrasion resistant steel plate having low-temperature toughness and hydrogen embrittlement resistance, and manufacturing method therefor

    CN105189803A

  • HL-grade novel sucker rod steel and preparation method thereof

    CN116855851A

  • Non-magnetic stainless steel having excellent cold forgeability and hydrogen embrittlement resistance or corrosion resistance