Microstructure homogenization determination method and recycled aluminum alloy preparation method

The method addresses the challenge of inconsistent inclusion distribution and microstructure homogenization in aluminum alloy production by implementing real-time detection and variance analysis, ensuring closed-loop control for uniformity and consistent product quality.

CN118817993BActive Publication Date: 2024-12-06SHANDONG NANSHAN ALUMINUM +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411258867.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-12-06
Estimated Expiration
2044-09-10

AI Technical Summary

Technical Problem

Existing aluminum alloy production methods fail to monitor the content and distribution of micron-sized inclusions in the melt and the degree of homogenization of ingot microstructure in real time, leading to open-loop control and inconsistent product quality.

Method used

A method involving melt inclusion detection using a liquid metal purity analyzer or multi-microporous circular plate filtration analyzer, and ingot structure detection using an optical microscope and scanning electron microscope, with variance analysis to assess inclusion and microstructure uniformity, followed by targeted refining and homogenization treatments.

Benefits of technology

Ensures real-time quality feedback and closed-loop control, enabling timely adjustments to achieve uniform inclusion distribution and microstructure in the melt and ingot, thereby guaranteeing consistent product quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118817993B_ABST
    Figure CN118817993B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of aluminum alloy smelting, and provides a method for determining microstructure homogenization and a method for preparing a recycled aluminum alloy, including melt inclusion detection: detecting the inclusion content of multiple regions of the melt; calculating the variance δ of the inclusion content; i ; If δ i ≤0.1, it is judged as qualified for uniformity; the ingot structure detection includes: sampling at multiple positions of the ingot; detecting and calculating the average grain size variance δ g ; Z3, detect and calculate the phase distribution variance δ p ; If δ g ≤0.1, and δ p ≤0.1, it is judged as qualified in uniformity. Thus, the present invention measures the degree of deviation of each detection value from the average value through variance analysis, and establishes a judgment standard. The present invention introduces the judgment link of the uniformity of the inclusions in the melt and the microstructure of the ingot. By adding the quality feedback link, two closed-loop controls on the melt quality and the ingot quality are formed respectively, which effectively guarantees the quality of the finished ingot.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum alloy smelting, and in particular relates to a microstructure homogenization determination method and a recycled aluminum alloy preparation method. Background Art

[0002] The recycled aluminum alloy melt contains a large number of micron-sized inclusions with high melting points. They exist in the melt in the form of solid particles and cannot diffuse evenly. During the solidification process, solid inclusions will serve as precipitation sites for high-melting-point precipitation phases such as iron-rich phases, resulting in uneven distribution of ingot composition and precipitation phases.

[0003] Therefore, the content and distribution uniformity of these inclusions in the aluminum alloy melt directly affect the microstructure morphology of the ingot and ultimately affect the mechanical properties of the aluminum alloy.

[0004] Although the existing aluminum alloy production method can remove inclusions in the melt to a certain extent, it can also refine the grains of the ingot structure, such as the technical solutions disclosed in Chinese patent applications CN201810780660.4 and CN202011182043.8. However, during the production process, it is impossible to grasp the content and distribution of inclusions in the melt, as well as the degree of homogenization of the ingot microstructure. Therefore, the existing production process is open-loop control, lacking quality feedback information, making it impossible to make timely adjustments during the production process and effectively guaranteeing the quality of the finished product.

[0005] In summary, the prior art obviously has inconveniences and defects in practical use, so it is necessary to improve it. Summary of the invention

[0006] In view of the above-mentioned defects, the present invention mainly provides a method for determining microstructure homogenization, which solves the technical problem that the existing aluminum alloy refining technology cannot grasp the distribution of melt inclusions and the degree of homogenization of ingot microstructure in real time.

[0007] In order to solve the above problems, the present invention provides a method for determining microstructure homogenization, including melt inclusion detection and ingot structure detection; specifically:

[0008] The melt inclusion detection includes:

[0009] S1, detect the inclusion content in multiple areas of the melt;

[0010] S2, calculate the variance δ of inclusion content in each region i ;

[0011] S3, determine whether the uniformity of inclusions in the melt is qualified:

[0012] If δ i≤0.1, the uniformity is considered qualified;

[0013] If δ i >0.1, it is judged as unqualified uniformity;

[0014] The ingot structure detection includes:

[0015] Z1, sampling at multiple positions of the ingot; the sampling positions can cover the three-dimensional space of the ingot;

[0016] Z2, detect the grain size at each sampling position and calculate the average grain size variance δ g ;

[0017] Z3, detect the phase distribution at each sampling position and calculate the phase distribution variance δ p ;

[0018] Z4, determine whether the uniformity of the microstructure of the ingot is qualified:

[0019] If δ g ≤0.1, and δ p ≤0.1, the uniformity is considered qualified;

[0020] If δ g and δ p If any one of the values ​​is greater than 0.1, or both values ​​are greater than 0.1, it is judged as unqualified uniformity.

[0021] According to the microstructure homogenization determination method of the present invention, the melt inclusion detection comprises: using a liquid metal purity analyzer or a multi-microporous circular plate filtration analyzer to detect the content of inclusions in each area of ​​the melt.

[0022] According to the microstructure homogenization determination method of the present invention, the ingot structure detection includes: using an optical microscope, a scanning electron microscope and backscattered electron diffraction to detect the grain size, the phase and the phase distribution of the ingot.

[0023] According to the microstructure homogenization determination method of the present invention, an optical microscope is used to detect the grain size of the ingot; a scanning electron microscope and / or backscattered electron diffraction is used to detect the phase and phase distribution of the ingot.

[0024] According to the microstructure homogenization determination method of the present invention, the melt inclusion detection comprises: the selected detection areas can be evenly distributed in the melt, and the number of the selected detection areas is not less than 15.

[0025] According to the microstructure homogenization determination method of the present invention, the ingot structure detection includes: the sampling positions can cover various areas of the ingot, and the number of sampling positions is not less than 15.

[0026] A method for preparing a recycled aluminum alloy comprises the following steps:

[0027] S1, refinement;

[0028] heating the recycled aluminum alloy melt to a predetermined refining temperature;

[0029] Inert gas is introduced into the melt for refining to remove hydrogen and inclusions in the melt;

[0030] S2, stirring;

[0031] Stirring the refined recycled aluminum alloy melt to make the residual inclusions evenly distributed in the melt;

[0032] S3, inclusion detection;

[0033] The residual inclusion content of multiple regions in the melt is detected by using the melt inclusion detection step in the microstructure homogenization determination method; and the variance δ of the inclusion content is calculated. i ;

[0034] S4, determine whether the uniformity of residual inclusions in the melt is qualified:

[0035] If δ i ≤0.1, it is judged as uniformity qualified and proceed to the next step;

[0036] If δ i >0.1, it is judged as unqualified uniformity, and steps S1-S3 are repeated;

[0037] S5, pouring;

[0038] After the recycled aluminum alloy melt is poured and solidified, a recycled aluminum alloy ingot is obtained;

[0039] S6, homogenization heat treatment;

[0040] Performing homogenization heat treatment on the recycled aluminum alloy ingot to obtain an ingot with uniformly distributed microstructure;

[0041] S7, ingot microstructure detection;

[0042] Sampling multiple positions of the ingot using the ingot structure detection step in the microstructure homogenization determination method;

[0043] Detect the grain size at each sampling position and calculate the average grain size variance δ g ;

[0044] Detect the phase distribution at each sampling position and calculate the phase distribution variance δ p ;

[0045] S8, determine whether the uniformity of the microstructure of the ingot is qualified:

[0046] If δ g ≤0.1, and δ p ≤0.1, the uniformity is judged to be qualified and a qualified ingot product is obtained;

[0047] If δ g and δ p If any one of the values ​​is greater than 0.1, or both values ​​are greater than 0.1, it is determined that the uniformity is unqualified, and steps S6-S7 are repeated.

[0048] According to the method for preparing recycled aluminum alloy of the present invention, the inert gas is argon or nitrogen with a purity of not less than 99.9%; the gas supply method includes rotating inert gas blowing, ceramic tube blowing or graphite tube blowing.

[0049] According to the method for preparing recycled aluminum alloy of the present invention, the refining temperature is 750-850° C., so that the high melting point inclusions containing iron and / or copper elements in the recycled aluminum alloy melt are melted.

[0050] According to the method for preparing recycled aluminum alloy of the present invention, after the homogenization heat treatment, the ingot is subjected to milling treatment; the milling depth is 5-10 cm.

[0051] In summary, the microstructure homogenization determination method of the present invention performs multiple area sampling on the melt and the ingot respectively, and performs quantitative detection on the inclusion content of the melt, the grain size of the ingot and the phase distribution. The degree of deviation of each detection value from the average value is measured by variance analysis, and a determination standard is established based on the analysis results. Quantitative and qualitative determinations are made on the uniformity of inclusions in the melt and the uniformity of the microstructure of the ingot respectively. The present invention also provides a method for preparing a recycled aluminum alloy, which introduces a judgment link for the uniformity of inclusions in the melt and the microstructure of the ingot. A quality feedback link is added in the production process, and two closed-loop controls on the melt quality and the ingot quality are formed respectively. In the production process, targeted treatment can be made in a timely manner to effectively ensure the quality of the finished ingot. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 is a process diagram of the method for preparing a recycled aluminum alloy of the present invention; DETAILED DESCRIPTION

[0053] See also Figure 1 The present invention provides a method for determining microstructure homogenization, including melt inclusion detection and ingot structure detection; specifically:

[0054] The melt inclusion detection includes:

[0055] S1, detect the inclusion content in multiple areas of the melt;

[0056] Preferably, the selected detection areas can be evenly distributed in the melt so that the detection results can reflect the content and distribution of the inclusions in the melt as a whole. The number of the selected detection areas is not more than 15.

[0057] S2, calculate the variance δ of inclusion content in each region i ;

[0058] S3, determine whether the uniformity of inclusions in the melt is qualified:

[0059] If δ i ≤0.1, the uniformity is considered qualified;

[0060] If δ i >0.1, it is judged as unqualified uniformity;

[0061] After the judgment, corresponding treatment methods can be made for qualified melt and unqualified melt respectively.

[0062] Qualified melt can be processed in the next step, such as casting production, to ensure the quality of castings;

[0063] Unqualified melt can be adjusted until it reaches the qualified standard; or the unqualified melt can be downgraded for use to stop the loss in time to avoid quality accidents.

[0064] The ingot structure detection includes:

[0065] Z1, sampling is performed at multiple positions of the ingot; the sampling positions can cover the three-dimensional space of the ingot; further, the sampling positions are not less than 15, preferably more than 20, which can better cover various areas of the ingot, so that the test results can comprehensively evaluate the microstructure morphology of the ingot. Those skilled in the art can also adjust the number of sampling positions according to the volume adaptability of the ingot.

[0066] Z2, detect the grain size at each sampling position and calculate the average grain size variance δ g ;

[0067] Z3, detect the phase distribution at each sampling position and calculate the phase distribution variance δ p ;

[0068] Z4, determine whether the uniformity of the microstructure of the ingot is qualified:

[0069] If δ g ≤0.1, and δ p ≤0.1, the uniformity is considered qualified;

[0070] If δ g and δp If any one of the values ​​is greater than 0.1, or both values ​​are greater than 0.1, it is judged as unqualified uniformity;

[0071] After the determination, corresponding treatments can be made for qualified ingots and unqualified ingots respectively.

[0072] Qualified ingots can be processed in the next step, such as being put into storage as finished products or being machined;

[0073] Unqualified ingots can be adjusted to meet qualified standards; or unqualified ingots can be scrapped to stop losses in time to avoid quality accidents.

[0074] As an embodiment of detecting the inclusion content in the melt, the present invention uses a liquid metal purity analyzer (LiMCA) or a multi-porous circular plate filtration analyzer (PoDFA) to detect the inclusion content in each region of the melt.

[0075] As an embodiment of ingot structure detection, the present invention uses optical microscope (OM), scanning electron microscope (SEM) and / or backscattered electron diffraction (EBSD) to detect the grain size, physical phase and physical phase distribution of the ingot. Those skilled in the art can make reasonable configurations for each detection item according to the actual detection resource adaptability.

[0076] For example, an optical microscope (OM) is used to detect and count the grain size of the ingot; a scanning electron microscope (SEM) and / or electron backscatter diffraction (EBSD) is used to detect the phase and phase distribution of the ingot.

[0077] The phase of the present invention is a precipitation phase or a second phase, and the organizational components of the precipitation phase of different aluminum alloys are different. For example, the precipitation phase of 7050 alloy is Al 2 Cu and Al 3 Fe, etc.

[0078] The present invention uses an optical microscope (OM) or a scanning electron microscope (SEM) or other detection equipment to detect the physical phase at each sampling position. The physical phase distribution at the sampling position is calibrated by counting the total area of ​​all physical phases in the field of view of the detection equipment. Then, the physical phase distribution variance δ is calculated using the total area of ​​the physical phase counted at each sampling position. p ;

[0079] The microstructure homogenization determination method of the present invention samples multiple regions of the melt and the ingot, and quantitatively detects the inclusion content of the melt, the grain size of the ingot, and the phase distribution. The deviation degree of each detection value from the average value is measured by variance analysis, and a determination standard is established based on the analysis results. Quantitative and qualitative determinations are made on the uniformity of inclusions in the melt and the uniformity of the microstructure of the ingot, respectively. Quality feedback information can be provided in a timely manner during the production process, so that the production process can be timely targeted and the quality of the finished product can be effectively guaranteed.

[0080] See also Figure 1 The present invention also provides a method for preparing a recycled aluminum alloy, comprising the following steps:

[0081] S1, refinement;

[0082] heating the recycled aluminum alloy melt to a predetermined refining temperature;

[0083] Inert gas is introduced into the melt for refining to remove hydrogen and inclusions in the melt;

[0084] Preferably, the inert gas of the present invention is argon or nitrogen with a purity of not less than 99.9%; the gas delivery method includes rotating inert gas injection (SNIF), ceramic tube injection or graphite tube injection;

[0085] The refining temperature of the present invention can be adaptively set according to the composition of the recycled aluminum alloy.

[0086] In order to control the oxidation and burning of the aluminum alloy, the refining temperature of the present invention does not exceed 900°C.

[0087] As an embodiment, the refining temperature of the present invention is 750-850°C, which can melt the high-melting-point inclusions containing elements such as iron and copper in the recycled aluminum alloy melt, reduce the nucleation points of the high-temperature precipitation phase, and prevent the high-melting-point precipitation phase such as the iron-rich phase from growing on it as a matrix. At the same time, it can also promote the full and uniform diffusion of inclusions in the melt.

[0088] The viscosity of the melt has a great influence on the uniformity of inclusion distribution. Aluminum alloys with different compositions have different melt viscosities. For example, aviation aluminum alloys have a high melting point of 630°C, and their Si content is high, resulting in high viscosity, which causes poor melt fluidity and affects the uniformity of inclusions. Increasing the melt temperature will reduce the melt viscosity, improve fluidity, and promote the uniform distribution of residual inclusions in the melt.

[0089] S2, stirring;

[0090] Stirring the refined recycled aluminum alloy melt to make the residual inclusions evenly distributed in the melt;

[0091] The presence of Al in the recycled aluminum alloy melt 2 O 3 、CaO、Al 2 MgO 4 、MgO、SiO 2 、Al 4 C 3 , SiC and other high melting point inclusions. In a static melt, inclusions in the solid phase lack sufficient diffusion driving force and cannot be fully diffused in the melt to achieve uniform distribution. By stirring the melt, the melt circulation can be promoted, providing diffusion driving force for high melting point inclusions in the melt, promoting their uniform distribution, and thus reducing their impact on the uniformity of the ingot structure after solidification.

[0092] As a preferred solution, the stirring method of the present invention is mechanical stirring; it can also be electromagnetic stirring.

[0093] S3, inclusion detection;

[0094] The residual inclusion content of multiple regions in the melt is detected by using the melt inclusion detection step in the microstructure homogenization determination method; and the variance δ of the inclusion content is calculated. i ;

[0095] S4, determine whether the uniformity of residual inclusions in the melt is qualified:

[0096] If δ i ≤0.1, it is judged as uniformity qualified and proceed to the next step;

[0097] If δ i >0.1, it is judged as unqualified uniformity, and steps S1-S3 are repeated;

[0098] S5, pouring;

[0099] After the recycled aluminum alloy melt is poured and solidified, a recycled aluminum alloy ingot is obtained;

[0100] As a preferred solution, the present invention adopts a uniform solidification solution after the melt is poured, and the temperature difference between various regions in the melt during the solidification process does not exceed 10° C. This makes the structure distribution in the ingot more uniform.

[0101] Those skilled in the art can select an applicable solution from the known uniform solidification casting processes and apply it to the melt solidification of the present invention.

[0102] S6, homogenization heat treatment;

[0103] Performing homogenization heat treatment on the recycled aluminum alloy ingot to obtain an ingot with uniformly distributed microstructure;

[0104] S7, ingot microstructure detection;

[0105] Sampling multiple positions of the ingot using the ingot structure detection step in the microstructure homogenization determination method;

[0106] Detect the grain size at each sampling position and calculate the average grain size variance δ g ;

[0107] Detect the phase distribution at each sampling position and calculate the phase distribution variance δ p ;

[0108] S8, determine whether the uniformity of the microstructure of the ingot is qualified:

[0109] If δ g ≤0.1, and δ p ≤0.1, the uniformity is judged to be qualified and a qualified ingot product is obtained;

[0110] If δ g and δ p If any one of the values ​​is greater than 0.1, or both values ​​are greater than 0.1, it is determined that the uniformity is unqualified, and steps S6 and S7 are repeated;

[0111] The ingot homogenization heat treatment of the present invention comprises a heating process, a heat preservation process and a cooling process.

[0112] Heating process: The ingot to be processed is heated to a predetermined temperature so that the atoms of various structures in the ingot begin to diffuse; the heating temperature can be set according to the specific grade of aluminum alloy;

[0113] Insulation process: Insulate the ingot for a predetermined time within a predetermined temperature range; make the non-equilibrium structure in the ingot uniform through atomic diffusion; the insulation temperature and time are adaptively set according to the thickness of the ingot and the heating temperature;

[0114] Cooling process: After the insulation reaches the predetermined time, the ingot is cooled down at an appropriate cooling rate and cooling method to obtain a recycled aluminum alloy ingot with uniform microstructure.

[0115] Those skilled in the art can adaptively set the aforementioned parameters of the homogenization heat treatment of the present invention according to the specific grade of aluminum alloy and heat treatment requirements in combination with common knowledge.

[0116] As an embodiment, the heating temperature of the homogenization heat treatment of the present invention is 470° C.; the temperature is kept at 450-470° C. for 20-30 hours; and air cooling is adopted for cooling.

[0117] Furthermore, after the homogenization heat treatment, the ingot is subjected to milling treatment; the milling depth is 5-10 cm; the solidified crust layer on the surface of the ingot is removed to reduce the influence on the grain size and the phase uniformity detection value.

[0118] The method for preparing recycled aluminum alloy of the present invention introduces the judgment link of the inclusions of the melt and the uniformity of the microstructure of the ingot. A quality feedback link is added in the production process, forming two closed-loop controls on the melt quality and the ingot quality respectively. In the production process, targeted treatment can be made in time to effectively ensure the quality of the finished ingot.

[0119] As an embodiment, before the melt of the present invention is stirred, a high-melting-point modifier is added to the melt. The modifier forms a large number of high-melting-point spherical intermetallic compounds with Al in the melt, and is dispersed in the melt, providing heterogeneous nucleation sites for the growth of the iron-rich phase. In the subsequent solidification process, elements such as Fe in the melt are used as a substrate for the spherical intermetallic compounds, and continue to grow on the substrate, eventually forming a spheroidized, dispersedly distributed second phase structure. The original harmful iron-rich phase morphology in the melt is transformed into a spherical iron-rich phase, which reduces the stress concentration of the material during the strain process and avoids tearing the matrix to cause crack propagation.

[0120] At the same time, during the solidification process of the melt, since the atomic radius of the elements in the modifier is larger than that of the aluminum atom, they can become heterogeneous nucleation sites when they enter the melt, reduce the interfacial tension between the solid and liquid phases, increase the nucleation speed and nucleation rate, promote the nucleation of the second phase and inhibit its growth; ultimately, the second phase structure is refined, so that the modified spheroidized iron-rich phase plays a dispersion strengthening role, which can significantly improve the strength and fracture toughness of the recycled aluminum alloy products.

[0121] The modifier of the present invention may be one or more of rare earth elements, zirconium (Zr), titanium (Ti) or boron (B).

[0122] In summary, the present invention provides a method for determining the homogenization of a microstructure, by sampling a plurality of regions of a melt and an ingot, respectively, and performing quantitative detection on the inclusion content of the melt, the grain size of the ingot, and the phase distribution. The degree of deviation of each detection value from the average value is measured by variance analysis, and a determination standard is established based on the analysis results. Quantitative and qualitative determinations are made on the uniformity of inclusions in the melt and the uniformity of the microstructure of the ingot, respectively. The present invention also provides a method for preparing a recycled aluminum alloy, which introduces a link for determining the uniformity of inclusions in the melt and the microstructure of the ingot. A quality feedback link is added during the production process, forming two closed-loop controls on the melt quality and the ingot quality, respectively. During the production process, targeted treatments can be made in a timely manner to effectively ensure the quality of the finished ingot.

[0123] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art may make various corresponding changes and modifications based on the present invention, but these corresponding changes and modifications should all fall within the scope of protection of the claims attached to the present invention.

Claims

1. A method for determining microstructure homogenization, characterized in that: Including melt inclusion detection and ingot structure detection; specifically: The melt inclusion detection includes: S1, detect the inclusion content in multiple areas of the melt; S2, calculate the variance δ of inclusion content in each region i ; S3, determine whether the uniformity of inclusions in the melt is qualified: If δ i ≤0.1, the uniformity is considered qualified; If δ i >0.1, it is judged as unqualified uniformity; The ingot structure detection includes: Z1, sampling at multiple positions of the ingot; the sampling positions can cover the three-dimensional space of the ingot; Z2, detect the grain size at each sampling position and calculate the average grain size variance δ g ; Z3, detect the phase distribution at each sampling position and calculate the phase distribution variance δ p ; Z4, determine whether the uniformity of the microstructure of the ingot is qualified: If δ g ≤0.1, and δ p ≤0.1, the uniformity is considered qualified; If δ g and δ p If at least one of the values ​​is greater than 0.1, it is judged as unqualified uniformity.

2. The method for determining microstructure homogenization according to claim 1, characterized in that: The melt inclusion detection includes: using a liquid metal purity analyzer or a multi-microporous circular plate filtration analyzer to detect the content of inclusions in each area of ​​the melt.

3. The method for determining microstructure homogenization according to claim 1, characterized in that: The ingot structure detection includes: using an optical microscope, a scanning electron microscope and backscattered electron diffraction to detect the grain size of the ingot, the physical phase and the physical phase distribution of the ingot.

4. The method for determining microstructure homogenization according to claim 1, characterized in that: The melt inclusion detection comprises: the selected detection areas can be evenly distributed in the melt, and the number of the selected detection areas is not less than 15.

5. The method for determining microstructure homogenization according to claim 1, wherein: The ingot structure detection includes: the sampling positions can cover various areas of the ingot, and the number of the sampling positions is not less than 15.

6. A method for preparing a recycled aluminum alloy, characterized in that: The steps include: S1, refinement; heating the recycled aluminum alloy melt to a predetermined refining temperature; Inert gas is introduced into the melt for refining to remove hydrogen and inclusions in the melt; S2, stirring; Stirring the refined recycled aluminum alloy melt to make the residual inclusions evenly distributed in the melt; S3, inclusion detection; Detecting the residual inclusion content of multiple regions in the melt by using the melt inclusion detection step in the microstructure homogenization determination method according to any one of claims 1 to 5; and calculating the variance δ of the inclusion content i ; S4, determine whether the uniformity of residual inclusions in the melt is qualified: If δ i ≤0.1, it is judged as uniformity qualified and proceed to the next step; If δ i >0.1, it is judged as unqualified uniformity, and steps S1-S3 are repeated; S5, pouring; After the recycled aluminum alloy melt is poured and solidified, a recycled aluminum alloy ingot is obtained; S6, homogenization heat treatment; Performing homogenization heat treatment on the recycled aluminum alloy ingot to obtain an ingot with uniformly distributed microstructure; S7, ingot microstructure inspection; Sampling multiple positions of the ingot using the ingot structure detection step in the microstructure homogenization determination method according to any one of claims 1 to 5; Detect the grain size at each sampling position and calculate the average grain size variance δ g ; Detect the phase distribution at each sampling position and calculate the phase distribution variance δ p ; S8, determine whether the uniformity of the microstructure of the ingot is qualified: If δ g ≤0.1, and δ p ≤0.1, the uniformity is judged to be qualified and a qualified ingot product is obtained; If δ g and δ p If at least one of the values ​​is greater than 0.1, it is determined that the uniformity is unqualified and steps S6-S7 are repeated.

7. The method for preparing a recycled aluminum alloy according to claim 6, characterized in that: The inert gas is argon or nitrogen with a purity of not less than 99.9%; the gas supply method includes rotating inert gas blowing, ceramic tube blowing or graphite tube blowing.

8. The method for preparing a recycled aluminum alloy according to claim 6, characterized in that: The refining temperature is 750-850° C., so as to melt the high melting point inclusions containing iron and / or copper elements in the recycled aluminum alloy melt.

9. The method for preparing a recycled aluminum alloy according to claim 6, characterized in that: After the homogenization heat treatment, the ingot is milled; the milling depth is 5-10cm.