A high temperature resistant composite insulating column and preparation method thereof

Through mesoporous silica load curing accelerator and periodic pressure technology, the failure problem of high-temperature composite insulating materials in high-temperature environments is solved, and the overall performance homogenization and high-temperature stability of the material are achieved. It is suitable for large currents, Application under high temperature conditions.

CN118824650BActive Publication Date: 2024-11-22ZHEJIANG FLYAFORD ELECTRON CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202411315842.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-11-22
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

Existing high-temperature resistant composite insulating materials are prone to failure problems caused by pores or cracks in high temperature environments, and traditional processes are difficult to effectively improve the overall performance uniformity and bonding force of the material.

Method used

The mesoporous silica loads a specific curing accelerator to actively induce enhanced curing of fracture or weak bonding. Combined with periodic pressure technology, the overall uniformity of the insulating material and the uniform distribution of internal stress are ensured, so as to be under high temperature and high current conditions. Reduce weaknesses and singularities.

Benefits of technology

It achieves homogenization of the overall performance of high-temperature composite insulating materials, extends service life, and maintains excellent mechanical properties in high-temperature environments above 200℃, meeting the application needs of high current and high temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118824650B_ABST
    Figure CN118824650B_ABST
Patent Text Reader

Abstract

The invention discloses a high temperature resistant composite insulating column and a preparation method thereof, comprising a high temperature resistant composite insulating material and a metal structural part, wherein the metal structural part is coated or bonded by the high temperature resistant composite insulating material, the high temperature resistant composite insulating material is composed of epoxy resin, phenolic resin, inorganic filler, curing accelerator, mesoporous nano-silica reinforcing agent and auxiliary additives, the metal structural part is prepared from gold, silver, copper, aluminum or their alloys, the mesoporous nano-silica reinforcing agent is loaded with a specific reinforcing agent, and periodic pressurization is performed on a specific rheological stage of a resin cake or slice during the temperature-raising curing rheological state, so as to induce weak bonding to guide the mesoporous nano-silica reinforcing agent to exert its effect, enhance the overall curing uniformity, and finally realize the preparation of a high Tg, high heat-resistant high temperature resistant composite insulating column.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of insulating materials, and in particular relates to a high temperature resistant composite insulating column and a preparation method thereof. Background Art

[0002] As the charging speed requirements for new energy vehicles are increasing, the battery pack needs to withstand greater voltage and current, and the battery temperature will be higher, resulting in a simultaneous increase in the performance requirements of the insulating column. The performance of the conventional BMC plastic currently used is significantly weakened after aging at 200°C, and the torque, tension, shear force, etc. are all lower than the use standard. Therefore, the sealing material needs to have better thermal conductivity and flame retardant properties than conventional sealing materials. Epoxy resin is a type of thermosetting resin formed by curing epoxy prepolymers with curing agents. It has excellent water resistance, heat resistance, chemical stability, and excellent electrical insulation and mechanical properties. High-temperature resistant composite insulation materials (EMC) prepared from epoxy resin, curing agent, various organic / inorganic fillers and a series of auxiliary additives have become an indispensable packaging material in the electronic packaging industry. Its different process routes achieve different performance requirements, enriching the selection capabilities of downstream industry applications.

[0003] In the high-temperature resistant composite insulating material composition provided by the invention of patent CN107446316 B, by adding isocyanate-modified polyether silicone as a stress absorber, the isocyanate (-NCO) group at the end of the silicone material can react with the hydroxyl (-OH) group produced during the curing process, so that the silicone enters the cross-linking network and increases the cross-linking density, thereby achieving the effect of increasing the glass transition temperature of the material (Tg>140°C), and at the same time, it can further reduce the flexural modulus of the material.

[0004] The invention patent of patent CN 103992641 B provides a thermosetting resin composition, which is prepared by a method of co-curing epoxy resin with active ester resin and allyl modified bismaleimide resin. The processing and curing molding conditions are relatively mild, and the dielectric constant and dielectric loss are relatively low. The heat resistance and toughness of the resin composition after curing are improved to a certain extent. However, the Tg of the thermosetting resin composition after curing is less than 220°C, and the heat resistance is still not ideal, and it cannot meet the requirements of use in high temperature environments above 250°C.

[0005] The epoxidized 1,2-polybutadiene provided by the invention of patent CN111978726 A has epoxy groups and unsaturated double bonds, and can react with phenolic resin and maleimide resin at the same time to participate in resin curing, so that the thermosetting resin composition has high impact strength after curing and exhibits good toughness, overcoming the shortcomings of the traditional bismaleimide resin cured product, which is brittle and lacks toughness. After curing, it has a high glass transition temperature (Tg>300℃) and thermal stability, and can be used as a matrix resin in the fields of electronic packaging molding compounds, copper-clad laminates, high-temperature resistant adhesives and composite materials.

[0006] According to background information, most patents improve heat resistance and other properties by modifying epoxy resin or changing the matrix resin material. In practice, the failure cause of high-temperature resistant composite insulation materials does not necessarily require the pursuit of excessively high Tg and other material properties. Aging is manifested in the vicious cycle caused by pores or cracks, which is equally important. At present, the technical achievements in improving the preparation process are general. In the "Study on the Preparation and Performance Optimization of Epoxy Molding Compounds for Electronic Packaging", the effects on pores or gaps are discussed from aspects such as cookie density, raw material-carried gas, reaction production gas, the relationship between material rheological properties and pores, and the relationship between silicon micropowder particle size and distribution and pores. Finally, the pores are transformed into nano-scale dispersed micropores in each situ to solve the problem. There is also a lack of problem of improving its principle.

[0007] The purpose of the present invention is to improve the heat resistance and other application properties of the product by improving the preparation process. Summary of the invention

[0008] In view of the problems in the related art, the present invention proposes a high temperature resistant composite insulating column and a preparation method thereof to overcome the above technical problems existing in the existing related art.

[0009] The technical solution of the present invention is achieved by loading a specific curing accelerator on mesoporous silica to strengthen the curing of the fracture or weak bonding actively induced during the curing process, thereby ensuring the overall curing effect, achieving the overall uniformity of the high-temperature resistant composite insulating material, and uniform internal stress distribution, so that there are no weak points or singular points under the conditions of high temperature and skin effect generated when the metal structure of the insulating column carries a large current, thereby improving the failure extension problem of traditional devices caused by weak links in the material. The specific content of the invention is as follows:

[0010] A high temperature resistant composite insulating column comprises a high temperature resistant composite insulating material and a metal structural part.

[0011] Preferably, the high temperature resistant composite insulating material is composed of epoxy resin, phenolic resin, inorganic filler, curing accelerator, mesoporous nano-silica reinforcing agent and auxiliary additives.

[0012] Preferably, the metal structural part is made of gold, silver, copper, aluminum or their alloys, preferably a copper-containing structural part.

[0013] Preferably, the metal structural member is coated or bonded with the high temperature resistant composite insulating material.

[0014] Preferably, during the coating or bonding, periodic pressure is applied to the high temperature resistant composite insulating material in a rheological state.

[0015] The present invention also discloses a method for preparing a high temperature resistant composite insulating column, which comprises the following preparation steps:

[0016] S1: The high temperature resistant composite insulation material includes the following raw materials in parts by weight:

[0017] 10-20 parts of epoxy resin, 5-10 parts of phenolic resin, 80-50 parts of inorganic filler, 0.05-0.5 parts of curing accelerator, 0.5-1.5 parts of mesoporous nano-silica reinforcing agent and 0.1-2 parts of auxiliary additives;

[0018] S2: Mixing

[0019] The prepared raw materials are configured according to a preset weight ratio, and mixed evenly at a high speed to obtain a premix;

[0020] S3: Rubber Mixing

[0021] The premix is ​​mixed in an extruder at a mixing temperature of 100-110°C, and the extruder is extruded at high speed, and after cooling, the mixture is crushed to make cakes or slices for discharging;

[0022] S4: Heating and curing

[0023] The cake or slice is placed in the preheating mold cavity, and a metal structure is set in the preheating mold cavity. It is heated and cured at a constant heating rate. When the starting temperature (125-160°C) is reached, periodic pressure is applied until the cut-off temperature (140-170°C) is reached, and then the peak pressure is maintained until the gel curing is completed after the curing temperature.

[0024] Preferably, the epoxy resin is one or more of o-cresol epoxy resin, polyaromatic epoxy resin, and polyfunctional epoxy resin.

[0025] Preferably, the phenolic resin is one or more of linear phenolic resin, polyaromatic ring phenolic resin and polyfunctional phenolic resin.

[0026] More preferably, the combination of the epoxy resin and the phenolic resin is one of a combination of a multifunctional epoxy resin and a linear phenolic resin, and a combination of a multifunctional epoxy resin and a multifunctional phenolic resin.

[0027] Preferably, the inorganic filler is one or more of crystalline rounded silica, molten spherical silica, spherical boron nitride, alumina, and aluminum nitride.

[0028] More preferably, the particle size of the inorganic filler is 5 to 50 um.

[0029] Preferably, the curing accelerator is an organic phosphine compound, preferably one of triphenylphosphine-p-benzoquinone, tetraphenylphosphine-dihydroxynaphthalene, and tetraphenylphosphine-dihydroxydiphenyl sulfone.

[0030] Preferably, the mesoporous nano-silica reinforcing agent is composed of coupling agent-modified mesoporous nano-silica with a particle size of 100 to 200 nm, the mesopore diameter is 10 to 30 nm, and the reinforcing agent is loaded in the mesopores.

[0031] More preferably, the reinforcing agent is one or more of methylimidazole and aminoimidazole, preferably one of aminoimidazole and methylimidazole.

[0032] More preferably, the coupling agent is one or more of silane, titanate, aluminum chelate and zirconium aluminum oxide, preferably one of KH550, KH560 and KH570.

[0033] More preferably, the nano-silica reinforcing agent is prepared by mixing the reinforcing agent with the silane coupling agent at a high speed and then drying the mixture under a negative pressure of 0.8 to 1.2 atm.

[0034] Preferably, the raw materials for preparing the high temperature resistant composite insulating material also include one or more combinations of 0.5 to 1.5 parts of coupling agent, 1 to 2 parts of flame retardant, 0.2 to 0.5 parts of colorant, 0.3 to 0.5 parts of release agent and 0.2 to 1.5 parts of stress modifier.

[0035] Preferably, the release agent is one or more of palm wax, polyethylene wax, and polyamide wax, preferably palm wax.

[0036] Preferably, the flame retardant is a phosphorus-based flame retardant, a hydroxide flame retardant, preferably a combination of one or more of phosphate ester and aluminum hydroxide.

[0037] Preferably, the stress modifier is one of silicone oil, silicone resin and silicone rubber, preferably silicone oil.

[0038] Preferably, the colorant is one of carbon black with a particle size of 20 to 30 nm and black nano-silicon dioxide with a particle size of 20 to 30 nm, preferably carbon black.

[0039] Preferably, the periodic pressure peak value is 12 to 16 MPa, the valley value is 6 to 8 MPa, and the periodic frequency is 2 to 8 times / min.

[0040] More preferably, the ratio of the periodic pressure peak to valley value is 2:1.

[0041] More preferably, the cycle frequency is 4 to 6 times / min.

[0042] Preferably, the initial temperature of the preheating mold cavity is 105-115°C, the constant temperature rise rate is 4-12°C / min, the starting temperature is 125-160°C, the cut-off temperature is 140-170°C, and the curing temperature is 160-200°C.

[0043] More preferably, the constant temperature rise rate is 6-10°C / min.

[0044] More preferably, the starting temperature and the ending temperature are determined according to the heat flow rate of the cake. During the temperature rise and curing process, the temperature when the heat flow rate rises to -0.1w / g is the starting temperature, and the temperature when the heat flow rate rises to 0.1w / g is the ending temperature.

[0045] More preferably, the measured value of the heat flow rate is obtained under non-periodic pressurization and 10°C / min temperature increase conditions.

[0046] Beneficial effects of the present invention:

[0047] Compared with the prior art, the present invention improves the high temperature resistant composite insulation column and its preparation method. Based on the use of normal curing accelerators, the deformation of weak bonds or weak bonding parts is actively induced by periodic pressure at a specific stage of material gelation, thereby releasing special curing accelerators such as aminoimidazole loaded by mesoporous silica to promote the curing level of weak bonds or weak bonding parts, thereby achieving the overall homogenization of the performance of high temperature resistant composite insulation materials. This solves the problem that defects are easily extended from weak bonds or weak bonding parts when the bonding force of the materials is uneven;

[0048] Furthermore, the high temperature resistant composite insulating material of aminoimidazole loaded by mesoporous silica of the present invention can gradually release aminoimidazole when its surface is stimulated by high current, high temperature and other conditions, thereby repairing the corroded parts to a certain extent, thereby extending its service life;

[0049] Furthermore, the multifunctional epoxy resin-linear phenolic resin system selected by the present invention can achieve high performance such as Tg exceeding 220° C. through the technical solution of the present invention, and can meet the use conditions of high current, high temperature and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the specific implementation of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are some implementations of the present invention. For those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work.

[0051] Figure 1 It is a schematic diagram of the change of the preparation pressure with the temperature of the present invention;

[0052] Figure 2 It is a schematic diagram of the change of the preparation pressure over time of the present invention;

[0053] Figure 3 This is a schematic diagram of the starting and ending temperature settings of the present invention;

[0054] Figure 4 It is a schematic side view of the structure of a high temperature resistant composite insulating column of the present invention;

[0055] Figure 5 The figure is a schematic top view of the structure of a high temperature resistant composite insulating column of the present invention. DETAILED DESCRIPTION

[0056] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0057] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0058] Embodiments 1 to 6 of the present invention are for testing material properties, and do not cover or bond the high-temperature resistant composite material with a metal structural member, which is specifically illustrated by Embodiment 7 of the present invention.

[0059] Embodiment 1, the preparation method of high temperature resistant composite insulating material comprises the following steps:

[0060] S1: The high temperature resistant composite insulation material includes the following raw materials in parts by weight:

[0061] 10 parts of multifunctional epoxy resin, 5 parts of linear phenolic resin, 60 parts of crystalline silica microspheres, 15 parts of fused silica microspheres, 0.35 parts of curing accelerator, 0.5 parts of release agent, 0.5 parts of mesoporous nano-silica reinforcing agent;

[0062] S2: Mixing

[0063] The prepared raw materials are configured according to the preset weight proportions, and mixed at a high speed of 800 r / min for 10 min to obtain a premix;

[0064] S3: Rubber Mixing

[0065] The premix is ​​mixed in an extruder at a mixing temperature of 105°C and a speed of 750 r / min, and after cooling, the mixture is crushed to form a cake;

[0066] S4: Heating and curing

[0067] Place the 20 mm*40 mm columnar cake into a 20 mm*20 mm closed mold cavity preheated at 110°C, heat at a rate of 6°C / min, and start cyclic pressure application at 138°C at a rate of 6 times / min, with a pressure valley of 8 MPa and a peak of 16 MPa, and stop at 150°C. That is, 12 pressure changes are completed. Then maintain the pressure of 16 MPa until the temperature rises to 175°C to complete gel curing, and cure at 175°C for 2 hours after demolding. See the start and end temperatures for details. Figure 3 The heat flow rate of Example 1 is in the range of -0.1 to 0.1 w / g.

[0068] The preparation of mesoporous nano-silica reinforcing agent comprises the following steps:

[0069] (A) 2 g of silane coupling agent was hydrolyzed in anhydrous ethanol (50 ml) at 30°C for 30 min, 10 g of mesoporous nano-silica was added to the anhydrous ethanol solution (60 ml) and mixed, and the mixture was stirred at 90°C at a speed of 300 r / min for 30 min to obtain an intermediate product, i.e., mesoporous nano-silica modified with a silane coupling agent, and surface amino ion properties were obtained;

[0070] (B) mixing the intermediate product obtained in step (A) with 2 g of a curing agent, stirring and reacting at 70° C. and 200 r / min for 1.5 h to obtain a functional mesoporous nano-silica mixed solution loaded with a curing accelerator;

[0071] (C) The mixed solution obtained in step (B) is dried and separated under a negative pressure of 0.9 atm.

[0072] The multifunctional epoxy resin used in the preparation of this embodiment is EPPN502H from Nippon Kayaku, the linear phenolic resin is PN5080 from Changchun Chemical, the particle size of the inorganic filler is 15um, the curing accelerator is triphenylphosphine, the particle size of the mesoporous nano-silica is 200nm, the pore size is 15nm, the release agent is palm wax, the silane coupling agent is KH550, and the reinforcing agent is aminoimidazole. The aminoimidazole is more suitable for combining with the mesoporous nano-silica modified by the silane coupling agent to ensure the delayed expression of the thermal latent function.

[0073] Embodiment 2, the preparation method of high temperature resistant composite insulating material comprises the following steps:

[0074] S1: The high temperature resistant composite insulation material includes the following raw materials in parts by weight:

[0075] 15 parts of multifunctional epoxy resin, 8 parts of linear phenolic resin, 70 parts of crystalline silica microspheres, 10 parts of fused silica microspheres, 0.4 parts of curing accelerator, 1 part of coupling agent, 0.3 parts of release agent, 1 part of flame retardant, 0.2 parts of colorant, 0.5 parts of stress modifier and 1.5 parts of mesoporous nano-silica reinforcing agent;

[0076] S2: Mixing

[0077] The prepared raw materials are configured according to the preset weight proportions, and mixed at a high speed of 800 r / min for 10 min to obtain a premix;

[0078] S3: Rubber Mixing

[0079] The premix is ​​mixed in an extruder at a mixing temperature of 105°C and a speed of 750 r / min, and after cooling, the mixture is crushed to form a cake;

[0080] S4: Heating and curing

[0081] Place the 20 mm*40 mm columnar cake into a 20 mm*20 mm closed mold cavity preheated at 110°C, heat at a rate of 5°C / min, and start cyclic pressure application at 155°C at a rate of 6 times / min, with a pressure valley of 7 MPa and a peak of 14 MPa, and stop at 165°C. That is, 12 pressure changes are completed. Then maintain the pressure of 14 MPa until the temperature rises to 180°C for gel curing, and cure at 175°C for 2 hours after demolding. See the start and end temperatures for details. Figure 3 The heat flow rate of Example 2 is in the range of -0.1 to 0.1 w / g.

[0082] The preparation of mesoporous nano-silica reinforcing agent comprises the following steps:

[0083] (A) 2g of silane coupling agent was hydrolyzed in anhydrous ethanol (50ml) at 30°C for 30min, 9g of mesoporous nano-silica was added to the anhydrous ethanol solution (60ml) and mixed, and stirred at 100°C at a speed of 300r / min for 30min to obtain an intermediate product, i.e., mesoporous nano-silica modified with a silane coupling agent, and surface amino ion properties were obtained;

[0084] (B) mixing the intermediate product obtained in step (A) with 3 g of a curing agent, stirring and reacting at 80° C. and 200 r / min for 1 h to obtain a functional mesoporous nano-silica mixed solution loaded with a curing accelerator;

[0085] (C) The mixed solution obtained in step (B) is dried and separated under a negative pressure of 1.0 atm.

[0086] The multifunctional epoxy resin used in the preparation of this embodiment is Nippon Kayaku EPPN502H, the linear phenolic resin is Changchun Chemical PN5080, the inorganic filler particle size is 15um, the curing accelerator is tetraphenylphosphine-dihydroxynaphthalene, the mesoporous nano-silica particle size is 150nm, the pore size is 10nm, the release agent is palm wax, the silane coupling agent is KH570, the reinforcing agent is methylimidazole, the colorant is Mitsubishi Chemical MA600, the flame retardant is phosphate, and the stress modifier is silicone oil. This embodiment adds additives to improve the stress, flame retardancy and other properties of the ordinary system. The coupling agent in the raw material for preparing the high-temperature resistant composite insulation material is also KH570.

[0087] Embodiment 3, the preparation method of high temperature resistant composite insulating material comprises the following steps:

[0088] S1: The high temperature resistant composite insulating material includes the following raw materials in parts by weight:

[0089] 15 parts of multifunctional epoxy resin, 8 parts of multifunctional phenolic resin, 70 parts of crystalline silica microspheres, 10 parts of fused silica microspheres, 0.4 parts of curing accelerator, 0.5 parts of coupling agent, 0.3 parts of release agent, 1 part of flame retardant, 0.2 parts of colorant, 0.5 parts of stress modifier and 1.5 parts of mesoporous nano-silica reinforcing agent;

[0090] S2: Mixing

[0091] The prepared raw materials are configured according to the preset weight proportions, and mixed at a high speed of 800 r / min for 10 min to obtain a premix;

[0092] S3: Rubber Mixing

[0093] The premix is ​​mixed in an extruder at a mixing temperature of 105°C and a speed of 750 r / min, and after cooling, the mixture is crushed to form a cake;

[0094] S4: Heating and curing

[0095] Place the Ф20 mm*40 mm columnar cake into a Ф20 mm*20 mm closed mold cavity preheated at 110℃, heat at a heating rate of 10℃ / min, and start cyclic pressure application at 160℃ at 8 times / min, with a pressure valley of 7Mpa and a peak of 14Mpa, and stop at 170℃. That is, 8 pressure changes are completed. Then maintain the pressure of 14Mpa until the temperature rises to 180℃ for gel curing, and cure at 175℃ for 2h after demolding. See the starting and ending temperatures for details. Figure 3 The heat flow rate of Example 3 is in the range of -0.1 to 0.1 w / g.

[0096] The preparation of mesoporous nano-silica reinforcing agent comprises the following steps:

[0097] (A) 2g of silane coupling agent was hydrolyzed in anhydrous ethanol (50ml) at 30°C for 30min, 9g of mesoporous nano-silica was added to the anhydrous ethanol solution (60ml) and mixed, and stirred at 100°C at a speed of 300r / min for 30min to obtain an intermediate product, i.e., mesoporous nano-silica modified with a silane coupling agent, and surface amino ion properties were obtained;

[0098] (B) mixing the intermediate product obtained in step (A) with 3 g of a curing agent, stirring and reacting at 80° C. and 200 r / min for 1 h to obtain a functional mesoporous nano-silica mixed solution loaded with a curing accelerator;

[0099] (C) The mixed solution obtained in step (B) is dried and separated under a negative pressure of 1.0 atm.

[0100] The multifunctional epoxy resin used in the preparation of this embodiment is Nippon Kayaku EPPN502H, the multifunctional phenolic resin is Meiwa Chemical MEH7500, the inorganic filler D50 particle size is 15um, the curing accelerator is tetraphenylphosphine-dihydroxynaphthalene, the mesoporous nano-silica D50 particle size is 150nm, the pore size is 10nm, the release agent is palm wax, the silane coupling agent is KH550, the reinforcing agent is methylimidazole, the colorant is Mitsubishi Chemical MA600, the flame retardant is phosphate ester, and the stress modifier is silicone oil. The coupling agent in the raw material for preparing the high-temperature resistant composite insulation material is also KH550.

[0101] Embodiment 4, the preparation method of high temperature resistant composite insulating material comprises the following steps:

[0102] S1: The high temperature resistant composite insulating material includes the following raw materials in parts by weight:

[0103] 10 parts of multifunctional epoxy resin, 5 parts of linear phenolic resin, 60 parts of crystalline silica microspheres, 15 parts of fused silica microspheres, 0.35 parts of curing accelerator, 1 part of coupling agent, 0.5 parts of release agent, 1 part of flame retardant, 0.2 parts of colorant, 0.5 parts of stress modifier and 0.5 parts of modified mesoporous nano-silica;

[0104] S2: Mixing

[0105] The prepared raw materials are configured according to the preset weight proportions, and mixed at a high speed of 800 r / min for 10 min to obtain a premix;

[0106] S3: Rubber Mixing

[0107] The premix is ​​mixed in an extruder at a mixing temperature of 105°C and a speed of 750 r / min, and after cooling, the mixture is crushed to form a cake;

[0108] S4: Step-by-step heating to completely cure

[0109] Place the 20 mm*40 mm columnar cake into a 20 mm*20 mm closed mold cavity preheated at 110°C, maintain a pressure of 16 MPa, and wait for the temperature to rise to 175°C for 40 seconds to complete the initial curing. After demoulding, cure at 175°C for 2 hours. See the starting and ending temperatures for details. Figure 3 The heat flow rate of Example 4 is in the range of -0.1 to 0.1 w / g, specifically 140°C and 160°C.

[0110] The preparation of mesoporous nano-silica reinforcing agent comprises the following steps:

[0111] (A) 2 g of silane coupling agent was hydrolyzed in anhydrous ethanol (50 ml) at 30°C for 30 min, 10 g of mesoporous nano-silica was added to the anhydrous ethanol solution (60 ml) and mixed, and the mixture was stirred at 90°C at a speed of 300 r / min for 30 min to obtain an intermediate product, i.e., mesoporous nano-silica modified with a silane coupling agent, and surface amino ion properties were obtained;

[0112] (B) The mixed solution obtained in step (A) is dried and separated under a negative pressure of 0.9 atm.

[0113] The multifunctional epoxy resin used in the preparation of this embodiment is EPPN502H from Nippon Kayaku, the linear phenolic resin is PN5080 from Changchun Chemical, the inorganic filler D50 has a particle size of 15um, the curing accelerator is triphenylphosphine, the mesoporous nano-silica D50 has a particle size of 200nm and a pore size of 15nm, the release agent is palm wax, and the silane coupling agent is KH560. The mesoporous nano-silica modified by the silane coupling agent has amino functionality and is also suitable for combining with epoxy resin to increase the interfacial bonding force between organic and inorganic substances. The coupling agent in the raw material for preparing the high-temperature resistant composite insulating material is also KH560.

[0114] Embodiment 5, the preparation method of high temperature resistant composite insulating material comprises the following steps:

[0115] S1: The high temperature resistant composite insulating material includes the following raw materials in parts by weight:

[0116] 16 parts of multifunctional epoxy resin, 8 parts of linear phenolic resin, 65 parts of crystalline silica microspheres, 10 parts of fused silica microspheres, 0.35 parts of curing accelerator, 0.5 parts of coupling agent, 0.5 parts of release agent, 1 part of flame retardant, 0.2 parts of colorant and 0.5 parts of stress modifier;

[0117] S2: Mixing

[0118] The prepared raw materials are configured according to the preset weight proportions, and mixed at a high speed of 800 r / min for 10 min to obtain a premix;

[0119] S3: Rubber Mixing

[0120] The premix is ​​mixed in an extruder at a mixing temperature of 105°C and a speed of 750 r / min, and after cooling, the mixture is crushed to form a cake;

[0121] S4: Heating and curing

[0122] Place the 20 mm*40 mm columnar cake into a 20 mm*20 mm closed mold cavity preheated at 110°C, maintain a pressure of 16 MPa, and wait for the temperature to rise to 175°C for 40 seconds to complete the initial curing. After demoulding, cure at 175°C for 2 hours. See the starting and ending temperatures for details. Figure 3 The heat flow rate of Example 5 is in the range of -0.1 to 0.1 w / g, specifically 125°C and 145°C.

[0123] The multifunctional epoxy resin used in the preparation of this embodiment is Nippon Kayaku EPPN502H, the linear phenolic resin is Changchun Chemical PN5080, the inorganic filler D50 has a particle size of 15 μm, the curing accelerator is triphenylphosphine, the release agent is palm wax, the colorant is Mitsubishi Chemical MA600, the flame retardant is phosphate ester, the stress modifier is silicone oil, and the coupling agent is KH550.

[0124] Embodiment 6, the preparation method of high temperature resistant composite insulating material comprises the following steps:

[0125] S1: The high temperature resistant composite insulating material includes the following raw materials in parts by weight:

[0126] 16 parts of polyaromatic ring epoxy resin, 8 parts of polyaromatic ring phenolic resin, 65 parts of crystalline silica microspheres, 10 parts of fused silica microspheres, 0.35 parts of curing accelerator, 0.5 parts of coupling agent, 0.5 parts of release agent, 1 part of flame retardant, 0.2 parts of colorant and 0.5 parts of stress modifier;

[0127] S2: Mixing

[0128] The prepared raw materials are configured according to the preset weight proportions, and mixed at a high speed of 800 r / min for 10 min to obtain a premix;

[0129] S3: Rubber Mixing

[0130] The premix is ​​mixed in an extruder at a mixing temperature of 105°C and a speed of 750 r / min, and after cooling, the mixture is crushed to form a cake;

[0131] S4: Heating and curing

[0132] Place the 20 mm*40 mm columnar cake into a 20 mm*20 mm closed mold cavity preheated at 110°C, maintain a pressure of 16 MPa, and wait for the temperature to rise to 175°C for 40 seconds to complete the initial curing. After demoulding, cure at 175°C for 2 hours. See the starting and ending temperatures for details. Figure 3 The heat flow rate of Example 5 is in the range of -0.1 to 0.1 w / g, specifically 125°C and 155°C.

[0133] The polyaromatic ring epoxy resin used in the preparation of this embodiment is Nippon Kayaku EPPN502H, the polyaromatic ring phenolic resin is Changchun Chemical PN5080, the inorganic filler D50 has a particle size of 15 μm, the curing accelerator is triphenylphosphine, the release agent is palm wax, the colorant is Mitsubishi Chemical MA600, the flame retardant is phosphate ester, the stress modifier is silicone oil, and the coupling agent is KH550.

[0134] The heat flow rate of the resin material in Example 6 is used to define the starting and ending temperatures as 125°C and 155°C, with a temperature difference of 30°C. The periodic pressurization is carried out 3 times / min at a heating rate of 12°C / min. Figure 1 It is a schematic diagram showing the change of the preparation pressure with the temperature of the present invention. Since the temperature difference range of other embodiments is smaller, this embodiment is used as an illustration and has nothing to do with other results. Figure 2 It is a schematic diagram showing the change of the preparation pressure with time of the present invention, and it can be seen that a rheological periodic pressurization working section of about 2 minutes can be provided.

[0135] In Examples 1 to 6, no metal support or connector is placed for performance measurement, so high temperature resistant composite insulation materials for more application fields are not fully prepared. However, the present invention can place copper, silver, aluminum and their alloys as a support or connector in the preheating mold cavity, preferably a copper-containing support or connector.

[0136] Example 7, preparing a mesoporous nano-silica reinforcing agent, comprising the following steps:

[0137] (A) 2g of silane coupling agent was hydrolyzed in anhydrous ethanol (50ml) at 30°C for 30min, 9g of mesoporous nano-silica was added to the anhydrous ethanol solution (60ml) and mixed, and stirred at 100°C at a speed of 300r / min for 30min to obtain an intermediate product, i.e., mesoporous nano-silica modified with a silane coupling agent, and surface amino ion properties were obtained;

[0138] The intermediate product obtained in step (A) and 3 g of a curing agent were mixed, and the mixture was stirred at 80° C. and 200 r / min for 1 h to obtain a functional mesoporous nano-silica mixed solution loaded with a curing accelerator;

[0139] (C) The mixed solution obtained in step (B) is dried and separated under a negative pressure of 1.0 atm.

[0140] The preparation of a high temperature resistant composite insulating column comprises the following steps:

[0141] S1: The high temperature resistant composite insulating material includes the following raw materials in parts by weight:

[0142] 12 parts of multifunctional epoxy resin, 6 parts of linear phenolic resin, 70 parts of crystalline silica microspheres, 10 parts of fused silica microspheres, 0.4 parts of curing accelerator, 0.8 parts of coupling agent, 0.3 parts of release agent, 1 part of flame retardant, 0.2 parts of colorant, 0.5 parts of stress modifier and 1.5 parts of mesoporous nano-silica reinforcing agent;

[0143] S2: Mixing

[0144] The prepared raw materials are configured according to the preset weight proportions, and mixed at a high speed of 800 r / min for 10 min to obtain a premix;

[0145] S3: Rubber Mixing

[0146] The premix is ​​mixed in an extruder at a mixing temperature of 105°C and a speed of 750 r / min, and after cooling, the mixture is crushed to form a cake;

[0147] S4: Heating and curing

[0148] Place a Ф17 mm*50 mm columnar cake into a Ф18 mm*25 mm closed mold cavity preheated at 110°C. There is a 15 mm long internal thread copper structure in the model cavity. The outer diameter of the structure is Ф10 mm, the inner diameter is Ф8 mm, and the internal thread depth is 10 mm. Heat at a heating rate of 5°C / min, and start cyclic pressure application at 155°C at a rate of 8 times / min. The pressure valley is 7Mpa and the peak is 14Mpa, and stop at 165°C. That is, 16 pressure changes are completed. Then maintain a pressure of 14Mpa and wait until the temperature rises to 180°C for gel curing. After demolding, cure at 175°C for 2 hours. See the starting and ending temperatures for details. Figure 3 The heat flow rate of Example 2 is in the range of -0.1 to 0.1 w / g.

[0149] The multifunctional epoxy resin used in the preparation of this embodiment is Nippon Kayaku EPPN502H, the linear phenolic resin is Changchun Chemical PN5080, the inorganic filler particle size is 15um, the curing accelerator is tetraphenylphosphine-dihydroxynaphthalene, the mesoporous nano-silica particle size is 150nm, the pore size is 10nm, the release agent is palm wax, the silane coupling agent is KH550, the reinforcing agent is methylimidazole, the colorant is Mitsubishi Chemical MA600, the flame retardant is phosphate, and the stress modifier is silicone oil. This embodiment adds additives to improve the stress, flame retardancy and other properties of the ordinary system. The coupling agent in the raw material for preparing the high-temperature resistant composite insulation material is also KH550.

[0150] The prepared high temperature resistant composite insulating column structure is as follows Figure 4 , Figure 5 Copper structural parts ( Figure 4 The surface of the insert 1 and the insert 2 in the side view diagram also has a protrusion to increase the bonding strength between the high temperature resistant insulation material and the copper structure. The high temperature resistant composite insulation material covers part of the copper structure, and the internal thread ( Figure 5 The circle with the smallest inner diameter and the semicircle with the second smallest inner diameter in the top view schematic diagram form a schematic diagram) to provide an external current connection port. When in use, the interface between the high-temperature resistant composite insulating material and the copper structural member is under high current working conditions, affected by the skin effect, with a high degree of heat accumulation, which places higher requirements on its heat resistance. The high-temperature resistant composite insulating material used in this embodiment has a Tg of more than 220°C, a Td of more than 340°C, and a bending strength of more than 180MPa. The differences in the torsion, tension, and shear force of the material in different axial directions are all less than 3%. Therefore, it is more suitable for applications under extreme conditions.

[0151] Comparative Example 1: A BMC bulk molding compound was prepared in a conventional manner.

[0152] In Examples 1 to 6, the closed mold cavity with a 110°C preheating temperature is used to prepare a high temperature resistant composite insulation material with a 20 mm*20 mm cylindrical inner cavity, and the preheating temperature can be selected in the range of 105 to 115°C. Relevant tests are performed on the high temperature resistant composite insulation materials and intermediates prepared in the above examples. The test standards are as follows:

[0153] (1) Spiral flow length: According to the method in SJ / T 11197-2013 High Temperature Resistant Composite Insulation Materials, take 15g of the resin composition sample to be tested and inject it into the spiral flow metal mold of EMMI-1-66 on a transfer molding press to measure the spiral flow length of the sample. Set the upper and lower mold temperatures to 175±3℃ and the transfer pressure to (125kg±5kg)cm -2 , the transmission speed is (6.0cm±0.1cm)s -1 , solidify for 120s, then take out the sample from the metal mold, read the spiral flow length, accurate to 0.5cm, test the same sample three times, take the average value, and the transmission pressure is calculated by dividing the total pressure by the injection head area;

[0154] (2) Gel time: According to the method in SJ / T 11197-2013 High-temperature resistant composite insulation materials, heat the hot plate to 175°C ± 2°C, take 0.5g of the resin composition sample and place it on the hot plate. The sample is spread over an area of ​​about 5cm 2 , start timing when melting begins, stir with a needle-shaped stirring tip or a flat spatula, and the end point is when the powder gradually turns into a gel (the sample cannot be pulled into a thread), read the required time, repeat the same operation twice, and take the average value;

[0155] (3) Glass transition temperature Tg: The resin composition is molded at 175°C using an injection molding machine and then post-cured at 175°C for 2 hours and 200°C for 2 hours; then measured using a differential scanning calorimeter in accordance with the National Standard of the People's Republic of China GB / T19466.2-2004 "Plastics Differential Scanning Calorimetry (DSC) Part 2: Determination of Glass Transition Temperature" for Tg testing;

[0156] (4) Flexural strength and flexural modulus: The resin composition was molded using an injection molding machine at 175°C and then post-cured at 175°C for 2 hours and 200°C for 2 hours; then tested in accordance with the National Standard of the People's Republic of China GB / T9341-2008 "Determination of Flexural Properties of Plastics";

[0157] (5) Initial thermal decomposition temperature (Td): The resin composition was molded at 175°C using an injection molding machine and then post-cured at 175°C for 2 hours and 200°C for 2 hours. Then, about 5 mg of the sample was tested using a thermogravimetric analyzer at a heating rate of 10°C / min from room temperature to 800°C in a nitrogen atmosphere. The temperature (Td) corresponding to the sample weight loss of 1 wt% was taken as the initial thermal decomposition temperature to evaluate the thermal stability of the resin composition after curing.

[0158] (6) Thermal expansion coefficient: The resin composition was molded using an injection molding machine at 175°C and then post-cured at 175°C for 2 hours and 220°C for 2 hours; then the test was performed in accordance with the National Standard of the People's Republic of China GB / T 36800.2-2018 "Thermomechanical Analysis (TMA) of Plastics Part 2: Determination of Linear Thermal Expansion Coefficient and Glass Transition Temperature";

[0159] (7) DSC curve: The rubber was mixed on an open mixer at 105°C for 4 min, then crushed and sieved to obtain a refined high-temperature resistant composite insulation material. About 10 mg of sample was placed in the sample tray, nitrogen protection was applied, the heating rate was 10°C / min, and the curing curve was obtained by a differential calorimeter;

[0160] (8) After aging at 200℃ for 4h, the high temperature resistant composite insulation material is tested for torque, tension and shear force. The test points are two points at the same position but in different axial directions.

[0161] The performance test results of Examples 1 to 6 and Comparative Example 1 are shown in Table 1 below, and the performance test results after aging at 200° C. for 4 hours are shown in Table 2 below.

[0162] Table 1

[0163]

[0164] As can be seen from Table 1, the curing time of EMC plastic is slightly longer than that of BMC plastic. However, due to the combination of epoxy resin-phenolic resin, as well as the synergistic effect of accelerators, inorganic fillers, etc., the glass transition temperature and thermal decomposition temperature of the prepared high-temperature resistant composite insulation material have higher bending strength and fracture deflection, showing good toughness. The mesoporous nano-silica reinforcing agent introduced in the preparation process and the technology of actively inducing periodic pressure to eliminate weak bonding during the melting process show a significant tendency to increase strength. The comprehensive performance of Example 2 is the best, which uses a combination of multifunctional epoxy resin and linear phenolic resin, but the thermal decomposition temperature and flexural strength are compared with the combination of multifunctional epoxy resin and multifunctional phenolic resin in Example 3. After removing the mesoporous nano-silica reinforcing agent and the technical process of actively inducing periodic pressure during the melting process compared to Example 5, the performance is reduced by 15% to 25%, and the difference is obvious.

[0165] Table 2

[0166]

[0167] As can be seen from Table 2, after aging, the test differences of torsion, tension, and shear force in different axial directions of Comparative Example 1, Example 5, and Example 6 are obviously discrete and uneven compared with Examples 1 to 4, with the largest discrete degree exceeding 15%, while the discrete degree of the best material performance of the present invention is less than 3%. This shows that the preparation method of the present invention significantly improves the overall performance consistency of the product, and the plastic encapsulation material of the present invention is more suitable for weakening the reliability defects caused by extreme conditions.

[0168] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high temperature resistant composite insulating column, characterized in that: It comprises a high temperature resistant composite insulating material and a metal structural part. The high temperature resistant composite insulating material is composed of epoxy resin, phenolic resin, inorganic filler, curing accelerator, mesoporous nano-silica reinforcing agent and auxiliary additives. The metal structural part is made of gold, silver, copper, aluminum or their alloys. The metal structural part is coated or bonded by the high temperature resistant composite insulating material. During the coating or bonding, periodic pressure is applied to the high temperature resistant composite insulating material in a rheological state. The mesoporous nano-silica reinforcing agent is composed of mesoporous nano-silica modified by a coupling agent with a particle size of 100 to 200 nm, the mesopore diameter is 10 to 30 nm, the reinforcing agent is loaded in the mesopores, the reinforcing agent is one or more of methylimidazole and aminoimidazole, and the coupling agent is one or more of silane, titanate, aluminum chelate and zirconium aluminum oxide.

2. The method for preparing a high temperature resistant composite insulating column according to claim 1, characterized in that: The method comprises the following preparation steps: S1: The high temperature resistant composite insulating material comprises the following raw materials in parts by weight: 10-20 parts of epoxy resin, 5-10 parts of phenolic resin, 80-50 parts of inorganic filler, 0.05-0.5 parts of curing accelerator, 0.5-1.5 parts of mesoporous nano-silica reinforcing agent and 0.1-2 parts of auxiliary additives; S2: Mixing The prepared raw materials are configured according to a preset weight ratio, and mixed evenly at a high speed to obtain a premix; S3: Rubber Mixing The premix is ​​mixed in an extruder at a mixing temperature of 100-110°C, and the extruder is extruded at high speed, and after cooling, the mixture is crushed to make cakes or slices for discharging; S4: Heating and curing The cake or slice is placed in the preheating mold cavity, and a metal structure is set in the preheating mold cavity. It is heated and cured at a constant heating rate. When the starting temperature (125-160°C) is reached, periodic pressure is applied until the cut-off temperature (140-170°C) is reached, and then the peak pressure is maintained until the gel curing is completed after the curing temperature.

3. The method for preparing the high temperature resistant composite insulating column according to claim 2, characterized in that: The epoxy resin is one or more of o-cresol epoxy resin, polyaromatic ring epoxy resin, and polyfunctional epoxy resin; the phenolic resin is one or more of linear phenolic resin, polyaromatic ring phenolic resin, and polyfunctional phenolic resin; the inorganic filler is one or more of crystalline rounded silica, fused spherical silica, spherical boron nitride, alumina, and aluminum nitride; and the curing accelerator is an organic phosphorus compound.

4. The method for preparing a high temperature resistant composite insulating column according to claim 3, characterized in that: The combination of the epoxy resin and the phenolic resin is one of a combination of a multifunctional epoxy resin and a linear phenolic resin and a combination of a multifunctional epoxy resin and a multifunctional phenolic resin.

5. The method for preparing a high temperature resistant composite insulating column according to claim 2, characterized in that: The auxiliary additives include one or more combinations of coupling agent 0.5-1.5 parts, flame retardant 0.5-1.5 parts, colorant 0.1-0.5 parts, release agent 0.3-0.5 parts and stress modifier 0.1-1.5 parts, wherein the release agent is one or more of palm wax, polyethylene wax and polyamide wax, the flame retardant is one or more of phosphate ester and aluminum hydroxide, the stress modifier is one of silicone oil, silicone resin and silicone rubber, and the colorant is one of carbon black with a particle size of 20-30 nm and black nano silica with a particle size of 20-30 nm.

6. The method for preparing a high temperature resistant composite insulating column according to claim 2, characterized in that: The periodic pressure peak value is 12-16 MPa, the valley value is 6-8 MPa, and the periodic frequency is 2-8 times / min.

7. The method for preparing a high temperature resistant composite insulating column according to claim 2, characterized in that: The initial temperature of the preheating model cavity is 105-115°C, the constant temperature rise rate is 4-12°C / min, and the curing temperature is 160-200°C.

8. The method for preparing a high temperature resistant composite insulating column according to claim 2, characterized in that: The starting temperature and the end temperature are determined according to the heat flow rate of the cake. During the temperature rise and curing process, the temperature when the heat flow rate rises to -0.1w / g is the starting temperature, and the temperature when the heat flow rate rises to 0.1w / g is the end temperature.

9. The method for preparing a high temperature resistant composite insulating column according to claim 8, characterized in that: The measured value of the heat flow rate is obtained under the conditions of non-periodic pressurization and 10°C / min temperature increase.

Citation Information

Patent Citations

  • Thermosetting resin compositions and prepregs and laminates made therefrom

    CN103992641B

  • An epoxy molding compound composition, an epoxy molding compound and its preparation method

    CN107446316B

  • Thermosetting resin composition as well as preparation method and application thereof

    CN111978726A

  • Process for preparing butyl-p-benzoylbenzoates

    EP0000502A1

  • Low dielectric-epoxy resin / mesoporous molecular sieve hybrid material and preparation method thereof

    CN101638505A