Chocolate glaze tile with anti-wear effect and preparation method thereof

By improving the formula of ceramic tile glaze, using raw materials such as quartz, alumina and silver-carrying composites to form mullite and aluminum polyphosphate structures, combined with the composite effect of zirconia, the wear resistance and antibacterial properties of ceramic tile glaze in the prior art are solved. The problem of insufficient results has achieved high wear resistance and antibacterial properties of the ceramic tile glaze layer.

CN118834058BActive Publication Date: 2024-12-06ZIBO GOLD LION KING TECH CERAMICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411318510.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-06
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

Existing ceramic tile glazes have shortcomings in wear resistance and antibacterial properties, and it is difficult to improve hardness and wear resistance at the same time.

Method used

By improving the glaze formula, adding raw materials such as quartz, alumina, silver-carrying composites and aluminum dihydrogen phosphate, the solid phase reaction is used to form a mullite structure and aluminium polyphosphate film, combining the composite effect of zirconia and zirconium silicate. Improve the wear resistance and hardness of the glaze layer, and achieve antibacterial effects through silver-carrying composites.

Benefits of technology

It significantly improves the wear resistance and hardness of the ceramic glaze layer, and also has excellent antibacterial properties, forming chocolate glaze ceramic tiles with excellent wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a chocolate glaze tile with anti-wear effect and a preparation method thereof, and belongs to the technical field of tile production. First, the preparation method of the chocolate glaze tile with anti-wear effect is as follows: kaolin, quartz, potassium feldspar, sodium feldspar and talcum powder are mixed and stirred, and then water is added thereto for stirring, ball milling and sieving, and then drying to obtain a mixed powder, and then the mixed powder is pressed into a tile body, and then pre-sintering is performed to obtain a tile body; the glaze is evenly coated on the surface of the tile body, and then dried, trimmed and polished to obtain a glazed tile body, and then fixedly fired and formed to obtain a chocolate glaze tile with anti-wear effect. Then, on the basis of the prior art, the invention improves the formula of the glaze and the preparation method of the tile, and finally realizes the improvement of the wear resistance, hardness and antibacterial properties of the prepared glazed tile.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of tile production, and in particular relates to a chocolate glaze tile with anti-wear effect and a preparation method thereof. Background Art

[0002] Among many decorative materials, ceramic tiles have the advantages of beautiful and diverse designs, convenient laying, and long service life, which makes them widely used in decoration, especially in the decoration of walls and floors. Among them, glazed tiles have the advantages of novel design and high gloss, and are favored by a large number of consumers. Among them, the wear resistance of the glazed surface of glazed tiles is an important indicator for evaluating its quality. In order to improve the wear resistance of the ceramic tile glaze, many improvements have been made in the existing technology:

[0003] The invention patent with application number 202111199737.7 discloses a wear-resistant digital ceramic glaze. The invention mainly improves the wear resistance of the glaze by adding zirconium silicate and zirconium oxide of different particle sizes. The invention patent with application number 202310294714.7 discloses a wear-resistant and corrosion-resistant ceramic glaze and its preparation method and application. The invention mainly improves the glaze formula ratio and precipitates mullite, calcium feldspar and aluminum phosphate film to ultimately achieve the purpose of improving the wear resistance and corrosion resistance of the glaze. The invention patent with application number 202211499622.4 discloses a wear-resistant ceramic glaze and its preparation method. The invention mainly improves the glaze formula, such as adding interrelated nano-scale chromium nitride and titanium nitride, to ultimately achieve the purpose of improving the hardness and wear resistance of the glaze layer. Summary of the invention

[0004] The present invention aims to further improve the formula of glaze and the preparation method of ceramic tiles on the basis of the existing technology, and finally prepare a chocolate glaze ceramic tile with excellent wear resistance, hardness and antibacterial properties.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] The method for preparing chocolate glaze ceramic tiles with anti-wear effect comprises the following steps:

[0007] S1. Mix kaolin, quartz, potassium feldspar, sodium feldspar and talc to obtain a mixture, add 45% to 60% of the mass of water to the mixture, ball mill for 1 to 2 hours, and sieve through 300 to 400 mesh to obtain a mixed slurry, dry the mixed slurry to a water content of 4% to 6% to obtain a mixed powder, press the mixed powder into a ceramic tile body, and pre-sinter to obtain a ceramic tile body;

[0008] S2. The glaze is evenly coated on the surface of the tile body, and then dried, trimmed and polished to obtain a glazed tile body, and then fired and formed to obtain a wear-resistant chocolate glaze tile.

[0009] Furthermore, the ceramic tile described in S1 comprises the following raw materials in parts by weight: 30-40 parts of kaolin, 18-20 parts of quartz, 12-20 parts of potassium feldspar, 12-15 parts of sodium feldspar and 7-10 parts of talc.

[0010] Furthermore, the specific process of pre-firing forming described in S1 is as follows: first, the temperature of the ceramic tile body is raised from room temperature to 750-800°C at a rate of 10°C / min, and then pre-fired at a constant temperature for 60-70 minutes, and finally naturally cooled to room temperature; the specific process of fixed-firing forming described in S2 is as follows: first, the temperature of the glazed ceramic tile body is raised from room temperature to 750-800°C at a rate of 10°C / min, and then the temperature is continued to be raised to 1280-1320°C at a rate of 6-7°C, and then the temperature is fired at a constant temperature for 1.5-2h, and finally cooled to room temperature naturally.

[0011] Further, the glaze in S2 is prepared by the following steps:

[0012] Potassium feldspar, quartz, calcined kaolin, zirconium silicate, aluminum oxide, iron oxide and silver-loaded composite were weighed in parts by mass, mixed, and ball-milled through a 200-300 mesh sieve to obtain a mixture. A binder and water were then added to the mixture with stirring, and the mixture was stirred and mixed for 1 hour to obtain a glaze.

[0013] Furthermore, the glaze comprises the following raw materials in parts by weight: 28 to 30 parts of potassium feldspar, 25 to 30 parts of quartz, 15 to 20 parts of calcined kaolin, 8 to 10 parts of zirconium silicate, 5 to 7 parts of aluminum oxide, 5 parts of iron oxide, 4 to 5 parts of silver-loaded composite, 10 to 13 parts of binder and 20 to 30 parts of water.

[0014] Furthermore, the adhesive is prepared by mixing aluminum dihydrogen phosphate, silica sol polyvinyl alcohol and water in a mass ratio of 50:13 to 15:7 to 15:100.

[0015] Furthermore, the silver-loaded composite is prepared by the following steps:

[0016] A1. Add urea to deionized water, stir until completely dissolved, add amyl alcohol, cyclohexane and hexadecyltrimethylammonium bromide, stir for 1-2 hours, add tetraethyl orthosilicate to obtain a suspension, place the suspension at 100-120° C. and stir for 12-24 hours, centrifuge, take a solid component, dry the solid component, calcine at 650-750° C. for 4-5 hours, grind and pass through 300 mesh to obtain a mesoporous silica carrier;

[0017] A2. Add yttrium nitrate hexahydrate, zirconium oxychloride octahydrate and silver nitrate to deionized water, stir for 20 to 30 minutes, then add a mesoporous silica carrier, stir magnetically for 20 to 30 minutes, adjust the pH of the system to 10.2 to 10.5, and let it stand at room temperature for 12 to 24 hours to obtain a precipitate, centrifuge, take a solid component, wash and dry the solid component, and then calcine it at 650 to 750° C. for 4 to 5 hours to obtain a silver-loaded composite.

[0018] Furthermore, the usage ratio of deionized water, urea, amyl alcohol, cyclohexane, hexadecyltrimethylammonium bromide and tetraethyl orthosilicate in A1 is 300 mL: 3.2-3.5 g: 4.5-5 mL: 150-200 mL: 13-15 g: 14-15 mL.

[0019] Furthermore, the usage ratio of the deionized water, yttrium nitrate hexahydrate, zirconium oxychloride octahydrate, silver nitrate and mesoporous silica carrier in A2 is 500 mL: 1.8-2.0 g: 1.2-1.5 g: 0.8-1 g: 20 g.

[0020] Beneficial effects of the present invention:

[0021] The invention provides a method for preparing chocolate glaze ceramic tiles with anti-wear effect, wherein the invention improves the formula of the glaze, and in the temperature rising process of sintering (>1100°C), quartz and alumina in the glaze form a mullite structure with excellent mechanical properties through solid phase reaction, thereby improving the wear resistance and hardness of the ceramic glaze layer. At the same time, the binder of the glaze of the invention contains aluminum dihydrogen phosphate solution, which loses water in the sintering process to form aluminum polyphosphate and exhibits excellent chemical bonding force. As the sintering temperature continues to rise (>1200°C), it will eventually sinter to form a dense and wear-resistant aluminum phosphate film, which is finally macroscopically manifested in improving the wear resistance and hardness of the ceramic glaze layer.

[0022] At the same time, the present invention adds a silver-loaded composite into the glaze. In the process of preparing the silver-loaded composite, the present invention first prepares a mesoporous silica carrier by a sol-gel method, and then further loads silver and yttrium. The silver ions and yttrium ions therein can achieve a synergistic antibacterial effect, and the zirconium oxychloride octahydrate in the silver-loaded composite forms zirconium oxide with excellent wear resistance and hardness after calcination. The composite of zirconium oxide and zirconium silicate can significantly improve the wear resistance and hardness of the ceramic glaze layer.

[0023] Finally, the present invention adds iron oxide to the glaze and strictly controls the production process of the ceramics to finally obtain a method for preparing chocolate glaze tiles with anti-wear effect. DETAILED DESCRIPTION

[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0025] Example 1

[0026] Preparation of silver-loaded complexes:

[0027] Urea was added to deionized water, and the mixture was stirred until the urea was completely dissolved. Pentanol, cyclohexane and hexadecyltrimethylammonium bromide were then added thereto. After the addition was completed, the mixture was stirred for 1 hour at room temperature. After the stirring was completed, a mixed solution was obtained. Tetraethyl orthosilicate was then added to the mixed solution with stirring, and the mixture was stirred for 30 minutes to obtain a suspension. The suspension was stirred at 100° C. for 12 hours, and then centrifuged to obtain a solid component. The solid component was then dried at 80° C. for 1 hour, and then calcined at 650° C. for 4 hours, and then ground and passed through 300 mesh to obtain a mesoporous silica carrier, wherein the amount ratio of deionized water, urea, pentanol, cyclohexane, hexadecyltrimethylammonium bromide and tetraethyl orthosilicate was 300 mL:3.2 g:4.5 mL:150 mL:13 g:14 mL. Then, yttrium nitrate hexahydrate, zirconium oxychloride octahydrate and silver nitrate were added to the deionized water with stirring, and the mixture was stirred for 20 minutes. Then, a mesoporous silica carrier was added thereto with stirring, and magnetic stirring was performed for 20 minutes. Then, a 10% ammonia solution by mass was added thereto to adjust the pH of the system to 10.2. After the adjustment, the mixture was allowed to stand at room temperature for 12 hours to obtain a precipitate, and the precipitate was centrifuged to obtain a solid component. The solid component was washed three times with anhydrous ethanol, and then the solid component was dried at 80° C. for 1 hour, and then calcined at 650° C. for 4 hours to obtain a silver-loaded composite, wherein the amount ratio of deionized water, yttrium nitrate hexahydrate, zirconium oxychloride octahydrate, silver nitrate and mesoporous silica carrier was 500 mL:1.8 g:1.2 g:0.8 g:20 g.

[0028] Example 2

[0029] Preparation of silver-loaded complex:

[0030] Urea was added to deionized water and stirred until the urea was completely dissolved. Pentanol, cyclohexane and hexadecyltrimethylammonium bromide were then added thereto. After the addition was completed, the mixture was stirred for 2 hours at room temperature. After the stirring was completed, a mixed solution was obtained. Tetraethyl orthosilicate was then added to the mixed solution and stirred for 50 minutes to obtain a suspension. The suspension was stirred at 120°C for 24 hours, and then centrifuged to obtain a solid component. The solid component was then dried at 100°C for 2 hours, and then calcined at 700°C for 5 hours, and then ground and passed through 300 mesh to obtain a mesoporous silica carrier, wherein the amount ratio of deionized water, urea, pentanol, cyclohexane, hexadecyltrimethylammonium bromide and tetraethyl orthosilicate was 300mL:3.4g:5mL:180mL:14g:15mL. Then, yttrium nitrate hexahydrate, zirconium oxychloride octahydrate and silver nitrate were added to the deionized water with stirring, and the mixture was stirred for 30 minutes. Then, a mesoporous silica carrier was added thereto with stirring, and magnetic stirring was performed for 30 minutes. Then, a 10% ammonia solution by mass was added thereto to adjust the pH of the system to 10.5. After the adjustment, the mixture was allowed to stand at room temperature for 24 hours to obtain a precipitate, and the mixture was centrifuged to obtain a solid component. The solid component was washed three times with anhydrous ethanol, and then the solid component was dried at 100° C. for 2 hours, and then calcined at 700° C. for 5 hours to obtain a silver-loaded composite, wherein the amount ratio of deionized water, yttrium nitrate hexahydrate, zirconium oxychloride octahydrate, silver nitrate and mesoporous silica carrier was 500 mL:2.0 g:1.4 g:1 g:20 g.

[0031] Example 3

[0032] Preparation of silver-loaded complex:

[0033] Urea was added to deionized water and stirred until the urea was completely dissolved. Pentanol, cyclohexane and hexadecyltrimethylammonium bromide were then added thereto. After the addition was completed, the mixture was stirred for 2 hours at room temperature. After the stirring was completed, a mixed solution was obtained. Tetraethyl orthosilicate was then added to the mixed solution and stirred for 50 minutes to obtain a suspension. The suspension was stirred at 120°C for 24 hours, and then centrifuged to obtain a solid component. The solid component was then dried at 100°C for 2 hours, and then calcined at 750°C for 5 hours, and then ground and passed through 300 mesh to obtain a mesoporous silica carrier, wherein the amount ratio of deionized water, urea, pentanol, cyclohexane, hexadecyltrimethylammonium bromide and tetraethyl orthosilicate was 300mL:3.5g:5mL:200mL:15g:15mL. Then, yttrium nitrate hexahydrate, zirconium oxychloride octahydrate and silver nitrate were added to the deionized water with stirring, and the mixture was stirred for 30 minutes. Then, a mesoporous silica carrier was added thereto with stirring, and magnetic stirring was performed for 30 minutes. Then, a 10% ammonia solution by mass was added thereto to adjust the pH of the system to 10.5. After the adjustment, the mixture was allowed to stand at room temperature for 24 hours to obtain a precipitate, which was centrifuged to obtain a solid component. The solid component was washed three times with anhydrous ethanol, and then the solid component was dried at 100° C. for 2 hours, and then calcined at 750° C. for 5 hours to obtain a silver-loaded composite, wherein the amount ratio of deionized water, yttrium nitrate hexahydrate, zirconium oxychloride octahydrate, silver nitrate and mesoporous silica carrier was 500 mL:2.0 g:1.5 g:1 g:20 g.

[0034] Comparative Example 1

[0035] Comparative Example 1 is the control group of Example 2, in which the yttrium nitrate hexahydrate in Example 2 is removed, and the other raw materials and the preparation process remain unchanged, and finally a silver-loaded composite is obtained.

[0036] Comparative Example 2

[0037] Comparative Example 2 is the control group of Example 2, except that the zirconium oxychloride octahydrate in Example 2 is removed, and the other raw materials and the preparation process remain unchanged, and finally a silver-loaded composite is obtained.

[0038] Comparative Example 3

[0039] Comparative Example 3 is the control group of Example 2, in which the mesoporous silica carrier in Example 2 is replaced with silica (item number S433676-2g, 50 μm, non-porous, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.), and the other raw materials and preparation process remain unchanged, and finally a silver-loaded composite is obtained.

[0040] Example 4

[0041] Prepare the glaze:

[0042] First, the glaze is composed of the following raw materials in parts by weight: 28 parts of potassium feldspar, 25 parts of quartz, 15 parts of calcined kaolin, 8 parts of zirconium silicate, 5 parts of aluminum oxide, 5 parts of iron oxide, 4 parts of the silver-loaded composite prepared in Example 1, 10 parts of a binder and 20 parts of water, wherein the binder is prepared by mixing aluminum dihydrogen phosphate, silica sol polyvinyl alcohol and water in a mass ratio of 50:13:7:100.

[0043] Then, the raw materials of the glaze are weighed according to the mass parts, mixed, and ball-milled through a 200-mesh sieve to obtain a mixture, and then a binder is added to the mixture with stirring, and the mixture is stirred and mixed for 1 hour to obtain a glaze.

[0044] Example 5

[0045] Prepare the glaze:

[0046] First, the glaze is composed of the following raw materials in parts by weight: 30 parts of potassium feldspar, 27 parts of quartz, 17 parts of calcined kaolin, 9 parts of zirconium silicate, 6 parts of aluminum oxide, 5 parts of iron oxide, 4 parts of the silver-loaded composite prepared in Example 2, 12 parts of a binder and 25 parts of water, wherein the binder is prepared by mixing aluminum dihydrogen phosphate, silica sol polyvinyl alcohol and water in a mass ratio of 50:14:12:100.

[0047] Then, the raw materials of the glaze are weighed according to the mass parts, mixed, and ball-milled through a 300-mesh sieve to obtain a mixture, and then a binder is added to the mixture with stirring, and the mixture is stirred and mixed for 1 hour to obtain a glaze.

[0048] Example 6

[0049] Prepare the glaze:

[0050] First, the glaze is composed of the following raw materials in parts by weight: 30 parts of potassium feldspar, 30 parts of quartz, 20 parts of calcined kaolin, 10 parts of zirconium silicate, 7 parts of aluminum oxide, 5 parts of iron oxide, 5 parts of the silver-loaded composite prepared in Example 3, 13 parts of a binder and 30 parts of water, wherein the binder is prepared by mixing aluminum dihydrogen phosphate, silica sol polyvinyl alcohol and water in a mass ratio of 50:15:15:100.

[0051] Then, the raw materials of the glaze are weighed according to the mass parts, mixed, and ball-milled through a 300-mesh sieve to obtain a mixture, and then a binder is added to the mixture with stirring, and the mixture is stirred and mixed for 1 hour to obtain a glaze.

[0052] Comparative Example 4

[0053] Comparative Example 4 is the control group of Example 5, in which the silver-loaded composite prepared in Example 2 in Example 5 is replaced by the silver-loaded composite prepared in Comparative Example 1, and the other raw materials and preparation process remain unchanged, to finally obtain a glaze.

[0054] Comparative Example 5

[0055] Comparative Example 5 is the control group of Example 5, in which the silver-loaded composite prepared in Example 2 in Example 5 is replaced by the silver-loaded composite prepared in Comparative Example 2, and the other raw materials and preparation process remain unchanged, to finally obtain a glaze.

[0056] Comparative Example 6

[0057] Comparative Example 6 is the control group of Example 5, in which the silver-loaded composite prepared in Example 2 in Example 5 is replaced by the silver-loaded composite prepared in Comparative Example 3, and the other raw materials and preparation process remain unchanged, to finally obtain a glaze.

[0058] Example 7

[0059] Preparation method of chocolate glaze tile with wear-resistant effect:

[0060] S1. First, the ceramic tile includes the following raw materials by weight: 30 parts of kaolin, 18 parts of quartz, 12 parts of potassium feldspar, 12 parts of sodium feldspar and 7 parts of talc. Then, weigh each raw material according to the above weight, mix and stir for 10 minutes to obtain a mixture, place the mixture in a ball mill, add 60% of the weight of the mixture into the mixture, ball mill for 1 hour, and then pass through a 300-mesh sieve to obtain a mixed slurry, dry the mixed slurry to a water content of 6% to obtain a mixed powder, and then press the mixed powder into a ceramic tile body. The ceramic tile body needs to be pre-fired. The specific process of pre-fired is as follows: first, the ceramic tile body is heated from room temperature to 750°C at a rate of 10°C / min, and then pre-fired at a constant temperature for 60 minutes, and finally naturally cooled to room temperature to obtain a ceramic tile body.

[0061] S2. The glaze prepared in Example 4 is evenly coated on the surface of the ceramic tile body, and then dried at 50°C for 10 minutes, and then trimmed and polished. The excess glaze is removed by trimming, and then polished to obtain a glazed ceramic tile body. The glazed ceramic tile body is fired and formed. The specific process of firing and forming is as follows: first, the temperature of the glazed ceramic tile body is raised from room temperature to 750°C at a rate of 10°C / min, and then the temperature is continued to be raised to 1280°C at a rate of 6°C, and then the ceramic tile is fired at a constant temperature for 1.5 hours, and finally naturally cooled to room temperature to obtain a wear-resistant chocolate glazed ceramic tile.

[0062] Example 8

[0063] Preparation method of chocolate glaze tile with wear-resistant effect:

[0064] S1. First, the ceramic tile includes the following raw materials by weight: 35 parts of kaolin, 20 parts of quartz, 15 parts of potassium feldspar, 15 parts of sodium feldspar and 8 parts of talc. Then, weigh each raw material according to the above weight, mix and stir for 30 minutes to obtain a mixture, place the mixture in a ball mill, add 50% of the weight of the mixture of water, ball mill for 2 hours, and then pass through a 400-mesh sieve to obtain a mixed slurry, dry the mixed slurry to a water content of 5% to obtain a mixed powder, and then press the mixed powder into a ceramic tile body. The ceramic tile body needs to be pre-fired. The specific process of pre-fired molding is as follows: first, the ceramic tile body is heated from room temperature to 780°C at a rate of 10°C / min, and then pre-fired at a constant temperature for 70 minutes, and finally naturally cooled to room temperature to obtain a ceramic tile body.

[0065] S2. The glaze prepared in Example 5 is evenly coated on the surface of the ceramic tile body, and then dried at 80°C for 20 minutes, and then trimmed and polished. The excess glaze is removed by trimming, and then polished to obtain a glazed ceramic tile body. The glazed ceramic tile body is fired and formed. The specific process of firing and forming is as follows: first, the temperature of the glazed ceramic tile body is raised from room temperature to 780°C at a rate of 10°C / min, and then the temperature is continued to be raised to 1300°C at a rate of 7°C, and then the ceramic tile is fired at a constant temperature for 2 hours, and finally naturally cooled to room temperature to obtain a wear-resistant chocolate glaze ceramic tile.

[0066] Example 9

[0067] Preparation method of chocolate glaze tile with wear-resistant effect:

[0068] S1. First, the ceramic tile includes the following raw materials by weight: 40 parts of kaolin, 20 parts of quartz, 20 parts of potassium feldspar, 15 parts of sodium feldspar and 10 parts of talc. Then, weigh each raw material according to the above weight, mix and stir for 30 minutes to obtain a mixture, place the mixture in a ball mill, add 45% of the weight of the mixture of water, ball mill for 2 hours, and then pass through a 400-mesh sieve to obtain a mixed slurry, dry the mixed slurry to a water content of 4% to obtain a mixed powder, and then press the mixed powder into a ceramic tile body. The ceramic tile body needs to be pre-fired. The specific process of pre-fired molding is as follows: first, the ceramic tile body is heated from room temperature to 800°C at a rate of 10°C / min, and then pre-fired at a constant temperature for 70 minutes, and finally naturally cooled to room temperature to obtain a ceramic tile body.

[0069] S2. The glaze prepared in Example 6 is evenly coated on the surface of the ceramic tile body, and then dried at 80°C for 20 minutes, and then trimmed and polished. The excess glaze is removed by trimming, and then polished to obtain a glazed ceramic tile body. The glazed ceramic tile body is fired and formed. The specific process of firing and forming is as follows: first, the temperature of the glazed ceramic tile body is raised from room temperature to 800°C at a rate of 10°C / min, and then the temperature is continued to be raised to 1320°C at a rate of 7°C, and then the ceramic tile is fired at a constant temperature for 2 hours. Finally, the ceramic tile is naturally cooled to room temperature to obtain a wear-resistant chocolate glaze ceramic tile.

[0070] Comparative Example 7

[0071] Comparative Example 7 is the control group of Example 8, in which the glaze prepared in Example 5 in Example 8 is replaced by the glaze in Comparative Example 4, and the other raw materials, raw material amounts and preparation steps remain unchanged, and finally a chocolate glaze tile with anti-wear effect is obtained.

[0072] Comparative Example 8

[0073] Comparative Example 8 is the control group of Example 8, in which the glaze prepared in Example 5 in Example 8 is replaced by the glaze in Comparative Example 5, and the other raw materials, raw material amounts and preparation steps remain unchanged, and finally a chocolate glaze tile with anti-wear effect is obtained.

[0074] Comparative Example 9

[0075] Comparative Example 9 is the control group of Example 8, in which the glaze prepared in Example 5 in Example 8 is replaced by the glaze in Comparative Example 6, and the remaining raw materials, raw material amounts and preparation steps remain unchanged, and finally a chocolate glaze tile with anti-wear effect is obtained.

[0076] The glaze layer of the chocolate glaze tiles with anti-wear effect prepared in Examples 7 to 9 and Comparative Examples 7 to 9 was tested, and the testing process was as follows:

[0077] Color: Use TS7700 spectrophotometer to test the color of the glaze on the surface of the tile, and record the test results in Table 1 below.

[0078] Wear resistance: Refer to the test method specified in GB / T 3810.7-2016 "Ceramic Tile Test Methods Part 7: Determination of Surface Wear Resistance of Glazed Tile", record the grinding revolutions for visible wear, and conduct graded evaluation. The data on the grinding revolutions and the results of the graded evaluation are recorded in Table 1 below.

[0079] Hardness: Refer to the test method in Appendix A of JC / T 908-2013 "Artificial Stone" for Mohs hardness test. The test principle is to use a standard ore of known hardness to manually scratch the tile glaze layer for testing, and record the test results in the following table 1

[0080] Antibacterial performance: Referring to the test method in Appendix A of JC / T 897-2014 "Antibacterial Performance of Antibacterial Ceramic Products", the antibacterial performance of the tile glaze layer against Staphylococcus aureus and Escherichia coli was tested respectively, that is, the antibacterial rate (%) was tested, and the test data of the antibacterial rate was recorded in the following Table 1.

[0081]

[0082] It can be seen from Table 1 that the glaze layer of the wear-resistant chocolate glazed tiles prepared in Examples 7 to 9 of the present invention has excellent wear resistance and hardness, and at the same time has excellent antibacterial properties against Staphylococcus aureus and Escherichia coli, and finally shows a dark brown color. Regardless of appearance or functionality, the wear-resistant chocolate glazed tiles prepared in Examples 7 to 9 of the present invention have outstanding substantial characteristics and significant progress.

[0083] It should be noted that, in this article, terms such as "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or equipment that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment.

[0084] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing chocolate glaze tiles with anti-wear effect, It is characterized in that The following steps are involved: S1. Mix kaolin, quartz, potassium feldspar, sodium feldspar and talc to obtain a mixture, add 45% to 60% of the mass of water to the mixture, ball mill for 1 to 2 hours, and sieve through 300 to 400 mesh to obtain a mixed slurry, dry the mixed slurry to a water content of 4% to 6% to obtain a mixed powder, press the mixed powder into a ceramic tile body, and pre-sinter to obtain a ceramic tile body; S2, evenly coating the glaze on the surface of the tile body, and then drying, trimming and grinding to obtain a glazed tile body, and then firing and forming to obtain a wear-resistant chocolate glaze tile; The glaze described in S2 is prepared by the following steps: Weigh potassium feldspar, quartz, calcined kaolin, zirconium silicate, aluminum oxide, iron oxide and silver-loaded composite according to mass parts, mix, and ball-mill through a 200-300 mesh sieve to obtain a mixture, and then stir and add a binder and water to the mixture, stir and mix for 1 hour to obtain a glaze; The glaze comprises the following raw materials by weight: 28 to 30 parts of potassium feldspar, 25 to 30 parts of quartz, 15 to 20 parts of calcined kaolin, 8 to 10 parts of zirconium silicate, 5 to 7 parts of aluminum oxide, 5 parts of iron oxide, 4 to 5 parts of silver-loaded composite, 10 to 13 parts of binder and 20 to 30 parts of water; The adhesive is prepared by mixing aluminum dihydrogen phosphate, silica sol, polyvinyl alcohol and water in a mass ratio of 50:13 to 15:7 to 15:100; The silver-loaded composite is prepared by the following steps: A1. Add urea to deionized water, stir until completely dissolved, add amyl alcohol, cyclohexane and hexadecyltrimethylammonium bromide, stir for 1-2 hours, add tetraethyl orthosilicate to obtain a suspension, place the suspension at 100-120° C. and stir for 12-24 hours, centrifuge, take a solid component, dry the solid component, calcine at 650-750° C. for 4-5 hours, grind and pass through 300 mesh to obtain a mesoporous silica carrier; A2, add yttrium nitrate hexahydrate, zirconium oxychloride octahydrate and silver nitrate to deionized water, stir for 20 to 30 minutes, then add mesoporous silica carrier thereto, stir magnetically for 20 to 30 minutes, then adjust the pH of the system to 10.2 to 10.5, then stand at room temperature for 12 to 24 hours to obtain a precipitate, centrifuge, take a solid component, wash and dry the solid component, and then calcine at 650 to 750 ° C for 4 to 5 hours to obtain a silver-loaded composite; The usage ratio of deionized water, yttrium nitrate hexahydrate, zirconium oxychloride octahydrate, silver nitrate and mesoporous silica carrier in A2 is 500mL:1.8-2.0g:1.2-1.5g:0.8-1g:20g.

2. The method for preparing the chocolate glaze tile with anti-wear effect according to claim 1, It is characterized in that The ceramic tile described in S1 comprises the following raw materials in parts by weight: 30-40 parts of kaolin, 18-20 parts of quartz, 12-20 parts of potassium feldspar, 12-15 parts of sodium feldspar and 7-10 parts of talc.

3. The method for preparing the chocolate glaze tile with anti-wear effect according to claim 1, It is characterized in that The specific process of pre-firing forming described in S1 is as follows: first, the temperature of the ceramic tile body is raised from room temperature to 750-800°C at a rate of 10°C / min, and then pre-fired at a constant temperature for 60-70 minutes, and finally naturally cooled to room temperature; the specific process of fixed-firing forming described in S2 is as follows: first, the temperature of the glazed ceramic tile body is raised from room temperature to 750-800°C at a rate of 10°C / min, and then continued to heat up to 1280-1320°C at a rate of 6-7°C, and then fired at a constant temperature for 1.5-2h, and finally naturally cooled to room temperature.

4. The method for preparing the chocolate glaze tile with anti-wear effect according to claim 1, It is characterized in that The usage ratio of deionized water, urea, amyl alcohol, cyclohexane, hexadecyltrimethylammonium bromide and tetraethyl orthosilicate described in A1 is 300mL:3.2-3.5g:4.5-5mL:150-200mL:13-15g:14-15mL.

5. Chocolate glazed tiles with anti-wear effect, It is characterized in that Prepared by the preparation method according to any one of claims 1 to 4.