A high-solid epoxy zinc-rich paint and preparation method thereof
By using components such as 4-aminopyrazole stannous chloride complex modified mica powder and rare earth salt in high-solid epoxy zinc-rich paint, the problems of poor density and easy cracking of paint film are solved, and the paint is improved The adhesion and corrosion resistance of the film achieve better protection effect.
Patent Information
- Application Number
- CN202411310750.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-09-20
AI Technical Summary
The existing high-solid epoxy zinc-rich paint has poor density, easy cracking of the paint film, and insufficient water and humidity resistance, resulting in corrosion and shedding.
The modified mica powder and rare earth salt are used to form layered arrangement and chemical reactions to improve the density and adhesion of the paint film, and enhance the corrosion resistance of the zinc powder.
It significantly improves the density, adhesion and corrosion resistance of the paint film, reduces pore density and brittleness, and enhances the mechanical strength and weather resistance of the paint film.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a high-solid epoxy zinc-rich paint and a preparation method thereof. Background Art
[0002] High-solid epoxy zinc-rich paint is a special industrial coating. Its zinc-rich formula enables it to form a solid protective layer after coating. It effectively prevents the substrate from corrosion by protecting the cathode through sacrificial anode, making it widely used in scenes such as bridges, marine facilities, petrochemical equipment and ships that require strong anti-corrosion ability and durability.
[0003] The existing high-solid epoxy zinc-rich paint uses a large amount of zinc powder, which makes the paint film brittle and poor in toughness. When the film thickness exceeds 150μm, it is easy to crack, especially at corners and welds, where paint film cracking and substrate corrosion often occur. In addition, the use of a large amount of zinc powder results in many pores after film formation, poor density of the paint film, poor water resistance, and poor resistance to moisture and heat, which easily leads to defects such as blistering, shedding, and rust.
[0004] Therefore, it is necessary to design a new high-solid epoxy zinc-rich paint to solve the technical problems of poor density and cracking of the paint film. Summary of the invention
[0005] In view of this, the present invention proposes a high-solid epoxy zinc-rich paint and a preparation method thereof, which solve the technical problems of poor density and paint film cracking of the existing high-solid epoxy zinc-rich paint.
[0006] The technical solution of the present invention is achieved as follows: On the one hand, the present invention provides a high-solid epoxy zinc-rich paint, comprising component A and component B, wherein the component A comprises liquid phenolic epoxy resin, solid epoxy resin, zinc powder, reactive diluent, mica powder, dispersant, anti-settling agent and mixed organic solvent, the component B comprises polyamide curing agent, silane coupling agent and mixed organic solvent, and the mica powder is modified mica powder loaded with 4-aminopyrazole stannous chloride complex.
[0007] After the modified mica powder loaded with 4-aminopyrazole stannous chloride complex is added to component A, the density of the paint film can be increased and the adhesion of the paint film can be improved. The principle is: mica powder has a flaky structure and can form a layered arrangement in the paint film, thereby improving the mechanical strength and density of the paint film, thereby reducing the presence of pores. 4-aminopyrazole stannous chloride complex contains amino groups and other active functional groups, which can chemically react or physically combine with other components in the paint (such as epoxy resin, curing agent), improve the bonding strength of the paint film, and enhance the toughness of the material. Stannous chloride can also interact with zinc powder to form a tighter cross-linked structure, thereby reducing the brittleness and pore density of the paint film.
[0008] On the basis of the above technical scheme, preferably, calculated by weight, the mass ratio of component A: component B is 15-20:1, wherein component A includes 8-12 parts of liquid phenolic epoxy resin, 6-15 parts of solid epoxy resin, 70-90 parts of zinc powder, 4-8 parts of mica powder, 1-3 parts of active diluent, 0.5-1 parts of dispersant, 1-3 parts of anti-settling agent and 6-8 parts of mixed organic solvent, and component B includes 4-6 parts of polyamide curing agent, 0.3-0.5 parts of silane coupling agent and 1-2 parts of mixed organic solvent.
[0009] On the basis of the above technical solution, preferably, the preparation method of the modified mica powder is:
[0010] S1, dissolving 4-aminopyrazole in an organic solvent to obtain a 4-aminopyrazole solution, dissolving stannous chloride in an organic solvent to obtain a stannous chloride solution, then mixing the 4-aminopyrazole solution and the stannous chloride solution, and reacting for 30-60 minutes to obtain a 4-aminopyrazole stannous chloride complex;
[0011] S2, immersing the mica powder in the 4-aminopyrazole stannous chloride complex for 1-2 hours, separating and drying after the reaction to obtain the modified mica powder loaded with the 4-aminopyrazole stannous chloride complex.
[0012] On the basis of the above technical solution, preferably, in step S1, the organic solvent is ethanol or isopropanol, the mass fraction of 4-aminopyrazole is 5%-10%, the mass fraction of stannous chloride is 10%-20%, and the volume ratio of 4-aminopyrazole solution:stannous chloride solution is 4-6:1.
[0013] On the basis of the above technical solution, preferably, the mica powder is first pre-treated by acidification and calcination and then immersed in 4-aminopyrazole stannous chloride complex, wherein the pre-treatment method comprises the following steps:
[0014] S21, adding mica powder to a dilute hydrochloric acid solution with a volume concentration of 10%-15%, stirring at 40° C.-60° C. for 0.5-1 h, and washing, filtering, and drying for later use after the reaction is completed;
[0015] S22, placing the acidified mica powder in a furnace, calcining at 400°C-500°C for 0.5-1h, cooling and grinding to obtain pretreated mica powder.
[0016] After acidification and calcination, the loading capacity of mica powder is increased. Specifically, the acidification treatment removes impurities and weak binding points on the surface of mica powder, making it easier for the surface to effectively bind with 4-aminopyrazole stannous chloride complex. Calcination improves the thermal stability and mechanical strength of mica powder, making it more excellent in the paint film and less likely to cause shedding and cracking. The pretreated mica powder has better dispersibility, so it can be more evenly distributed in the paint film, increasing the uniformity and consistency of the paint film.
[0017] On the basis of the above technical solution, preferably, the component A further comprises 3-5 parts by weight of 1-ethyl-3-methylimidazole methyl sulfate.
[0018] The addition of 1-ethyl-3-methylimidazolium methyl sulfate has the following effects: 1-ethyl-3-methylimidazolium methyl sulfate can improve the conductivity of the paint film and help reduce corrosion through the principle of electrochemical protection. 1-ethyl-3-methylimidazolium methyl sulfate stabilizes the mica powder, further promotes the combination of the complex and the resin matrix, and improves the overall mechanical properties and corrosion resistance. The good solubility and wettability of 1-ethyl-3-methylimidazolium methyl sulfate ensures the uniform distribution of the paint, reduces surface tension, and prevents cracking and bubble formation in the paint film.
[0019] On the basis of the above technical solution, preferably, the component A further comprises 4-8 parts by weight of a rare earth salt.
[0020] The addition of rare earth salts has the following effects: Rare earth salts can act as activators for zinc powder, and by enhancing the contact and reaction activity between zinc particles, improve the cathodic protection of zinc powder on the substrate, and help improve the overall protective performance of the paint film. Rare earth salts can promote the chemical bonding between the coating and the substrate and improve the adhesion of the paint film. Rare earth elements can also form stable compounds with metals, enhance interfacial bonding, and improve the wear resistance and scratch resistance of the paint film. Rare earth salts may increase the crosslinking degree of the paint film through interaction with the epoxy resin matrix, thereby enhancing the compactness of the coating, which helps to improve the weather resistance and moisture resistance of the coating. Rare earth elements such as cerium and yttrium have the ability to generate stable oxides under oxidizing conditions. These oxides can form a dense protective layer on the metal surface, reduce the penetration of oxygen and moisture, and thus improve the corrosion resistance of the metal.
[0021] On the basis of the above technical scheme, preferably, the solid epoxy resin is a bisphenol A epoxy resin, the active diluent is one of trimethylolpropane glycidyl ether, ethylene glycol glycidyl ether and tert-butyl glycidyl ether, the dispersant is one of Tego-760W, SN-5040 and DISPERBYK-191, the anti-settling agent is organic bentonite or oxidized polyethylene wax, the silane coupling agent is one or a combination of γ-aminopropyltriethoxysilane, vinyltrimethoxysilane, and 3-glycidyloxypropyltrimethoxysilane, the rare earth salt is one or a combination of cerium nitrate, yttrium nitrate and lanthanum nitrate; the mixed organic solvent in component A and component B is a mixture of ethylene glycol propyl ether, isopropanol, xylene and methyl isobutyl ketone, and the zinc powder particle size is 600-800 mesh.
[0022] On the other hand, the present invention also provides a method for preparing a high-solid epoxy zinc-rich paint, comprising the following steps:
[0023] S1, adding liquid phenolic epoxy resin, solid epoxy resin, reactive diluent, dispersant, anti-settling agent and 1-ethyl-3-methylimidazolium methyl sulfate to a mixed organic solvent, and stirring to obtain epoxy resin slurry;
[0024] S2, adding zinc powder and rare earth salt to epoxy resin slurry and stirring evenly, then adding mica powder and stirring evenly, and then filtering to obtain component A;
[0025] S3, adding a polyamide curing agent and a silane coupling agent into a mixed organic solvent and stirring the mixture, and then filtering the mixture to obtain a component B;
[0026] S4, mixing component A and component B evenly to obtain high solid epoxy zinc-rich paint.
[0027] On the basis of the above technical solution, preferably, the stirring speed is 1000-2000 r / min and the stirring time is 0.5-1 h.
[0028] The high-solid epoxy zinc-rich paint and the preparation method thereof of the present invention have the following beneficial effects compared with the prior art:
[0029] (1) Mica powder has a flaky structure and can form a layered arrangement in the paint film, thereby improving the mechanical strength and density of the paint film and reducing the presence of pores. 4-aminopyrazole stannous chloride complex contains amino groups and other active functional groups, which can react chemically or physically with other components in the paint (such as epoxy resin, curing agent) to improve the bonding strength of the paint film and enhance the toughness of the material. Stannous chloride can also interact with zinc powder to form a tighter cross-linked structure, thereby reducing the brittleness and pore density of the paint film. After the modified mica powder loaded with 4-aminopyrazole stannous chloride complex is added, the density and adhesion of the paint film are increased, thereby achieving the effect of enhancing corrosion resistance.
[0030] (2) The mica powder has a higher loading capacity after acidification and calcination, making it perform better in the paint film, increasing the uniformity and consistency of the paint film, and is less likely to cause falling off and cracking.
[0031] (3) The addition of 1-ethyl-3-methylimidazolium methyl sulfate can improve the stability of mica powder, promote the bonding of the complex with the resin matrix, and improve the mechanical properties and corrosion resistance of the paint film.
[0032] (4) The addition of rare earth salts can activate zinc powder and improve the protective properties of the paint film. At the same time, rare earth salts combined with other components can also enhance the adhesion, density and weather resistance of the paint film. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The liquid phenolic epoxy resin used in the present invention is a linear phenolic polyglycidyl ether (model F44), and the solid epoxy resin is a bisphenol A epoxy resin (model E-51, with a viscosity of 1200 mPa.s at 25°C), both of which are purchased from Shandong Deyuan Epoxy Technology Co., Ltd. The dispersant is one of Tego-760W (Germany Digo), SN-5040 (Japan San Nopco) and DISPERBYK-191 (Germany Bick). The polyamide curing agent contains an ultra-long carbon chain of more than C35 in the molecule, purchased from Zhenjiang Danbao Resin Co., Ltd., model 115-80. Silane coupling agents (γ-aminopropyl triethoxysilane, vinyl trimethoxysilane, 3-glycidyl ether oxypropyl trimethoxysilane) were purchased from Zhangjiagang Doer Chemical Co., Ltd.
[0035] Example 1
[0036] The high-solid epoxy zinc-rich paint of this embodiment includes component A and component B, wherein component A includes 8kg of liquid phenolic epoxy resin, 12kg of solid epoxy resin, 80kg of 800-mesh zinc powder, 6kg of modified mica powder loaded with 4-aminopyrazole stannous chloride complex, 2kg of trimethylolpropane glycidyl ether, 0.8kg of dispersant Tego-760W, 2kg of organic bentonite and 7kg of mixed organic solvent, and component B includes 5kg of polyamide curing agent, 0.4kg of γ-aminopropyltriethoxysilane and 1.5kg of mixed organic solvent.
[0037] The mixed organic solvent is prepared by mixing ethylene glycol propyl ether, isopropyl alcohol, xylene and methyl isobutyl ketone in a volume ratio of 1:1:1:1.
[0038] The preparation method of the modified mica powder loaded with 4-aminopyrazole stannous chloride complex is as follows:
[0039] S1, dissolving 4-aminopyrazole in ethanol or isopropanol to obtain a 4-aminopyrazole solution with a mass fraction of 8%, dissolving stannous chloride in ethanol or isopropanol to obtain a stannous chloride solution with a mass fraction of 15%, then mixing the 4-aminopyrazole solution and the stannous chloride solution in a volume ratio of 5:1, and reacting for 50 minutes to obtain a 4-aminopyrazole stannous chloride complex;
[0040] S2, immersing the mica powder in the 4-aminopyrazole stannous chloride complex for 1.5 hours, separating and drying after the reaction to obtain the modified mica powder loaded with the 4-aminopyrazole stannous chloride complex.
[0041] The preparation method of high solid epoxy zinc-rich paint comprises the following steps:
[0042] S1, adding liquid phenolic epoxy resin, solid epoxy resin, trimethylolpropane glycidyl ether, dispersant Tego-760W and organic bentonite into a mixed organic solvent, stirring at 2000 r / min for 1 hour to obtain epoxy resin slurry;
[0043] S2, adding zinc powder to the epoxy resin slurry, stirring at 1800 r / min for 1 h, then adding modified mica powder, stirring at 1800 r / min for 1 h, and then filtering to obtain component A;
[0044] S3, adding polyamide curing agent and γ-aminopropyltriethoxysilane into the mixed organic solvent, stirring at 1500 r / min for 1 hour, and then filtering to obtain component B;
[0045] S4, mixing component A and component B in a mass ratio of 18:1, stirring at 1000 r / min for 0.5 h, to obtain a high-solid epoxy zinc-rich paint.
[0046] Example 2
[0047] The difference between Example 2 and Example 1 is that when preparing the modified mica powder loaded with 4-aminopyrazole stannous chloride complex, the mica powder is first pretreated by acidification and calcination and then immersed in the 4-aminopyrazole stannous chloride complex. The rest of the contents are the same as Example 1.
[0048] The preparation method of modified mica powder loaded with 4-aminopyrazole stannous chloride complex is as follows:
[0049] S1, dissolving 4-aminopyrazole in ethanol or isopropanol to obtain a 4-aminopyrazole solution with a mass fraction of 8%, dissolving stannous chloride in ethanol or isopropanol to obtain a stannous chloride solution with a mass fraction of 15%, then mixing the 4-aminopyrazole solution and the stannous chloride solution in a volume ratio of 5:1, and reacting for 50 minutes to obtain a 4-aminopyrazole stannous chloride complex;
[0050] S2, adding mica powder into a diluted hydrochloric acid solution with a volume concentration of 15%, stirring at 50°C for 1 hour, washing, filtering, drying, placing in a furnace, calcining at 450°C for 1 hour, cooling and grinding to obtain pretreated mica powder.
[0051] S3, immersing the pretreated mica powder in 4-aminopyrazole stannous chloride complex for 1.5 hours, separating and drying after the reaction is completed to obtain modified mica powder loaded with 4-aminopyrazole stannous chloride complex.
[0052] Example 3
[0053] The difference between Example 3 and Example 2 is that 4 kg of 1-ethyl-3-methylimidazole methyl sulfate salt is added to component A. When preparing high solid epoxy zinc-rich paint, liquid phenolic epoxy resin, solid epoxy resin, trimethylolpropane glycidyl ether, dispersant, anti-settling agent and 1-ethyl-3-methylimidazole methyl sulfate salt are added to a mixed organic solvent, stirred at 2000 r / min for 1 hour to prepare epoxy resin slurry. The rest of the content is the same as Example 2.
[0054] Example 4
[0055] The difference between Example 4 and Example 3 is that 6 kg of cerium nitrate is added to component A. When preparing component A of high solid epoxy zinc-rich paint, zinc powder and cerium nitrate are added to epoxy resin slurry, stirred at 1800 r / min for 1 hour, and then modified mica powder is added, stirred at 1800 r / min for 1 hour, and then filtered to obtain component A. The rest of the contents are the same as in Example 3.
[0056] Example 5
[0057] The high-solid epoxy zinc-rich paint of this embodiment includes component A and component B, wherein component A includes 9kg of liquid phenolic epoxy resin, 15kg of solid epoxy resin, 90kg of 600-mesh zinc powder, 4kg of modified mica powder loaded with 4-aminopyrazole stannous chloride complex, 1kg of ethylene glycol glycidyl ether, 1kg of dispersant SN-5040, 1kg of oxidized polyethylene wax, 5kg of 1-ethyl-3-methylimidazole methyl sulfate, 4kg of yttrium nitrate and 6kg of mixed organic solvent, and component B includes 5.5kg of polyamide curing agent, 0.3kg of vinyl trimethoxy silane and 1kg of mixed organic solvent.
[0058] The mixed organic solvent is prepared by mixing ethylene glycol propyl ether, isopropyl alcohol, xylene and methyl isobutyl ketone in a volume ratio of 1:1:1:1.
[0059] The preparation method of the modified mica powder loaded with 4-aminopyrazole stannous chloride complex is as follows:
[0060] S1, dissolving 4-aminopyrazole in ethanol or isopropanol to obtain a 5% by mass 4-aminopyrazole solution, dissolving stannous chloride in ethanol or isopropanol to obtain a 12% by mass stannous chloride solution, then mixing the 4-aminopyrazole solution and the stannous chloride solution in a volume ratio of 5:1, and reacting for 50 minutes to obtain a 4-aminopyrazole stannous chloride complex.
[0061] S2, adding mica powder into a diluted hydrochloric acid solution with a volume concentration of 10%, stirring at 40°C for 1 hour, washing, filtering, drying, placing in a furnace, calcining at 500°C for 0.5 hour, cooling and grinding to obtain pretreated mica powder.
[0062] S3, immersing the mica powder in the 4-aminopyrazole stannous chloride complex for 2 hours, separating and drying after the reaction is completed to obtain the modified mica powder loaded with the 4-aminopyrazole stannous chloride complex.
[0063] The preparation method of high solid epoxy zinc-rich paint comprises the following steps:
[0064] S1, adding liquid phenolic epoxy resin, solid epoxy resin, ethylene glycol glycidyl ether, dispersant SN-5040, oxidized polyethylene wax and 1-ethyl-3-methylimidazole methyl sulfate into a mixed organic solvent, stirring at 2000 r / min for 0.5 h to obtain epoxy resin slurry.
[0065] S2, adding zinc powder and yttrium nitrate to the epoxy resin slurry, stirring at 1500 r / min for 1 hour, then adding modified mica powder, stirring at 1000 r / min for 0.5 hour, and then filtering to obtain component A.
[0066] S3, adding polyamide curing agent and vinyl trimethoxy silane into the mixed organic solvent, stirring at 1000 r / min for 1 hour, and then filtering to obtain component B.
[0067] S4, mixing component A and component B in a mass ratio of 15:1, stirring at 1000 r / min for 0.5 h, to obtain a high-solid epoxy zinc-rich paint.
[0068] Example 6
[0069] The high-solid epoxy zinc-rich paint of this embodiment includes component A and component B, wherein component A includes 9.5 kg of liquid phenolic epoxy resin, 6 kg of solid epoxy resin, 75 kg of 700-mesh zinc powder, 8 kg of modified mica powder loaded with 4-aminopyrazole stannous chloride complex, 3 kg of tert-butyl glycidyl ether, 0.5 kg of dispersant DISPERBYK-191, 1.5 kg of organic bentonite, 3 kg of 1-ethyl-3-methylimidazole methyl sulfate, 7 kg of lanthanum nitrate and 6.5 kg of mixed organic solvent, and component B includes 4 kg of polyamide curing agent, 0.5 kg of 3-glycidyloxypropyltrimethoxysilane and 2 kg of mixed organic solvent.
[0070] The mixed organic solvent is prepared by mixing ethylene glycol propyl ether, isopropyl alcohol, xylene and methyl isobutyl ketone in a volume ratio of 1:1:1:1.
[0071] The preparation method of the modified mica powder loaded with 4-aminopyrazole stannous chloride complex is as follows:
[0072] S1, dissolving 4-aminopyrazole in ethanol or isopropanol to obtain a 7% by mass 4-aminopyrazole solution, dissolving stannous chloride in ethanol or isopropanol to obtain a 18% by mass stannous chloride solution, then mixing the 4-aminopyrazole solution and the stannous chloride solution in a volume ratio of 6:1, reacting for 30 minutes to obtain a 4-aminopyrazole stannous chloride complex.
[0073] S2, adding mica powder into a diluted hydrochloric acid solution with a volume concentration of 15%, stirring and reacting at 60°C for 0.5h, washing, filtering, drying, placing in a furnace, calcining at 400°C for 1h, cooling and grinding to obtain pretreated mica powder.
[0074] S3, immersing the mica powder in the 4-aminopyrazole stannous chloride complex for 1 hour, separating and drying after the reaction is completed to obtain the modified mica powder loaded with the 4-aminopyrazole stannous chloride complex.
[0075] The preparation method of high solid epoxy zinc-rich paint comprises the following steps:
[0076] S1, adding liquid phenolic epoxy resin, solid epoxy resin, tert-butyl glycidyl ether, dispersant DISPERBYK-191, organic bentonite and 1-ethyl-3-methylimidazole methyl sulfate into a mixed organic solvent, stirring at 1500 r / min for 1 hour to obtain epoxy resin slurry.
[0077] S2, adding zinc powder and lanthanum nitrate to the epoxy resin slurry, stirring at 2000 r / min for 1 hour, then adding modified mica powder, stirring at 2000 r / min for 0.5 hour, and then filtering to obtain component A.
[0078] S3, adding polyamide curing agent and 3-glycidyloxypropyltrimethoxysilane into the mixed organic solvent, stirring at 1500 r / min for 0.5 h, and then filtering to obtain component B.
[0079] S4, mixing component A and component B in a mass ratio of 17:1, stirring at 2000 r / min for 0.5 h, to obtain a high-solid epoxy zinc-rich paint.
[0080] Example 7
[0081] The high-solid epoxy zinc-rich paint of this embodiment includes component A and component B, wherein component A includes 7.5 kg of liquid phenolic epoxy resin, 10 kg of solid epoxy resin, 85 kg of 600-mesh zinc powder, 5 kg of modified mica powder loaded with 4-aminopyrazole stannous chloride complex, 1.5 kg of trimethylolpropane glycidyl ether, 0.9 kg of dispersant Tego-760W, 2.5 kg of oxidized polyethylene wax, 3.5 kg of 1-ethyl-3-methylimidazole methyl sulfate, 5 kg of cerium nitrate and 7.5 kg of mixed organic solvent, and component B includes 4.5 kg of polyamide curing agent, 0.35 kg of γ-aminopropyltriethoxysilane and 1.3 kg of mixed organic solvent.
[0082] The mixed organic solvent is prepared by mixing ethylene glycol propyl ether, isopropyl alcohol, xylene and methyl isobutyl ketone in a volume ratio of 1:1:1:1.
[0083] The preparation method of the modified mica powder loaded with 4-aminopyrazole stannous chloride complex is as follows:
[0084] S1, dissolving 4-aminopyrazole in ethanol or isopropanol to obtain a 4-aminopyrazole solution with a mass fraction of 9%, dissolving stannous chloride in ethanol or isopropanol to obtain a stannous chloride solution with a mass fraction of 20%, then mixing the 4-aminopyrazole solution and the stannous chloride solution in a volume ratio of 4.5:1, and reacting for 40 minutes to obtain a 4-aminopyrazole stannous chloride complex.
[0085] S2, adding mica powder into a diluted hydrochloric acid solution with a volume concentration of 14%, stirring at 45°C for 1 hour, washing, filtering, drying, placing in a furnace, calcining at 420°C for 1 hour, cooling and grinding to obtain pretreated mica powder.
[0086] S3, immersing the mica powder in the 4-aminopyrazole stannous chloride complex for 2 hours, separating and drying after the reaction is completed to obtain the modified mica powder loaded with the 4-aminopyrazole stannous chloride complex.
[0087] The preparation method of high solid epoxy zinc-rich paint comprises the following steps:
[0088] S1, adding liquid phenolic epoxy resin, solid epoxy resin, trimethylolpropane glycidyl ether, dispersant Tego-760W, oxidized polyethylene wax and 1-ethyl-3-methylimidazole methyl sulfate into a mixed organic solvent, stirring at 1000 r / min for 1 hour to obtain epoxy resin slurry.
[0089] S2, adding zinc powder and cerium nitrate into epoxy resin slurry, stirring at 1000 r / min for 1 h, then adding modified mica powder, stirring at 2000 r / min for 0.5 h, and then filtering to obtain component A.
[0090] S3, adding the polyamide curing agent and γ-aminopropyltriethoxysilane into the mixed organic solvent, stirring at 2000 r / min for 0.5 h, and then filtering to obtain component B.
[0091] S4, mixing component A and component B in a mass ratio of 20:1, stirring at 1000 r / min for 1 h, to obtain a high-solid epoxy zinc-rich paint.
[0092] Example 8
[0093] The high-solid epoxy zinc-rich paint of this embodiment includes component A and component B, wherein component A includes 8.5 kg of liquid phenolic epoxy resin, 8 kg of solid epoxy resin, 90 kg of 800-mesh zinc powder, 7 kg of modified mica powder loaded with 4-aminopyrazole stannous chloride complex, 2.5 kg of ethylene glycol glycidyl ether, 0.7 kg of dispersant SN-5040, 3 kg of organic bentonite, 4.5 kg of 1-ethyl-3-methylimidazole methyl sulfate, 8 kg of yttrium nitrate and 8 kg of mixed organic solvent, and component B includes 6 kg of polyamide curing agent, 0.45 kg of vinyl trimethoxy silane and 1.8 kg of mixed organic solvent.
[0094] The mixed organic solvent is prepared by mixing ethylene glycol propyl ether, isopropyl alcohol, xylene and methyl isobutyl ketone in a volume ratio of 1:1:1:1.
[0095] The preparation method of the modified mica powder loaded with 4-aminopyrazole stannous chloride complex is as follows:
[0096] S1, dissolving 4-aminopyrazole in ethanol or isopropanol to obtain a 10% by mass 4-aminopyrazole solution, dissolving stannous chloride in ethanol or isopropanol to obtain a 10% by mass stannous chloride solution, then mixing the 4-aminopyrazole solution and the stannous chloride solution in a volume ratio of 5.5:1, and reacting for 40 minutes to obtain a 4-aminopyrazole stannous chloride complex.
[0097] S2, adding mica powder into a diluted hydrochloric acid solution with a volume concentration of 10%, stirring at 55°C for 1 hour, washing, filtering, drying, placing in a furnace, calcining at 480°C for 1 hour, cooling and grinding to obtain pretreated mica powder.
[0098] S3, immersing the mica powder in the 4-aminopyrazole stannous chloride complex for 1.5 hours, separating and drying after the reaction is completed to obtain the modified mica powder loaded with the 4-aminopyrazole stannous chloride complex.
[0099] The preparation method of high solid epoxy zinc-rich paint comprises the following steps:
[0100] S1, adding liquid phenolic epoxy resin, solid epoxy resin, ethylene glycol glycidyl ether, dispersant SN-5040, organic bentonite and 1-ethyl-3-methylimidazole methyl sulfate into a mixed organic solvent, stirring at 2000 r / min for 0.5 h, to obtain epoxy resin slurry.
[0101] S2, adding zinc powder and yttrium nitrate to the epoxy resin slurry, stirring at 1500 r / min for 1 hour, then adding modified mica powder, stirring at 1300 r / min for 1 hour, and then filtering to obtain component A.
[0102] S3, adding polyamide curing agent and vinyl trimethoxy silane into the mixed organic solvent, stirring at 1000 r / min for 1 hour, and then filtering to obtain component B.
[0103] S4, mixing component A and component B in a mass ratio of 19:1, stirring at 1000 r / min for 1 h, to obtain a high-solid epoxy zinc-rich paint.
[0104] Comparative Example 1
[0105] The difference between Comparative Example 1 and Example 1 is that the modified mica powder loaded with 4-aminopyrazole stannous chloride complex is missing, and the rest of the contents are the same.
[0106] Comparative Example 2
[0107] The difference between Comparative Example 2 and Example 1 is that the mica powder is ordinary mica powder and is not modified, and the rest of the contents are the same.
[0108] Comparative Example 3
[0109] The difference between Comparative Example 3 and Example 1 is that the mica powder only loads 4-aminopyrazole and lacks stannous chloride, and the rest of the contents are the same.
[0110] Comparative Example 4
[0111] The difference between Comparative Example 4 and Example 1 is that the amount of the modified mica powder loaded with 4-aminopyrazole stannous chloride complex exceeds the specified range, and the specific amount is 15 kg, and the rest of the contents are the same.
[0112] Comparative Example 5
[0113] The difference between Comparative Example 5 and Example 3 is that the amount of 1-ethyl-3-methylimidazole methyl sulfate used exceeds the specified range, and the specific amount used is 8 kg, and the rest of the contents are the same.
[0114] Comparative Example 6
[0115] The difference between Comparative Example 6 and Example 4 is that the amount of rare earth salt used exceeds the specified range, and the specific amount used is 12 kg, and the rest of the contents are the same.
[0116] The high-solid epoxy zinc-rich paint prepared in the above embodiments and comparative examples was sprayed or brushed on the surface of the steel plate and the surface of the weld with a thickness of 160 μm. It was cured for 10 days under standard conditions and its performance was tested. The results are shown in Table 1.
[0117] Adhesion test refers to GB / T 1720, impact resistance test refers to GB / T 1732, pull-off adhesion test refers to GB / T 5210, and salt spray resistance test refers to GB / T 1771. Moisture and heat resistance test refers to GB / T1740-2007, 38±2℃ temperature, 90±2% humidity, record the time when wrinkles appear.
[0118] Table 1 Properties of high solid epoxy zinc-rich paint
[0119]
[0120] As shown in Table 1, it can be seen from Examples 1-3 and Comparative Example 1 that after adding the modified mica powder loaded with 4-aminopyrazole stannous chloride complex, a tighter cross-linking structure is formed with other components, which increases the density of the paint film, thereby improving the strength, adhesion, salt spray resistance and moisture and heat resistance of the paint film. When a single 4-aminopyrazole or stannous chloride is loaded, the performance of the epoxy zinc-rich paint is reduced, thereby proving the technical effect of the mica powder modified with 4-aminopyrazole stannous chloride complex.
[0121] It can be seen from Examples 1-4 that after the mica powder is acidified and calcined, the loading amount of 4-aminopyrazole stannous chloride complex is increased, thereby improving the comprehensive performance of the paint film. After the addition of 1-ethyl-3-methylimidazole methyl sulfate, the combination of the paint film and the substrate is enhanced, and the adhesion and corrosion resistance (salt spray resistance and heat and humidity resistance) are improved. After the addition of rare earth salt, the zinc powder is activated and the anti-corrosion performance of the zinc powder is enhanced. At the same time, the combination of rare earth salt and other components also improves the adhesion and strength of the paint film.
[0122] Comparative Examples 4-6 show that when the amount of modified mica powder, 1-ethyl-3-methylimidazolium methyl sulfate, and rare earth salt exceeds the dosage range, the adhesion, erosion resistance, and corrosion resistance (salt spray resistance and heat and humidity resistance) of the epoxy zinc-rich paint are adversely affected. This is because:
[0123] Excessive amount of modified mica powder will lead to uneven internal adhesion of the paint layer, reduced density, and prone to micropores or cracks, thereby reducing its overall performance.
[0124] Excessive 1-ethyl-3-methylimidazolium methyl sulfate salt will cause internal stress during the curing process of epoxy zinc-rich paint, affecting the overall adhesion. At the same time, due to the characteristics of imidazole salts, excessive amount can easily cause the cured film to be too rigid, reduce flexibility and toughness, and make it more likely to break under impact.
[0125] A moderate amount of rare earth elements can improve the adhesion of the coating, but an excessive amount may lead to an incomplete reaction, and the remaining salts will form weak points in the coating. Under high stress, too much rare earth salt may form a fragile interface inside it, causing the coating to lose integrity under impact conditions. Excessive rare earth salts may also have an adverse effect on the internal structure of the coating, as it may promote the formation of cracks or holes and increase the electrochemical corrosion path.
[0126] Modified mica powder, 1-ethyl-3-methylimidazolium methyl sulfate, and rare earth salts all play an important role in epoxy zinc-rich paint. By adding appropriate amounts, they can synergistically improve the corrosion resistance of the coating. However, exceeding the appropriate amount will lead to a series of problems such as uneven structure, internal stress accumulation, poor film formation, and reduced density. These problems will directly or indirectly affect the mechanical properties and corrosion resistance of the coating, increase the risk of penetration of external corrosive media, and reduce the overall protection effect.
[0127] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high solid epoxy zinc-rich paint, characterized in that: The invention comprises a component A and a component B, wherein the mass ratio of the component A to the component B is 15-20:1, calculated by weight fraction, wherein the component A comprises 8-12 parts of liquid phenolic epoxy resin, 6-15 parts of solid epoxy resin, 70-90 parts of zinc powder, 4-8 parts of mica powder, 1-3 parts of active diluent, 0.5-1 parts of dispersant, 1-3 parts of anti-settling agent and 6-8 parts of mixed organic solvent, and the component B comprises 4-6 parts of polyamide curing agent, 0.3-0.5 parts of silane coupling agent and 1-2 parts of mixed organic solvent; The mica powder is a modified mica powder loaded with 4-aminopyrazole stannous chloride complex, and the preparation method is as follows: S1, dissolving 4-aminopyrazole in an organic solvent to obtain a 4-aminopyrazole solution, dissolving stannous chloride in an organic solvent to obtain a stannous chloride solution, then mixing the 4-aminopyrazole solution and the stannous chloride solution, and reacting for 30-60 minutes to obtain a 4-aminopyrazole stannous chloride complex; S2, immersing the mica powder in the 4-aminopyrazole stannous chloride complex for 1-2 hours, separating and drying after the reaction to obtain the modified mica powder loaded with the 4-aminopyrazole stannous chloride complex.
2. A high solid epoxy zinc-rich paint as claimed in claim 1, characterized in that: In step S1, the organic solvent is ethanol or isopropanol, the mass fraction of 4-aminopyrazole is 5%-10%, the mass fraction of stannous chloride is 10%-20%, and the volume ratio of 4-aminopyrazole solution:stannous chloride solution is 4-6:
1.
3. A high solid epoxy zinc-rich paint as claimed in claim 1, characterized in that: The mica powder is first pre-treated by acidification and calcination and then immersed in 4-aminopyrazole stannous chloride complex, wherein the pre-treatment method comprises the following steps: S21, adding mica powder to a dilute hydrochloric acid solution with a volume concentration of 10%-15%, stirring at 40° C.-60° C. for 0.5-1 h, and washing, filtering, and drying for later use after the reaction is completed; S22, placing the acidified mica powder in a furnace, calcining at 400°C-500°C for 0.5-1h, cooling and grinding to obtain pretreated mica powder.
4. The high solid epoxy zinc-rich paint according to claim 1, characterized in that: The component A further comprises 3-5 parts by weight of 1-ethyl-3-methylimidazole methyl sulfate.
5. A high solid epoxy zinc-rich paint as claimed in claim 4, characterized in that: The A component further comprises 4-8 parts by weight of a rare earth salt.
6. A high solid epoxy zinc-rich paint as claimed in claim 5, characterized in that: The solid epoxy resin is a bisphenol A epoxy resin, the active diluent is one of trimethylolpropane glycidyl ether, ethylene glycol glycidyl ether and tert-butyl glycidyl ether, the dispersant is one of Tego-760W, SN-5040 and DISPERBYK-191, the anti-settling agent is organic bentonite or oxidized polyethylene wax, the silane coupling agent is one or a combination of γ-aminopropyl triethoxysilane, vinyl trimethoxysilane and 3-glycidyloxypropyl trimethoxysilane, the rare earth salt is one or a combination of cerium nitrate, yttrium nitrate and lanthanum nitrate; the mixed organic solvent in component A and component B is a mixture of ethylene glycol propyl ether, isopropanol, xylene and methyl isobutyl ketone, and the particle size of the zinc powder is 600-800 meshes.
7. The method for preparing a high-solid epoxy zinc-rich paint according to claim 6, characterized in that: The following steps are involved: S1, adding liquid phenolic epoxy resin, solid epoxy resin, reactive diluent, dispersant, anti-settling agent and 1-ethyl-3-methylimidazolium methyl sulfate to a mixed organic solvent, and stirring to obtain epoxy resin slurry; S2, adding zinc powder and rare earth salt to epoxy resin slurry and stirring evenly, then adding mica powder and stirring evenly, and then filtering to obtain component A; S3, adding a polyamide curing agent and a silane coupling agent into a mixed organic solvent and stirring the mixture, and then filtering the mixture to obtain a component B; S4, mixing component A and component B evenly to obtain high solid epoxy zinc-rich paint.
8. The method for preparing a high-solid epoxy zinc-rich paint according to claim 7, characterized in that: The stirring speed is 1000-2000r / min and the stirring time is 0.5-1h.