Corrosion-resistant high-strength aluminum alloy and preparation method thereof
By adding silica-loaded silicon nitride microspheres to the aluminum alloy and using a specific process, a corrosion-resistant and high-strength aluminum alloy is formed, which solves the problem of aluminum alloys being easily corroded in humid environments and significantly improves its strength and acid resistance. Alkaline performance expands application scenarios.
Patent Information
- Application Number
- CN202410880720.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-02
- Publication Date
- 2024-10-25
AI Technical Summary
Aluminum alloy is prone to corrosion in humid environments, which limits its scope of use. In particular, its poor acid and alkali resistance makes it difficult to apply in harsh scenarios.
By adding silica-loaded silicon nitride microspheres to the aluminum alloy, and using ball milling mixing, vacuum hot-pressing sintering and solid solution treatment, a corrosion-resistant and high-strength aluminum alloy is formed. The silica-loaded silicon nitride microspheres are The solid solution grains are dispersed or granular, which improves the strength and hardness of the material.
It significantly improves the tensile strength, yield strength and elongation of aluminum alloy, enhances its resistance to salt spray and alkali, expands use scenarios, and is suitable for large-scale promotion.
Smart Images

Figure BDA0004924410390000091 
Figure BDA0004924410390000111
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum alloy materials, and in particular to a corrosion-resistant high-strength aluminum alloy and a preparation method thereof. Background Art
[0002] Aluminum alloy refers to an alloy formed by adding a certain amount of other metal elements to aluminum as the base material. It is a light metal material. Aluminum alloy has high strength and is easy to process. It is widely used in the fields of shipbuilding, aviation, construction, etc. However, in a humid environment, the surface of aluminum alloy is easily corroded, which limits its scope of use.
[0003] Constructing a hydrophobic surface on an aluminum alloy can greatly improve the protective power of the aluminum alloy. Usually, the hydrophobic surface is made by adding a film layer on the surface of the aluminum alloy, including spraying, physical vapor deposition, chemical vapor deposition, etc. Since aluminum is easily oxidized, the surface of the aluminum alloy is usually covered with aluminum oxide, and aluminum oxide is an amphoteric oxide that can react with both acid and alkali. Due to the loose and porous structure of aluminum oxide, the acid and alkali resistance of the aluminum alloy is poor. After applying the nano-coating, the acid and alkali resistance of the aluminum alloy has been greatly improved, but the aluminum alloy still cannot be used as a substrate in harsh usage scenarios.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] One of the objects of the present invention is to provide a corrosion-resistant high-strength aluminum alloy to alleviate at least one of the above-mentioned technical problems in the prior art.
[0006] A second object of the present invention is to provide a method for preparing a corrosion-resistant high-strength aluminum alloy.
[0007] In order to solve the above-mentioned technical problems, the present invention particularly adopts the following technical solutions:
[0008] A first aspect of the present invention provides a corrosion-resistant high-strength aluminum alloy comprising silicon dioxide-loaded silicon nitride microspheres and an aluminum alloy.
[0009] Furthermore, the aluminum alloy includes the following elements in percentage by mass: Zr 0.01% to 0.6%, Er 0.03-0.2%, Mg 0.1-2%, Ti 0.1-3%, and the balance is Al.
[0010] Preferably, the particle size of the silicon dioxide-loaded silicon nitride microspheres is 0.2 μm to 0.9 μm.
[0011] Preferably, the mass ratio of the silica-loaded silicon nitride microspheres to the aluminum alloy is 4.5-5.2:100.
[0012] Furthermore, the preparation method of the silicon dioxide-loaded silicon nitride microspheres is:
[0013] A. Adding initiator, silica sol and crosslinking agent solution to acrylamide monomer solution to obtain polyacrylamide composite silica;
[0014] B. Immersing the polyacrylamide composite silicon dioxide in silicon nitride sol, and then calcining to remove the polyacrylamide template to obtain the silicon dioxide-loaded silicon nitride microspheres.
[0015] Furthermore, the concentration of the monomer polyacrylamide in the prepolymerization solution is 3 mg / mL to 10 mg / mL.
[0016] Preferably, the concentration of the initiator in the prepolymerization solution is 0.2 mg / mL to 5 mg / mL.
[0017] Preferably, the concentration of the cross-linking agent in the prepolymerization solution is 0.01 mg / mL to 0.5 mg / mL.
[0018] Furthermore, in step A, the volume ratio of the silica sol to the prepolymer solution is 3-4:1-2.
[0019] Furthermore, the initiator includes potassium persulfate.
[0020] Preferably, the cross-linking agent comprises N,N-methylenebisacryloyl.
[0021] Preferably, the reaction time is 40°C to 50°C and the reaction time is 10h to 15h.
[0022] Preferably, the immersion temperature is 10°C to 60°C, and the immersion time is 8h to 16h.
[0023] Preferably, the mass percentage concentration of the silica sol is 10% to 40%.
[0024] Preferably, the mass percentage concentration of the silicon nitride sol is 10% to 50%.
[0025] The second aspect of the present invention provides a method for preparing the corrosion-resistant high-strength aluminum alloy, which comprises ball-milling all raw materials of the aluminum alloy, then adding silicon dioxide-loaded silicon nitride microspheres, mixing evenly, performing vacuum hot pressing sintering, and finally performing solid solution treatment to obtain the corrosion-resistant high-strength aluminum alloy.
[0026] Furthermore, the vacuum hot pressing sintering pressure is 500MPa to 600MPa.
[0027] Preferably, the vacuum hot pressing sintering temperature is 450°C to 500°C.
[0028] Preferably, the temperature of the solution treatment is 410° C. to 470° C., and the time is 1 h to 3 h.
[0029] Furthermore, a planetary ball mill is used to perform the ball milling mixing.
[0030] Preferably, the ball milling mixing is performed under argon protection.
[0031] Furthermore, the rotation speed of the ball milling mixing is 420rpm to 490rpm.
[0032] Preferably, the ball-to-material ratio of the ball milling mixture is 20-26:1-5.
[0033] Preferably, the ball milling mixing time is 25 min to 35 min.
[0034] Compared with the prior art, the present invention has at least the following beneficial effects:
[0035] The corrosion-resistant high-strength aluminum alloy provided by the present invention significantly improves the strength and hardness of the aluminum alloy by adding silicon dioxide-loaded silicon nitride microspheres to the aluminum alloy, and has little effect on the plasticity and toughness of the aluminum alloy. The corrosion-resistant high-strength aluminum alloy has a tensile strength of up to 445MPa, a yield strength of up to 396MPa, an elongation of up to 7.52%, and excellent salt spray and alkali resistance, which greatly expands the use scenarios of the aluminum alloy and is suitable for large-scale promotion and use.
[0036] The preparation method provided by the invention has simple process, high mechanization degree, large batch processing volume and is suitable for large-scale industrial production. DETAILED DESCRIPTION
[0037] To make the purpose, technical solution and advantages of the present invention clearer, the technical solution in the embodiment of the present invention will be clearly and completely described below in combination with the embodiment of the present invention. Obviously, the described embodiment is a part of the embodiment of the present invention, but not all of the embodiments. The components of the embodiment of the present invention can be arranged and designed in various different configurations.
[0038] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0039] A first aspect of the present invention provides a corrosion-resistant high-strength aluminum alloy comprising silicon dioxide-loaded silicon nitride microspheres and an aluminum alloy.
[0040] The corrosion-resistant high-strength aluminum alloy provided by the present invention significantly improves the strength and hardness of the aluminum alloy by adding silicon dioxide-loaded silicon nitride microspheres to the aluminum alloy, and has little effect on the plasticity and toughness of the aluminum alloy. The corrosion-resistant high-strength aluminum alloy has a tensile strength of up to 445MPa, a yield strength of up to 396MPa, an elongation of up to 7.52%, and excellent salt spray and alkali resistance, which greatly expands the use scenarios of the aluminum alloy and is suitable for large-scale promotion and use.
[0041] Furthermore, the aluminum alloy includes the following elements in percentage by mass: Zr 0.01% to 0.6%, Er 0.03-0.2%, Mg 0.1-2%, Ti 0.1-3%, and the balance is Al.
[0042] When aluminum alloy is melted and cast, a large amount of gas and oxidized inclusions (mainly hydrogen, oxygen and nitrogen) will be introduced, causing defects such as pinholes, cracks and inclusions in the casting, reducing the strength of the aluminum alloy. The present invention adds zirconium, erbium, magnesium and titanium to the aluminum matrix. During vacuum hot pressing and sintering, these elements can form compounds with low density and high melting point with harmful impurities. The compounds float up and can be removed, thereby purifying the aluminum liquid and playing a role in modifying and refining the aluminum alloy structure; at the same time, magnesium and titanium will undergo oxidation reactions to form a dense passivation film on the material surface, thereby improving the corrosion resistance of the material.
[0043] The corrosion-resistant high-strength aluminum alloy provided by the present invention can be applied to more scenarios after being matched with a hydrophobic coating, replacing stainless steel and reducing the cost of material use.
[0044] Typically, but not limiting, in the aluminum alloy, the mass percentage of Zr is 0.01%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5% or 0.6%, or any value in the range of 0.01% to 0.6%; the mass percentage of Er is 0.03%, 0.05%, 0.08%, 0.1% or 0.2%, or any value in the range of 0.03-0.2%. The mass percentage of Mg is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 1%, 1.5% or 2%, and can also be any value in the range of 0.1-2%; the mass percentage of Ti is 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 1%, 1.5%, 2%, 2.5% or 3%, and can also be any value in the range of 0.1-3%.
[0045] Preferably, the particle size of the silicon dioxide-loaded silicon nitride microspheres is 0.2 μm to 0.9 μm.
[0046] Typically but not limiting, the particle size of the silica-supported silicon nitride microspheres may be, for example, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm or 0.9 μm, or any value within the range of 0.2 μm to 0.9 μm.
[0047] Preferably, the mass ratio of the silica-loaded silicon nitride microspheres to the aluminum alloy is 4.5-5.2:100.
[0048] When the mass ratio of silica-loaded silicon nitride microspheres to aluminum alloy is lower than 4.5:100, the amount of silica-loaded silicon nitride microspheres is relatively small, and when subjected to external force, dislocation movement causes material deformation; when the mass ratio of silica-loaded silicon nitride microspheres to aluminum alloy is higher than 5.2:100, the amount of silica-loaded silicon nitride microspheres is too much, and the material is prone to breakage.
[0049] Typically but not limiting, the mass ratio of silica-loaded silicon nitride microspheres to aluminum alloy can be, for example, 4.5:100, 4.6:100, 4.7:100, 4.8:100, 4.9:100, 5.0:100, 5.1:100 or 5.2:100, or any value within the range of 4.5 to 5.2:100.
[0050] Furthermore, the preparation method of the silicon dioxide-loaded silicon nitride microspheres is:
[0051] A. Adding initiator, silica sol and crosslinking agent solution to acrylamide monomer solution to obtain polyacrylamide composite silica;
[0052] B. Immersing the polyacrylamide composite silicon dioxide in silicon nitride sol, and then calcining to remove the polyacrylamide template to obtain the silicon dioxide-loaded silicon nitride microspheres.
[0053] In the above preparation method, polyacrylamide plays a good structural guiding role, and the obtained polyacrylamide composite silica has a high specific surface area and a uniform pore size distribution, which is conducive to loading silicon nitride microspheres.
[0054] Furthermore, the concentration of the monomer polyacrylamide in the prepolymerization solution is 3 mg / mL to 10 mg / mL.
[0055] Typically but not limiting, the concentration of monomeric polyacrylamide can be, for example, 3 mg / mL, 4 mg / mL, 5 mg / mL, 6 mg / mL, 7 mg / mL, 8 mg / mL, 9 mg / mL or 10 mg / mL, or any value within the range of 3 mg / mL to 10 mg / mL.
[0056] Preferably, the concentration of the initiator in the prepolymerization solution is 0.2 mg / mL to 5 mg / mL.
[0057] Typically, but not limiting, the concentration of the initiator can be, for example, 0.2 mg / mL, 0.5 mg / mL, 1 mg / mL, 2 mg / mL, 3 mg / mL, 4 mg / mL or 5 mg / mL, or
[0058] Any value within the range of 0.2 mg / mL to 5 mg / mL.
[0059] Preferably, the concentration of the cross-linking agent in the prepolymerization solution is 0.01 mg / mL to 0.5 mg / mL.
[0060] Typically but not limiting, the concentration of the cross-linking agent can be, for example, 0.01 mg / mL, 0.05 mg / mL, 0.1 mg / mL, 0.2 mg / mL, 0.3 mg / mL, 0.4 mg / mL or 0.5 mg / mL, or any value within the range of 0.01 mg / mL to 0.5 mg / mL.
[0061] Furthermore, in step A, the volume ratio of the silica sol to the prepolymer solution is 3-4:1-2.
[0062] If the volume ratio of silica sol to prepolymer solution is smaller than the above range, that is, the amount of silica sol used is small, the amount of carrier silica generated will be small, affecting the reinforcement effect; if the volume ratio of silica sol to prepolymer solution is larger than the above range, that is, the amount of silica sol used is large, the reinforcement phase structure will change and the structural functionality of the material will be greatly reduced.
[0063] Typically but not limiting, the volume ratio of silica sol to prepolymer solution may be, for example, 3:1, 3:2, 4:1, or 4:2, or any value within the range of 3-4:1-2.
[0064] Furthermore, the initiator includes potassium persulfate.
[0065] Preferably, the cross-linking agent comprises N,N-methylenebisacryloyl.
[0066] Preferably, the reaction time is 40°C to 50°C and the reaction time is 10h to 15h.
[0067] Preferably, the immersion temperature is 10°C to 60°C, and the immersion time is 8h to 16h.
[0068] Preferably, the mass percentage concentration of the silica sol is 10% to 40%.
[0069] When the mass percentage concentration of silica sol is lower than 10%, the proportion of silicon dioxide is too small, which is not conducive to the uniform shape and size of silica microspheres; when the mass percentage concentration of silica sol is higher than 40%, the proportion of silicon dioxide is too high, which will make the size of some silica microspheres too large.
[0070] Typically but not limiting, the mass percentage concentration of silica sol can be, for example, 10%, 20%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39% or 40%, or any value within the range of 10% to 40%.
[0071] Preferably, the mass percentage concentration of the silicon nitride sol is 10% to 50%.
[0072] When the mass percentage concentration of silicon nitride sol is lower than 10%, the content of silicon nitride loaded in the support will be low, which will affect the hydrophobic properties of the final material; when the mass percentage concentration of silicon nitride sol is higher than 50%, part of the oxygen element will be replaced by nitrogen, and the structure and properties of the substance will change.
[0073] Typically but not limiting, the mass percentage concentration of the silicon nitride sol may be, for example, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%, or any value within the range of 10% to 50%.
[0074] The second aspect of the present invention provides a method for preparing the corrosion-resistant high-strength aluminum alloy, which comprises ball-milling all raw materials of the aluminum alloy, then adding silicon dioxide-loaded silicon nitride microspheres, mixing evenly, performing vacuum hot pressing sintering, and finally performing solid solution treatment to obtain the corrosion-resistant high-strength aluminum alloy.
[0075] The preparation method provided by the invention has simple process, high mechanization degree, large batch processing volume and is suitable for large-scale industrial production.
[0076] Furthermore, the vacuum hot pressing sintering pressure is 500MPa to 600MPa.
[0077] Typically but not limitatively, the pressure of vacuum hot pressing sintering can be, for example, 500 MPa, 510 MPa, 520 MPa, 530 MPa, 540 MPa, 550 MPa, 560 MPa, 570 MPa, 580 MPa, 590 MPa or 600 MPa, or any value within the range of 500 MPa to 600 MPa.
[0078] Preferably, the vacuum hot pressing sintering temperature is 450°C to 500°C.
[0079] Typically but not limiting, the temperature of vacuum hot pressing sintering may be, for example, 450°C, 460°C, 470°C, 480°C, 490°C or 500°C, or any value within the range of 450°C to 500°C.
[0080] Preferably, the temperature of the solution treatment is 410° C. to 470° C., and the time is 1 h to 3 h.
[0081] Typically but not limiting, the temperature of the solution treatment can be, for example, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C or 470°C, or any value within the range of 410°C to 470°C; the time can be, for example, 1h, 2h or 3h, or any value within the range of 1h to 3h.
[0082] Furthermore, a planetary ball mill is used to perform the ball milling mixing.
[0083] Preferably, the ball milling mixing is performed under argon protection.
[0084] Furthermore, the rotation speed of the ball milling mixing is 420rpm to 490rpm.
[0085] Preferably, the ball-to-material ratio of the ball milling mixture is 20-26:1-5.
[0086] Preferably, the ball milling mixing time is 25 min to 35 min.
[0087] In the following, some embodiments of the present invention are described in detail in conjunction with the embodiments. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.
[0088] The silicon dioxide-loaded silicon nitride microspheres used in the following examples and comparative examples were prepared by the following method:
[0089] 1. Take 10 g of acrylamide and 5 g of N,N-methylenebisacrylamide monomers respectively, dissolve them in 1425 g of deionized water and stir evenly to obtain solution A.
[0090] 2. Add 3 mg of potassium persulfate to 10 g of deionized water to prepare an aqueous solution to obtain solution B.
[0091] 3. Add solution B and silica sol (mass percentage concentration is 35%) to solution A, the volume ratio of solution A and solution B to silica sol is 1:3, stir evenly, react at 40°C for 12h to obtain polyacrylamide composite silica.
[0092] 4. Place the polyacrylamide composite silica powder in silicon nitride sol (mass percentage concentration is 20%), immerse at room temperature for 10 hours, and then filter and dry to obtain silica-loaded silicon nitride microspheres.
[0093] The product formulations of the embodiments of the present invention and the comparative examples are shown in Table 1 below.
[0094] Table 1
[0095]
[0096] Note: “ / ” means that the substance is not added.
[0097] It should be noted that the sum of the mass proportions of the metal elements in the above aluminum alloy is 100%, and the amount of silicon dioxide-loaded silicon nitride microspheres added is the mass ratio of the mass of the silicon dioxide-loaded silicon nitride microspheres to the aluminum alloy. For example, 4.8% means that the mass ratio of silicon dioxide-loaded silicon nitride microspheres to the aluminum alloy is 4.8:100.
[0098] The specific preparation methods of the embodiments and comparative examples are as follows:
[0099] According to the formula in Table 1, aluminum, zirconium, erbium, magnesium and titanium are added to the planetary ball mill, and 25 times the mass of zirconium oxide beads are added as grinding balls. Argon is introduced as a protective atmosphere, and the ball mill speed is controlled at 450rpm. The ball mill is milled for half an hour. Then silicon dioxide-loaded silicon nitride microspheres are added and mixed evenly. Finally, vacuum hot pressing sintering is performed at a pressure of 500MPa and a temperature of 480℃. After sintering, the corrosion-resistant high-strength aluminum alloy is obtained by solid solution treatment at 430℃ for 2h.
[0100] Test Example 1
[0101] The mechanical properties of the corrosion-resistant high-strength aluminum alloys obtained in the examples and comparative examples were tested in accordance with the provisions of GB / T13239-2006 “Low-temperature tensile test methods for metallic materials”. The obtained data are shown in Table 2 below.
[0102] Table 2
[0103] Tensile strength / MPa Yield strength / MPa Elongation / % Example 1 437.9 390.5 7.52 Example 2 422.8 383.6 7.23 Example 3 445.1 396.4 6.98 Example 4 440.7 375.6 7.12 Example 5 370.4 336.4 6.90 Example 6 380.3 350.6 6.10 Example 7 365.9 349.5 6.55 Example 8 386.2 360.7 6.25 Example 9 389.5 368.1 6.34 Example 10 369.4 343.2 6.56 Embodiment 11 376.9 351.4 6.77 Example 12 382.1 369.5 6.48 Comparative Example 1 300.6 275.3 8.63
[0104] As can be seen from Table 2, Examples 1 to 4 show that the content of each component is within the scope of the claims, and the performance thereof is not much different; Examples 5 to 12 show that when the content of each component exceeds the range or even the component is missing, the mechanical properties of the material decrease; in Comparative Example 1, the reinforcing phase is missing, and the strength of the material decreases significantly, but because the material becomes soft, its elongation after fracture increases.
[0105] Test Example 2
[0106] The corrosion-resistant and high-strength aluminum alloys obtained in the embodiments and comparative examples were tested for acid and alkali resistance, and the acid resistance was tested according to the NSS test method of GB / T 10125-2021 "Artificial atmosphere corrosion test salt spray test". The test lasted 48 hours, and the surface changes of the material were observed.
[0107] Alkali resistance is in accordance with GB / T 32095.3-2015 "Performance and test specifications for non-stick surfaces of metal cooking utensils for household food Part 3: Corrosion resistance test specifications", and the data obtained are shown in Table 3 below.
[0108] Table 3
[0109]
[0110] As can be seen from Table 3, Examples 1 to 4 show that the content of each component is within the scope of the claims, and the acid and alkali resistance is the best; Examples 5 to 12 show that when the content of each component exceeds the range or even the component is missing, the acid and alkali resistance of the material decreases, and corrosion areas of varying degrees begin to appear; in Comparative Example 1, the reinforcing phase is missing, the density of the material decreases, the acid and alkali liquids are easily penetrated, and large-scale corrosion occurs.
[0111] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A corrosion-resistant high-strength aluminum alloy, It is characterized in that The invention comprises silicon dioxide-loaded silicon nitride microspheres and aluminum alloy.
2. The corrosion-resistant high-strength aluminum alloy according to claim 1, It is characterized in that The aluminum alloy includes the following elements in percentage by mass: Zr 0.01% to 0.6%, Er 0.03-0.2%, Mg 0.1-2%, Ti 0.1-3%, and the balance is Al; Preferably, the particle size of the silicon dioxide-loaded silicon nitride microspheres is 0.2 μm to 0.9 μm; Preferably, the mass ratio of the silica-loaded silicon nitride microspheres to the aluminum alloy is 4.5-5.2:
100.
3. The corrosion-resistant high-strength aluminum alloy according to claim 1, It is characterized in that The preparation method of the silicon dioxide-loaded silicon nitride microspheres is as follows: A. Adding initiator, silica sol and crosslinking agent solution to acrylamide monomer solution to react to obtain polyacrylamide composite silica; B. Immersing the polyacrylamide composite silicon dioxide in silicon nitride sol, and then calcining to remove the polyacrylamide template to obtain the silicon dioxide-loaded silicon nitride microspheres.
4. The corrosion-resistant high-strength aluminum alloy according to claim 3, It is characterized in that The concentration of the monomer polyacrylamide in the prepolymerization solution is 3 mg / mL to 10 mg / mL; Preferably, the concentration of the initiator in the prepolymerization solution is 0.2 mg / mL to 5 mg / mL; Preferably, the concentration of the cross-linking agent in the prepolymerization solution is 0.01 mg / mL to 0.5 mg / mL.
5. The corrosion-resistant high-strength aluminum alloy according to claim 3, It is characterized in that In step A, the volume ratio of the silica sol to the prepolymer solution is 3-4:1-2.
6. The corrosion-resistant high-strength aluminum alloy according to any one of claims 3 to 5, It is characterized in that The initiator includes potassium persulfate; Preferably, the cross-linking agent comprises N,N-methylenebisacryloyl; Preferably, the reaction time is 40°C to 50°C, and the time is 10h to 15h; Preferably, the immersion temperature is 10°C to 60°C, and the time is 8h to 16h; Preferably, the mass percentage concentration of the silica sol is 10% to 40%; Preferably, the mass percentage concentration of the silicon nitride sol is 10% to 50%.
7. A method for preparing the corrosion-resistant high-strength aluminum alloy according to any one of claims 1 to 6, It is characterized in that All raw materials of the aluminum alloy are ball-milled and mixed, and then silicon dioxide-loaded silicon nitride microspheres are added and mixed evenly, and vacuum hot-pressed and sintered, and finally solution treated to obtain the corrosion-resistant high-strength aluminum alloy.
8. The preparation method according to claim 7, It is characterized in that The vacuum hot pressing sintering pressure is 500MPa to 600MPa; Preferably, the vacuum hot pressing sintering temperature is 450°C to 500°C; Preferably, the solution treatment is carried out at a temperature of 410° C. to 470° C. and for a time of 1 h to 3 h.
9. The preparation method according to claim 7, It is characterized in that Using a planetary ball mill to perform the ball milling mixing; Preferably, the ball milling mixing is performed under argon protection.
10. The preparation method according to claim 7, It is characterized in that The rotation speed of the ball milling mixing is 420rpm~490rpm; Preferably, the ball-to-material ratio of the ball milling mixture is 20-26:1-5; Preferably, the ball milling mixing time is 25 min to 35 min.
Citation Information
Cited By
High-strength corrosion-resistant aluminum alloy strip and preparation method thereof
CN121737605A