Method for directly growing ZnO porous film by introducing air

The method of directly growing a ZnO porous film through air ventilation, and using the electrochemical deposition method to prepare a ZnO porous film in a three-electrode system, solves the problems of expensive equipment and complex operation in the existing technology, achieves rapid growth and high sensitivity, and is suitable for Biosensing and gas sensing fields.

CN118835291APending Publication Date: 2024-10-25WUYI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410836347.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

When preparing metal oxide porous films using existing technology, the equipment is expensive or the operation is complicated, making it difficult to achieve large-scale production and rapid growth, and the gas-sensitive properties of the materials need to be improved.

Method used

The method of directly growing ZnO porous films through air ventilation is used to prepare a growth solution containing ZnCl2 and KCl, adjust the pH value to 2.0-3.0, and use electrochemical deposition method to use FTO conductive glass as the working electrode in a three-electrode system, saturated calomel The electrode was used as the reference electrode, and the platinum electrode was used as the auxiliary electrode. Electrochemical deposition was performed by the potential step method to prepare a ZnO porous film.

Benefits of technology

It achieves rapid growth and good uniformity of ZnO porous films, improves the sensitivity and gas-sensing performance of the material, simplifies the preparation process, reduces costs, and has good biosensing and gas-sensing application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118835291A_ABST
    Figure CN118835291A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of gas-sensitive materials, and particularly discloses a method for directly growing a ZnO porous film by introducing air. The method for directly growing the ZnO porous film by introducing air comprises the following steps: S1) cleaning and pretreating FTO (Fluorine-doped Tin Oxide); s2) preparing a growth solution; s3), assembling the electrodes; s4) setting reaction parameters; the preparation process is simple, the preparation cost is low, and the prepared ZnO porous film is stable in performance and has good gas-sensitive performance; the porous structure of the ZnO porous film prepared by the method is relatively uniform in distribution, so that the specific surface area of a film material can be increased; the ZnO porous film prepared by the method has a good application prospect in the fields of biosensing, gas-sensitive sensing, photoelectric conversion and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of gas-sensitive material preparation, and in particular to a method for directly growing a ZnO porous film through air. Background Art

[0002] With the rapid development of gas sensors, gas-sensitive materials have also developed rapidly. At present, gas sensors are mainly based on semiconductor metal oxides such as ZnO, SnO2, and WO3. These metal oxides are widely studied gas-sensitive materials due to their excellent performance, environmental friendliness, abundant resources, and low prices. The gas-sensitive properties of materials can be improved through processes such as metal oxide surface modification and metal / precious metal doping, which have very wide applications in the field of gas sensors.

[0003] At present, the methods for preparing porous metal oxide films are mainly hydrothermal method, magnetron sputtering method, chemical deposition method and atomic deposition method. Among them, the instruments and equipment used in magnetron sputtering, chemical deposition and atomic deposition are expensive and not conducive to large-scale production, while the hydrothermal method requires the preparation of specific solutions and temperature control, and the operation is more complicated and the preparation time is long. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention proposes a method for directly growing a ZnO porous film by air, which can prepare a ZnO porous film and has the advantages of fast growth speed and good uniformity.

[0005] A first aspect of the present invention provides a method for directly growing a ZnO porous thin film by air ventilation.

[0006] Specifically, the method for directly growing a ZnO porous film by air flow comprises the following steps:

[0007] Prepare a growth solution containing ZnCl2 and KCl, and adjust the pH value of the growth solution to 2.0-3.0;

[0008] Passing air into the growth solution having a pH value of 2.0-3.0 to obtain an oxygen-saturated growth solution;

[0009] In an electrochemical workstation of a three-electrode system, FTO conductive glass is used as a working electrode, a saturated calomel electrode is used as a reference electrode, a platinum sheet electrode is used as an auxiliary electrode, and the oxygen-saturated growth solution is used as an electrolyte. Electrochemical deposition is performed at 80-100° C. by a potential step method to prepare a ZnO porous film.

[0010] The electrochemical deposition process includes: depositing at a potential value of -1.3V for 5-20s to form ZnO seed crystals on at least a portion of the surface of the FTO conductive glass, and then depositing at a potential value of -1.0V for 1500-2000s.

[0011] It can be understood that the deposition time using a potential value of -1.3V can be, for example, any point value among 5s, 8s, 11s, 14s, 17s, 20s, or a range value between two arbitrary point values; the deposition time using a potential value of -1.0V can be, for example, any point value among 1500s, 1600s, 1700s, 1800s, 1900s, 2000s, or a range value between two arbitrary point values.

[0012] Specifically, the reaction equation involved in the electrochemical deposition process is as follows:

[0013] O2+H2O+4e - =4OH - ;

[0014] Zn 2+ +OH - =Zn(OH)2;

[0015] Zn(OH)2=ZnO+H2O.

[0016] It should be noted that the present invention uses a saturated calomel electrode as a reference electrode because the electrode potential of the saturated calomel electrode is about 0.2412V or 0.2415V at 25°C, while the standard electrode potential of the silver chloride reference electrode is +0.2224V (at 25°C). Their constant potentials are different, and a small potential gap may also bring different results in electrochemical deposition. In addition, the voltage and time of the potential step method have strict requirements. For example, if there is no pre-deposition in the first step of the present invention (using a potential value of -1.3V to deposit for 5-20s), dense ZnO seed crystals will not be formed, and the material grown will inevitably be different from the ZnO porous film formed by the method of the present invention.

[0017] In some embodiments of the present invention, in the growth solution, the concentration of ZnCl2 is 0.001-0.01 mol / L, for example, it can be any point value among 0.001 mol / L, 0.002 mol / L, 0.003 mol / L, 0.004 mol / L, 0.005 mol / L, 0.006 mol / L, 0.007 mol / L, 0.008 mol / L, 0.009 mol / L, and 0.01 mol / L, or a range value between two arbitrary point values.

[0018] In some embodiments of the present invention, in the growth solution, the concentration of KCl is 0.05-0.15 mol / L, for example, it can be any point value among 0.05 mol / L, 0.06 mol / L, 0.07 mol / L, 0.08 mol / L, 0.09 mol / L, 0.1 mol / L, 0.11 mol / L, 0.12 mol / L, 0.13 mol / L, 0.14 mol / L, and 0.15 mol / L, or a range value between two arbitrary point values.

[0019] In some embodiments of the present invention, the pH value of the growth liquid is adjusted to 2.0-3.0 using a hydrochloric acid solution. The pH value may be, for example, any value among 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, or a range between two arbitrary values.

[0020] In some embodiments of the present invention, the hydrochloric acid solution is a solution of concentrated hydrochloric acid and water mixed in a volume ratio of 1:9.

[0021] In some embodiments of the present invention, the step of pretreating the FTO conductive glass is further included. The pretreatment process includes: ultrasonically cleaning the FTO conductive glass with a solvent, then immersing the FTO conductive glass in an acidic solution, and then taking it out and drying it.

[0022] In some embodiments of the present invention, the solvent comprises at least one of acetone, ethanol and water.

[0023] In some embodiments of the present invention, the acidic solution is a solution of concentrated hydrochloric acid and water mixed in a volume ratio of 1:9.

[0024] In some embodiments of the present invention, the ultrasonic cleaning time is 10-30 minutes.

[0025] In some embodiments of the present invention, the soaking time is 1-10 min.

[0026] In some embodiments of the present invention, the flow rate of the air introduction is 1-2 L / min; and / or the time of the air introduction is 5-20 min.

[0027] A second aspect of the present invention provides a ZnO porous film.

[0028] Specifically, the ZnO porous film is prepared by the method described in the first aspect of the present invention.

[0029] In some embodiments of the present invention, the specific surface area of ​​the ZnO porous film is 0.01-0.1 m 2 / g; and / or, the pore size of the ZnO porous film is 1200-1500nm; and / or, the thickness of the ZnO porous film is 100-200nm.

[0030] A third aspect of the present invention provides a device.

[0031] Specifically, the device includes the ZnO porous film described in the second aspect of the present invention.

[0032] In some embodiments of the present invention, the device includes any one of a solar cell, a biosensor, and a gas detector.

[0033] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0034] 1. The method of directly growing a ZnO porous film by passing air in the present invention has a short growth cycle, and the pores of the prepared ZnO porous film have good uniformity, which can improve the sensitivity of the ZnO porous film.

[0035] 2. The method of directly growing a ZnO porous film by passing air in the present invention is simple and easy to operate, has a low preparation cost, and the performance of the prepared ZnO porous film is stable and has good biosensing function.

[0036] 3. The pore structure distribution of the ZnO porous film prepared by the present invention is relatively regular, which is beneficial to increase the specific surface area of ​​the porous film material.

[0037] 4. The ZnO porous film prepared by the present invention has good application prospects in the fields of biosensing, gas sensing, photoelectric conversion, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 This is a low-magnification scanning electron microscope (SEM) image of the ZnO porous film prepared in Example 1 of the present invention;

[0039] Figure 2 This is a high-magnification scanning electron microscope (SEM) image of the ZnO porous film prepared in Example 1 of the present invention;

[0040] Figure 3 This is a low-magnification scanning electron microscope (SEM) image of the ZnO porous film prepared in Example 2 of the present invention;

[0041] Figure 4 A high-power scanning electron microscope (SEM) image of the ZnO porous film prepared in Example 2 of the present invention;

[0042] Figure 5 This is a low-magnification scanning electron microscope (SEM) image of the ZnO porous film prepared in Example 3 of the present invention;

[0043] Figure 6 This is a high-magnification scanning electron microscope (SEM) image of the ZnO porous film prepared in Example 3 of the present invention;

[0044] Figure 7 This is a low-magnification scanning electron microscope (SEM) image of the ZnO porous film prepared in Comparative Example 1 of the present invention;

[0045] Figure 8 This is a high-magnification scanning electron microscope (SEM) image of the ZnO porous film prepared in Comparative Example 1 of the present invention;

[0046] Fig. 9 This is a low-magnification scanning electron microscope (SEM) image of the ZnO porous film prepared in Comparative Example 2 of the present invention;

[0047] Fig.10 This is a high-magnification scanning electron microscope (SEM) image of the ZnO porous film prepared in Comparative Example 2 of the present invention;

[0048] Fig.11 This is a gas-sensitive response diagram of the ZnO porous film prepared in Example 1 of the present invention to 50 ppm NO;

[0049] Fig.12 This is a gas-sensitive response diagram of the ZnO porous film prepared in Example 2 of the present invention to 1000 ppm ammonia;

[0050] Fig.13 This is a gas-sensitive response diagram of the ZnO porous film prepared in Comparative Example 1 of the present invention to 1000 ppm ethanol;

[0051] Fig.14 This is the gas-sensitive response diagram of the ZnO porous film prepared in Example 1 of the present invention to 1000 ppm ethanol. DETAILED DESCRIPTION

[0052] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0053] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0054] The instrument and electrode information used in the present invention are shown in Table 1.

[0055] Table 1

[0056] Device Name model Manufacturer Electrochemical workstation CHI760E Shanghai Chenhua Co., Ltd. Platinum electrode clip LG13-401-1 Lithium Technology Co., Ltd. Platinum electrode 5*5*0.2mm LG13-201-5 Lithium Technology Co., Ltd. Saturated calomel electrode (SCE) LG13-302-1 Lithium Technology Co., Ltd.

[0057] Example 1

[0058] A method for directly growing a ZnO porous film by ventilation, comprising the following steps:

[0059] S1) Cleaning and pretreatment of FTO conductive glass

[0060] S101), first, clean the FTO conductive glass with acetone, ethanol and deionized water for 10 minutes respectively, then prepare a hydrochloric acid solution (the volume ratio of concentrated hydrochloric acid to deionized water is 1:9), and immerse the FTO conductive glass in the hydrochloric acid solution for 3 minutes, and then put it in a blast drying oven for drying;

[0061] S2) Preparation of growth solution

[0062] S201), 0.0685g ZnCl2, 0.7455g KCl and 100mL deionized water are mixed to obtain a growth solution, and the pH value of the growth solution is adjusted to 2.5±0.1 by dripping the hydrochloric acid solution prepared in step S101);

[0063] S3) Assembly of electrodes

[0064] S301), combine the sheet electrode clip, the platinum electrode and the SCE electrode on the electrolytic cell cover, use a multimeter to measure the conductive surface of the FTO conductive glass, and connect the FTO conductive glass and the sheet electrode clip group together; note that the conductive surface of the FTO conductive glass is in a parallel and opposite position to the platinum electrode; pour the growth solution with a pH value of 2.5±0.1 prepared in step S201) into the electrolytic cell as an electrolyte, tighten the electrolytic cell cover and the electrolytic cell to seal it; put the sealed electrolytic cell into a heat-collecting magnetic stirrer, and connect it to the three-electrode system electrode clip of the electrochemical workstation; wherein the FTO conductive glass is used as the working electrode, the saturated calomel electrode is used as the reference electrode, and the platinum electrode is used as the auxiliary electrode;

[0065] S4) Setting of reaction parameters

[0066] S401), before the reaction, first install a stop valve on the oxygen pump, and adjust the flow rate to 1L / min, and pass air into the electrolyte for 10 minutes to saturate the electrolyte with oxygen, turn on the heat-collecting magnetic stirrer, set the reaction temperature to 80°C, and carry out electrochemical deposition reaction. The deposition process uses a potential step method, and a potential value of -1.3V is used for deposition for 10s to form more ZnO seeds on the surface of the FTO conductive glass substrate, and then a potential value of -1.0V is used for deposition for 1800s. After the deposition is completed, the FTO is taken out, the residual chloride salt on the surface is rinsed with deionized water, and the film is blown dry. The film is removed to obtain the ZnO porous film.

[0067] The specific surface area of ​​the ZnO porous film prepared in this example is 0.0110 m 2 / g, the average pore diameter is 1294.5765nm, and the thickness is 153nm.

[0068] Example 2

[0069] A method for directly growing a ZnO porous film by ventilation, comprising the following steps:

[0070] S1) Cleaning and pretreatment of FTO conductive glass

[0071] S101), first, clean the FTO conductive glass with acetone, ethanol and deionized water for 10 minutes respectively, then prepare a hydrochloric acid solution (the volume ratio of concentrated hydrochloric acid to deionized water is 1:9), and immerse the FTO conductive glass in the hydrochloric acid solution for 3 minutes, and then put it in a blast drying oven for drying;

[0072] S2) Preparation of growth solution

[0073] S201), 0.0685g ZnCl2, 0.7455g KCl and 100mL deionized water are mixed to obtain a growth solution, and the pH value of the growth solution is adjusted to 2.2±0.1 by dripping the hydrochloric acid solution prepared in step S101);

[0074] S3) Assembly of electrodes

[0075] S301), combine the sheet electrode clip, the platinum electrode and the SCE electrode on the electrolytic cell cover, use a multimeter to measure the conductive surface of the FTO conductive glass, and connect the FTO conductive glass and the sheet electrode clip group together; note that the conductive surface of the FTO conductive glass is in a parallel and opposite position to the platinum electrode; pour the growth solution with a pH value of 2.2±0.1 prepared in step S201) into the electrolytic cell as an electrolyte, tighten the electrolytic cell cover and the electrolytic cell to seal it; put the sealed electrolytic cell into a heat-collecting magnetic stirrer, and connect it to the three-electrode system electrode clip of the electrochemical workstation; wherein the FTO conductive glass is used as the working electrode, the saturated calomel electrode is used as the reference electrode, and the platinum electrode is used as the auxiliary electrode;

[0076] S4) Setting of reaction parameters

[0077] S401), before the reaction, first install a stop valve on the oxygen pump, and adjust the flow rate to 1L / min, and pass air into the electrolyte for 10 minutes to saturate the electrolyte with oxygen, turn on the heat-collecting magnetic stirrer, set the reaction temperature to 80°C, and carry out electrochemical deposition reaction. The deposition process uses a potential step method, and a potential value of -1.3V is used for deposition for 10s to form more ZnO seeds on the surface of the FTO conductive glass substrate, and then a potential value of -1.0V is used for deposition for 1800s. After the deposition is completed, the FTO is taken out, the residual chloride salt on the surface is rinsed with deionized water, and the film is blown dry. The film is removed to obtain the ZnO porous film.

[0078] Example 3

[0079] A method for directly growing a ZnO porous film by ventilation, comprising the following steps:

[0080] S1) Cleaning and pretreatment of FTO conductive glass

[0081] S101), first, clean the FTO conductive glass with acetone, ethanol and deionized water for 10 minutes respectively, then prepare a hydrochloric acid solution (the volume ratio of concentrated hydrochloric acid to deionized water is 1:9), and immerse the FTO conductive glass in the hydrochloric acid solution for 3 minutes, and then put it in a blast drying oven for drying;

[0082] S2) Preparation of growth solution

[0083] S201), 0.0685g ZnCl2, 0.7455g KCl and 100mL deionized water are mixed to obtain a growth solution, and the pH value of the growth solution is adjusted to 2.8±0.1 by dripping the hydrochloric acid solution prepared in step S101);

[0084] S3) Assembly of electrodes

[0085] S301), combine the sheet electrode clip, the platinum electrode and the SCE electrode on the electrolytic cell cover, use a multimeter to measure the conductive surface of the FTO conductive glass, and connect the FTO conductive glass and the sheet electrode clip group together; note that the conductive surface of the FTO conductive glass is in a parallel and opposite position to the platinum electrode; pour the growth solution with a pH value of 2.8±0.1 prepared in step S201) into the electrolytic cell as an electrolyte, tighten the electrolytic cell cover and the electrolytic cell to seal it; put the sealed electrolytic cell into a heat-collecting magnetic stirrer, and connect it to the three-electrode system electrode clip of the electrochemical workstation; wherein the FTO conductive glass is used as the working electrode, the saturated calomel electrode is used as the reference electrode, and the platinum electrode is used as the auxiliary electrode;

[0086] S4) Setting of reaction parameters

[0087] S401), before the reaction, first install a stop valve on the oxygen pump, and adjust the flow rate to 1L / min, and pass air into the electrolyte for 10 minutes to saturate the electrolyte with oxygen, turn on the heat-collecting magnetic stirrer, set the reaction temperature to 80°C, and carry out electrochemical deposition reaction. The deposition process uses a potential step method, and a potential value of -1.3V is used for deposition for 10s to form more ZnO seeds on the surface of the FTO conductive glass substrate, and then a potential value of -1.0V is used for deposition for 1800s. After the deposition is completed, the FTO is taken out, the residual chloride salt on the surface is rinsed with deionized water, and the film is blown dry. The film is removed to obtain the ZnO porous film.

[0088] Comparative Example 1 (the difference from Example 1 is that the pH value of the growth liquid is less than 2.0)

[0089] A method for directly growing a ZnO porous film by ventilation, comprising the following steps:

[0090] S1) Cleaning and pretreatment of FTO conductive glass

[0091] S101), first, clean the FTO conductive glass with acetone, ethanol and deionized water for 10 minutes respectively, then prepare a hydrochloric acid solution (the volume ratio of concentrated hydrochloric acid to deionized water is 1:9), and immerse the FTO conductive glass in the hydrochloric acid solution for 3 minutes, and then put it in a blast drying oven for drying;

[0092] S2) Preparation of growth solution

[0093] S201), 0.0685g ZnCl2, 0.7455g KCl and 100mL deionized water are mixed to obtain a growth solution, and the pH value of the growth solution is adjusted to 1.5±0.1 by dripping the hydrochloric acid solution prepared in step S101);

[0094] S3) Assembly of electrodes

[0095] S301), combine the sheet electrode clip, the platinum electrode and the SCE electrode on the electrolytic cell cover, use a multimeter to measure the conductive surface of the FTO conductive glass, and connect the FTO conductive glass and the sheet electrode clip group together; note that the conductive surface of the FTO conductive glass is in a parallel and opposite position to the platinum electrode; pour the growth solution with a pH value of 1.5±0.1 prepared in step S201) into the electrolytic cell as an electrolyte, tighten the electrolytic cell cover and the electrolytic cell to seal it; put the sealed electrolytic cell into a heat-collecting magnetic stirrer, and connect it to the three-electrode system electrode clip of the electrochemical workstation; wherein the FTO conductive glass is used as the working electrode, the saturated calomel electrode is used as the reference electrode, and the platinum electrode is used as the auxiliary electrode;

[0096] S4) Setting of reaction parameters

[0097] S401), before the reaction, first install a stop valve on the oxygen pump, and adjust the flow rate to 1L / min, and pass air into the electrolyte for 10 minutes to saturate the electrolyte with oxygen, turn on the heat-collecting magnetic stirrer, set the reaction temperature to 80°C, and carry out electrochemical deposition reaction. The deposition process uses a potential step method, and a potential value of -1.3V is used for deposition for 10s to form more ZnO seeds on the surface of the FTO conductive glass substrate, and then a potential value of -1.0V is used for deposition for 1800s. After the deposition is completed, the FTO is taken out, the residual chloride salt on the surface is rinsed with deionized water, and the film is blown dry. The film is removed to obtain the ZnO porous film.

[0098] Comparative Example 2 (the difference from Example 1 is that the pH value of the growth liquid is greater than 3.0)

[0099] A method for directly growing a ZnO porous film by ventilation, comprising the following steps:

[0100] S1) Cleaning and pretreatment of FTO conductive glass

[0101] S101), first, clean the FTO conductive glass with acetone, ethanol and deionized water for 10 minutes respectively, then prepare a hydrochloric acid solution (the volume ratio of concentrated hydrochloric acid to deionized water is 1:9), and immerse the FTO conductive glass in the hydrochloric acid solution for 3 minutes, and then put it in a blast drying oven for drying;

[0102] S2) Preparation of growth solution

[0103] S201), 0.0685g ZnCl2, 0.7455g KCl and 100mL deionized water are mixed to obtain a growth solution, and the pH value of the growth solution is adjusted to 3.5±0.1 by dripping the hydrochloric acid solution prepared in step S101);

[0104] S3) Assembly of electrodes

[0105] S301), combine the sheet electrode clip, the platinum electrode and the SCE electrode on the electrolytic cell cover, use a multimeter to measure the conductive surface of the FTO conductive glass, and connect the FTO conductive glass and the sheet electrode clip group together; note that the conductive surface of the FTO conductive glass is in a parallel and opposite position to the platinum electrode; pour the growth solution with a pH value of 3.5±0.1 prepared in step S201) into the electrolytic cell as an electrolyte, tighten the electrolytic cell cover and the electrolytic cell to seal it; put the sealed electrolytic cell into a heat-collecting magnetic stirrer, and connect it to the three-electrode system electrode clip of the electrochemical workstation; wherein the FTO conductive glass is used as the working electrode, the saturated calomel electrode is used as the reference electrode, and the platinum electrode is used as the auxiliary electrode;

[0106] S4) Setting of reaction parameters

[0107] S401), before the reaction, first install a stop valve on the oxygen pump, and adjust the flow rate to 1L / min, and pass air into the electrolyte for 10 minutes to saturate the electrolyte with oxygen, turn on the heat-collecting magnetic stirrer, set the reaction temperature to 80°C, and carry out electrochemical deposition reaction. The deposition process uses a potential step method, and a potential value of -1.3V is used for deposition for 10s to form more ZnO seeds on the surface of the FTO conductive glass substrate, and then a potential value of -1.0V is used for deposition for 1800s. After the deposition is completed, the FTO is taken out, the residual chloride salt on the surface is rinsed with deionized water, and the film is blown dry. The film is removed to obtain the ZnO porous film.

[0108] Shape detection:

[0109] The products obtained in Examples 1-3 and Comparative Examples 1-2 were examined by scanning electron microscopy.

[0110] Depend on Figure 1-6 It can be seen that the porous structure distribution of the ZnO porous films prepared in Examples 1-3 of the present invention is relatively regular under low-magnification and high-magnification scanning electron microscopes, which is beneficial to increasing the specific surface area of ​​the film material.

[0111] Depend on Figure 7-10 It can be seen that the overall porous morphology of the ZnO porous film prepared in Comparative Example 1-2 disappears, and is replaced by a very poor nanorod morphology. It can be seen that the pH value of the growth solution has a significant effect on the morphology.

[0112] Gas sensitive performance test:

[0113] The ZnO porous films prepared in Examples 1-2 and Comparative Example 1 were respectively electrodeposited on ITO (ZnO / ITO for short), and silver interdigital electrodes were evaporated on ZnO / ITO using a coating machine to obtain a device for testing. The device was placed on a gas-sensitive test platform, which consists of four parts: a gas source, a gas box, a data acquisition source table, and a temperature heating table. The gas source is selected by selecting the target gas to be tested, the gas box dilutes the target gas to a corresponding concentration, the data acquisition source table is responsible for collecting changes in the resistance value of the device under gas flow, and the temperature heating table is set at different temperatures to allow the device to be tested at a suitable temperature.

[0114] The test method is as follows:

[0115] First, select the target gas source, set up the program through the corresponding software, and open the source table and its software responsible for collecting data;

[0116] The program is generally set to three steps. The first step is to set the time for the device resistance value to saturate, the second step is to set the time for the device resistance value change to stabilize under the target gas, and the third step is to set the time for the device to return to the initial resistance value in the air after desorption of the target gas.

[0117] The operating temperature of the device is set to 300°C through the temperature heating stage;

[0118] Start the gas-sensitive program for testing and record the test data using the corresponding software.

[0119] Test results such as Figure 11-14 As shown; Ra in the figure is the resistance value of the device after saturation in air (generally the maximum resistance value), and Rg is the resistance value of the device after stabilization in the target gas (generally the minimum resistance value).

[0120] From the gas-sensitive response diagram, we can see the device's maximum response value, response time, and recovery time to the gas. These three parameters are important performance indicators for measuring gas-sensitive sensing. Generally speaking, the larger the maximum response value, the shorter the recovery time and response time, which means that the device has better gas-sensitive performance to the target gas.

[0121] from Figure 11-14 It can be seen that the device made of the ZnO porous film prepared according to the embodiment of the present invention has good gas sensing performance.

[0122] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution obtained by any modification, equivalent replacement, improvement, etc. made by a person skilled in the art based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art shall be within the scope of protection determined by the claims.

Claims

1. A method for directly growing a ZnO porous film by air ventilation, characterized in that: The following steps are involved: Prepare a growth solution containing ZnCl2 and KCl, and adjust the pH value of the growth solution to 2.0-3.0; Passing air into the growth solution having a pH value of 2.0-3.0 to obtain an oxygen-saturated growth solution; In an electrochemical workstation of a three-electrode system, FTO conductive glass is used as a working electrode, a saturated calomel electrode is used as a reference electrode, a platinum sheet electrode is used as an auxiliary electrode, and the oxygen-saturated growth solution is used as an electrolyte. Electrochemical deposition is performed at 80-100° C. by a potential step method to prepare a ZnO porous film. The electrochemical deposition process includes: depositing at a potential value of -1.3V for 5-20s to form ZnO seed crystals on at least a portion of the surface of the FTO conductive glass, and then depositing at a potential value of -1.0V for 1500-2000s.

2. The method according to claim 1, characterized in that In the growth solution, the concentration of ZnCl2 is 0.001-0.01 mol / L.

3. The method according to claim 1, characterized in that In the growth solution, the concentration of KCl is 0.05-0.15 mol / L.

4. The method according to claim 1, characterized in that: The pH value of the growth liquid is adjusted to 2.0-3.0 using hydrochloric acid solution.

5. The method according to claim 1, characterized in that The method also includes the step of pre-treating the FTO conductive glass. The pre-treating process includes: ultrasonically cleaning the FTO conductive glass with a solvent, then immersing the FTO conductive glass in an acidic solution, and then taking it out to dry.

6. The method according to claim 1, characterized in that The air introduction flow rate is 1-2 L / min; and / or, the air introduction time is 5-20 min.

7. A ZnO porous film, characterized in that: The ZnO porous film is prepared by the method according to any one of claims 1 to 6.

8. The ZnO porous film according to claim 7, characterized in that: The specific surface area of ​​the ZnO porous film is 0.01-0.1m 2 / g; and / or, the pore size of the ZnO porous film is 1200-1500nm; and / or, the thickness of the ZnO porous film is 100-200nm.

9. A device, characterized in that The device comprises the ZnO porous film according to claim 7 or 8.

10. The device according to claim 9, characterized in that The device includes any one of a solar cell, a biosensor, and a gas-sensitive detector.