Preparation method of high-thermal-conductivity diamond / copper composite conductive thin film material and corresponding material

By preparing an organic carrier/diamond powder mixture in copper conductive slurry and uniformly mixing bonded glass powder and copper powder, combined with vacuum leveling and sintering processes, the problem of doping diamond powder in copper conductive slurry to improve thermal conductivity is solved. Problem, a diamond/copper composite conductive film material with high thermal conductivity and low resistivity is realized, which is suitable for high-precision integrated circuits.

CN118841222AActive Publication Date: 2024-10-25HEFEI UNIV OF TECH +1
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202411026978.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-10-25
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

It is difficult with the existing technology to dope diamond powder into copper conductive slurry to improve thermal conductivity while maintaining high electrical conductivity. The electrical conductivity of diamond is extremely low, and adding it directly will reduce the electrical conductivity.

Method used

By preparing an organic carrier/diamond powder mixture, uniformly mixing bonded glass powder and copper powder to form a diamond/copper composite conductive slurry, and preparing a high thermal conductivity diamond/copper composite conductive film material through vacuum leveling, degreasing and sintering processes. Make sure the diamond powder is evenly dispersed and does not damage the conductive paths.

Benefits of technology

A diamond/copper composite conductive film material with high thermal conductivity and low resistivity has been achieved, which has strong heat dissipation and high thermal stability and is suitable for high-precision integrated circuit applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841222A_ABST
    Figure CN118841222A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of conductive films, in particular to a preparation method of a high-thermal-conductivity diamond / copper composite conductive film material and a corresponding material. Preparing an organic carrier / diamond powder mixed solution from diamond powder and the organic carrier mixed solution; the preparation method comprises the following steps: sequentially carrying out vitrification treatment and refining treatment on inorganic mixed powder obtained by mixing silicon dioxide, sodium oxide and calcium oxide to prepare bonding glass powder; preparing diamond / copper composite conductive paste from copper powder, organic carrier / diamond powder mixed liquid and adhesive glass powder; and coating the diamond / copper composite conductive slurry on the surface of a ceramic substrate, carrying out vacuum leveling treatment, placing an obtained diamond / copper composite conductive slurry coating leveling assembly in a protective atmosphere, and sequentially carrying out degreasing treatment and sintering treatment to prepare the high-thermal-conductivity diamond / copper composite conductive thin film material. The diamond / copper composite conductive film with high thermal conductivity and low resistivity can be prepared.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of conductive films, and in particular to a preparation method of a high thermal conductivity diamond / copper composite conductive film material and corresponding materials. Background Art

[0002] High-temperature printed circuit boards (PCBs) are electronic materials made by printing conductive copper paste on a ceramic substrate, followed by high-temperature degreasing and sintering. Unlike normal-temperature PCB materials, high-temperature PCB materials must withstand higher ambient temperatures during use. Therefore, in addition to having good electrical conductivity and bonding strength, they must also have higher thermal conductivity to meet stringent heat dissipation requirements. The thermal conductivity of PCB materials is mainly determined by the copper conductive paste on the surface and the substrate material. Since the thermal conductivity of copper metal paste is much higher than that of the ceramic substrate, further improving the thermal conductivity of the conductive paste plays an important role in improving the thermal conductivity of PCB materials.

[0003] At present, the method for improving copper conductive paste is mainly to add high thermal conductivity materials such as gold and graphene to conductive copper powder. The Chinese invention patent with publication number CN113481491B discloses a copper / graphene composite film material and a preparation method thereof. The copper / graphene composite film material is prepared by co-depositing metallic copper and monolayer graphene on the surface of the substrate, and a composite film material with high thermal conductivity is obtained. However, raw materials such as gold and graphene are expensive and are not conducive to large-scale application in the industrial field. In contrast, diamond powder materials that also have high thermal conductivity and low price have greater application prospects in copper conductive paste. However, the electrical conductivity of diamond is extremely low, and directly adding it to the conductive copper paste will greatly reduce the conductivity of the conductive paste.

[0004] Therefore, how to dope diamond into copper conductive paste to improve thermal conductivity while maintaining high electrical conductivity has become a technical problem that needs to be solved urgently. Summary of the invention

[0005] In view of this, in order to overcome the deficiencies of the prior art, the present invention provides a method for preparing a high thermal conductivity diamond / copper composite conductive film material and corresponding materials.

[0006] According to one aspect of the present invention, the present invention provides a method for preparing a high thermal conductivity diamond / copper composite conductive film material, the method comprising the following steps:

[0007] Step 1: Preparation of organic carrier / diamond powder mixture

[0008] A first mixed material is prepared by using terpineol, polyethylene glycol 400, ethyl cellulose and polyoxypropylene according to a ratio, and the prepared first mixed material is subjected to a first water bath stirring treatment to prepare an organic carrier mixed solution;

[0009] A second mixed material is prepared by using a mixture of diamond powder and an organic carrier according to a ratio, and the prepared second mixed material is subjected to a second water bath stirring treatment to obtain an organic carrier / diamond powder mixed solution;

[0010] Step 2: Preparation of diamond / copper composite conductive slurry

[0011] Mixing silicon dioxide, sodium oxide and calcium oxide according to a ratio to obtain an inorganic mixed powder, and sequentially performing vitrification treatment and refinement treatment on the obtained inorganic mixed powder to obtain a bonding glass powder;

[0012] A third mixed material is prepared by using copper powder, organic carrier / diamond powder mixed solution and bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment to obtain a diamond / copper composite conductive slurry;

[0013] Step 3: Preparation of high thermal conductivity diamond / copper composite conductive film material

[0014] The diamond / copper composite conductive slurry is coated on the surface of the ceramic substrate, and the ceramic substrate coated with the diamond / copper composite conductive slurry is subjected to vacuum leveling treatment to obtain a diamond / copper composite conductive slurry coated leveling component;

[0015] The diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere for degreasing treatment and sintering treatment in sequence to obtain a high thermal conductivity diamond / copper composite conductive film material.

[0016] Preferably, in the preparation method of the high thermal conductivity diamond / copper composite conductive film material of the present invention, in step one, a first mixed material is prepared according to a ratio of pine alcohol, polyethylene glycol 400, ethyl cellulose and polyoxypropylene, and the prepared first mixed material is subjected to a first water bath stirring treatment, including: preparing the first mixed material with 70-80 parts by weight of pine alcohol, 14-24 parts by weight of polyethylene glycol 400, 3 parts by weight of ethyl cellulose and 3 parts by weight of polyoxypropylene, and stirring the prepared first mixed material in a water bath at a temperature of 80-100°C for 1-3h.

[0017] Preferably, in the preparation method of the high thermal conductivity diamond / copper composite conductive film material of the present invention, in step one, a second mixed material is prepared by using a mixed solution of diamond powder and an organic carrier according to a ratio, and the prepared second mixed material is subjected to a second water bath stirring treatment, including: preparing the second mixed material using 1-4 parts by weight of diamond powder and 14-18 parts by weight of an organic carrier mixed solution, stirring the prepared second mixed material in a water bath at a temperature of 60-80°C for 2-4h, and the average particle size of the diamond powder is 0.2-0.25μm.

[0018] Preferably, in the preparation method of the high thermal conductivity diamond / copper composite conductive film material of the present invention, in step 2, silica powder, sodium oxide powder and calcium oxide powder are mixed in proportion to obtain an inorganic mixed powder, comprising: mixing 70-85 parts by weight of silica powder, 10-20 parts by weight of sodium oxide and 5-10 parts by weight of calcium oxide powder to obtain an inorganic mixed powder.

[0019] Preferably, in the method for preparing the high thermal conductivity diamond / copper composite conductive film material of the present invention, in step 2, the obtained inorganic mixed powder is subjected to vitrification treatment and refinement treatment in sequence to prepare bonding glass powder, comprising:

[0020] The obtained inorganic mixed powder is roller-milled for 12-18 hours, heated to 1000-1200°C, kept warm for 1-3 hours, and then water-cooled to obtain a vitrified material;

[0021] The vitrified material is ball-milled for 24-36 hours at a ball-to-material ratio of 20:1, and the ball-milled material is screened to obtain a bonding glass powder.

[0022] Preferably, in the preparation method of the high thermal conductivity diamond / copper composite conductive film material of the present invention, in step 2, a third mixed material is prepared according to a ratio of copper powder, an organic carrier / diamond powder mixed solution and a bonding glass powder, and the prepared third mixed material is subjected to a third water bath stirring treatment, including: 70-78 parts by weight of copper powder and 6-10 parts by weight of bonding glass powder are roller-milled for 6 hours, the roller-milled mixed material is mixed with 15-22 parts by weight of an organic carrier / diamond powder mixed solution, and then stirred in a water bath at a temperature of 60-80°C for 2-4 hours, and the average particle size of the copper powder is 3-5μm.

[0023] Preferably, in the method for preparing the high thermal conductivity diamond / copper composite conductive film material of the present invention, in step three, coating the diamond / copper composite conductive slurry on the surface of the ceramic substrate, comprising: using a screen with an aperture of 200 mesh to print the diamond / copper composite conductive slurry on the surface of the ceramic substrate, the ceramic substrate is made of an aluminum oxide material with a purity of not less than 99%, and the average surface roughness of the ceramic substrate is not greater than Ra0.8.

[0024] Preferably, in the method for preparing the high thermal conductivity diamond / copper composite conductive film material of the present invention, in step three, the ceramic substrate coated with the diamond / copper composite conductive slurry is subjected to vacuum leveling treatment, including: placing the ceramic substrate coated with the diamond / copper composite conductive slurry in a vacuum and heating it to 80-120° C., and keeping it warm for 10-50 minutes.

[0025] Preferably, in the preparation method of the high thermal conductivity diamond / copper composite conductive film material of the present invention, in step three, the diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere for degreasing treatment and sintering treatment in sequence, including: placing the diamond / copper composite conductive slurry coated leveling component in a protective atmosphere, heating the temperature to 500°C at a heating rate of 1-3°C / min and then keeping it warm for 2-5h, heating the temperature to 700-900°C at a heating rate of 5-10°C / min and then keeping it warm for 0.5-2h.

[0026] According to another aspect of the present invention, the present invention provides a high thermal conductivity diamond / copper composite conductive film material, and the high thermal conductivity diamond / copper composite conductive film material is prepared according to the above method.

[0027] The preparation method of the high thermal conductivity diamond / copper composite conductive film material and the corresponding material of the present invention have the following beneficial effects:

[0028] 1. By preparing an organic carrier mixed liquid and mixing it with diamond powder to form an organic carrier / diamond powder mixed liquid, the submicron diamond powder is evenly dispersed in the organic carrier, so that the diamond powder in the conductive film is concentrated in the gap formed after the organic carrier volatilizes, so that the conductive channel of the conductive film is not destroyed;

[0029] 2. By preparing a bonding glass powder with a low thermal expansion coefficient and uniformly mixing it with copper powder and an organic carrier / diamond powder mixture to form a diamond / copper composite conductive slurry, the prepared conductive film has a higher resistance to thermal deformation, thereby improving the thermal stability of the composite conductive film;

[0030] 3. Through vacuum leveling, degreasing and sintering processes, the conductive slurry is prepared into a diamond / copper composite conductive film with high thermal conductivity and low resistivity;

[0031] 4. The prepared high thermal conductivity diamond / copper composite conductive film material has strong heat dissipation, can withstand higher operating temperatures, and is suitable for application in high-precision integrated circuits. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0033] Figure 1 A flow chart of a method for preparing a high thermal conductivity diamond / copper composite conductive film material according to exemplary embodiments 1-5 of the present invention;

[0034] Figure 2 This is a SEM morphology image of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 1 of the present invention;

[0035] Figure 3 This is a SEM morphology image of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 2 of the present invention;

[0036] Figure 4 This is a SEM morphology image of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 3 of the present invention;

[0037] Figure 5 This is a SEM morphology image of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 4 of the present invention;

[0038] Figure 6 This is a SEM morphology image of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 5 of the present invention;

[0039] Figure 7 This is a SEM morphology image of the copper conductive thin film material prepared in Example 6 (comparative example) of the present invention;

[0040] Figure 8 This is a local area EDS spectrum of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 3 of the present invention;

[0041] Fig. 9 This is a local area EDS spectrum of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 5 of the present invention;

[0042] Fig.10 : This is the TMA curve of the bonding glass powder and the ceramic substrate in Example 5 of the present invention. DETAILED DESCRIPTION

[0043] The embodiments of the present invention are described in detail below with reference to the accompanying drawings.

[0044] It should be noted that the following embodiments and features in the embodiments may be combined with each other in the absence of conflict; and, based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in the field without making any creative work are within the scope of protection of the present disclosure.

[0045] It should be noted that various aspects of the embodiments within the scope of the appended claims are described below. It should be apparent that the aspects described herein may be embodied in a wide variety of forms, and any specific structure and / or function described herein is merely illustrative. Based on the present disclosure, it should be understood by those skilled in the art that an aspect described herein may be implemented independently of any other aspect, and two or more of these aspects may be combined in various ways. For example, any number of aspects described herein may be used to implement the device and / or practice the method. In addition, other structures and / or functionalities other than one or more of the aspects described herein may be used to implement this device and / or practice this method.

[0046] The present invention prepares a diamond / copper composite conductive slurry having both high thermal conductivity and low resistivity by uniformly mixing submicron ultrafine diamond powder with an organic carrier mixed liquid to form an organic carrier / diamond powder mixed liquid, and doping the diamond powder into the gaps of micron copper powder through the organic carrier mixed liquid, and then prepares a high thermal conductivity diamond / copper composite conductive film material through vacuum leveling treatment, degreasing treatment and sintering treatment. Figure 1 Flow chart of the method for preparing the high thermal conductivity diamond / copper composite conductive film material of exemplary embodiments 1 to 5 of the present invention. Figure 1 Implemented in the manner shown.

[0047] Example 1

[0048] Preparation of high thermal conductivity diamond / copper composite conductive film materials:

[0049] Step 1: Preparation of organic carrier / diamond powder mixture

[0050] A first mixed material is prepared by using terpineol, polyethylene glycol 400, ethyl cellulose and polyoxypropylene according to a ratio, and the prepared first mixed material is subjected to a first water bath stirring treatment. Specifically, 80 parts by weight of terpineol, 14 parts by weight of polyethylene glycol 400, 3 parts by weight of ethyl cellulose and 3 parts by weight of polyoxypropylene are used to prepare the first mixed material, and the prepared first mixed material is stirred in a water bath at a temperature of 80° C. for 1 hour to obtain an organic carrier mixed solution;

[0051] A second mixed material is prepared by using a mixture of diamond powder and an organic carrier according to a ratio, and the prepared second mixed material is subjected to a second water bath stirring treatment. Specifically, 1 part by weight of diamond powder with an average particle size of 0.2-0.25 μm and 14 parts by weight of an organic carrier mixed solution are used to prepare the second mixed material, and the prepared second mixed material is stirred in a water bath at a temperature of 60° C. for 2 hours to obtain an organic carrier / diamond powder mixed solution;

[0052] Step 2: Preparation of diamond / copper composite conductive slurry

[0053] Silicon dioxide, sodium oxide and calcium oxide are mixed according to a ratio to obtain an inorganic mixed powder, and the obtained inorganic mixed powder is subjected to a vitrification treatment and a refinement treatment in sequence. Specifically, 85 parts by weight of silicon dioxide powder, 10 parts by weight of sodium oxide and 5 parts by weight of calcium oxide powder are mixed to obtain an inorganic mixed powder; the obtained inorganic mixed powder is subjected to a roller milling treatment for 12 hours, and then heated to 1000° C., kept warm for 1 hour and then water-cooled to obtain a vitrified material; the vitrified material is ball-milled for 24 hours at a ball-to-material ratio of 20:1, and the ball-milled material is screened with a 200-mesh sieve to obtain a bonding glass powder;

[0054] A third mixed material is prepared by using copper powder, an organic carrier / diamond powder mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment. Specifically, the third mixed material is prepared by using copper powder, an organic carrier / diamond powder mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment, including: 70 parts by weight of copper powder with an average particle size of 3-5 μm and 6 parts by weight of bonding glass powder are roller-milled for 6 hours, the roller-milled mixed material is mixed with 15 parts by weight of the organic carrier / diamond powder mixed solution, and then stirred in a water bath at 60° C. for 2 hours to obtain a diamond / copper composite conductive slurry;

[0055] Step 3: Preparation of high thermal conductivity diamond / copper composite conductive film material

[0056] The diamond / copper composite conductive slurry is coated on the surface of the ceramic substrate, and the ceramic substrate coated with the diamond / copper composite conductive slurry is subjected to vacuum leveling treatment. Specifically, the diamond / copper composite conductive slurry is printed on a ceramic substrate made of an aluminum oxide material with a purity of not less than 99% and a surface average roughness of not more than Ra0.8 using a screen with an aperture of 200 meshes, and the ceramic substrate coated with the diamond / copper composite conductive slurry is placed in a vacuum and heated to 80° C., and kept warm for 10 minutes to obtain a diamond / copper composite conductive slurry coated leveling component;

[0057] The diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere for degreasing treatment and sintering treatment in sequence. Specifically, the diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere, heated to 500°C at a heating rate of 3°C / min and then kept warm for 2 hours, and heated to 700°C at a heating rate of 10°C / min and then kept warm for 0.5 hours to obtain a high thermal conductivity diamond / copper composite conductive film material.

[0058] Example 2

[0059] Preparation of high thermal conductivity diamond / copper composite conductive film materials:

[0060] Step 1: Preparation of organic carrier / diamond powder mixture

[0061] A first mixed material is prepared by using terpineol, polyethylene glycol 400, ethyl cellulose and polyoxypropylene according to a ratio, and the prepared first mixed material is subjected to a first water bath stirring treatment. Specifically, the first mixed material is prepared by using 76 parts by weight of terpineol, 18 parts by weight of polyethylene glycol 400, 3 parts by weight of ethyl cellulose and 3 parts by weight of polyoxypropylene, and the prepared first mixed material is stirred in a water bath at a temperature of 90° C. for 1.5 hours to obtain an organic carrier mixed solution;

[0062] A second mixed material is prepared by using a mixture of diamond powder and an organic carrier according to a ratio, and the prepared second mixed material is subjected to a second water bath stirring treatment. Specifically, 1 part by weight of diamond powder with an average particle size of 0.2-0.25 μm and 14 parts by weight of an organic carrier mixed solution are used to prepare the second mixed material, and the prepared second mixed material is stirred in a water bath at a temperature of 70° C. for 3 hours to obtain an organic carrier / diamond powder mixed solution;

[0063] Step 2: Preparation of diamond / copper composite conductive slurry

[0064] Silicon dioxide, sodium oxide and calcium oxide are mixed according to a ratio to obtain an inorganic mixed powder, and the obtained inorganic mixed powder is subjected to a vitrification treatment and a refinement treatment in sequence. Specifically, 85 parts by weight of silicon dioxide powder, 10 parts by weight of sodium oxide and 5 parts by weight of calcium oxide powder are mixed to obtain an inorganic mixed powder; the obtained inorganic mixed powder is subjected to a roller milling treatment for 14 hours, and then heated to 1000° C., kept warm for 1 hour and then water-cooled to obtain a vitrified material; the vitrified material is ball-milled for 28 hours at a ball-to-material ratio of 20:1, and the ball-milled material is screened with a 200-mesh sieve to obtain a bonding glass powder;

[0065] A third mixed material is prepared by using copper powder, an organic carrier / diamond powder mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment. Specifically, the third mixed material is prepared by using copper powder, an organic carrier / diamond powder mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment, including: 72 parts by weight of copper powder with an average particle size of 3-5 μm and 6 parts by weight of bonding glass powder are roller-milled for 6 hours, the roller-milled mixed material is mixed with 15 parts by weight of the organic carrier / diamond powder mixed solution, and then stirred in a water bath at a temperature of 70° C. for 3 hours to obtain a diamond / copper composite conductive slurry;

[0066] Step 3: Preparation of high thermal conductivity diamond / copper composite conductive film material

[0067] The diamond / copper composite conductive slurry is coated on the surface of the ceramic substrate, and the ceramic substrate coated with the diamond / copper composite conductive slurry is subjected to vacuum leveling treatment. Specifically, the diamond / copper composite conductive slurry is printed on a ceramic substrate made of an aluminum oxide material with a purity of not less than 99% and a surface average roughness of not more than Ra0.8 using a screen with an aperture of 200 meshes, and the ceramic substrate coated with the diamond / copper composite conductive slurry is placed in a vacuum and heated to 90° C., and kept warm for 20 minutes to obtain a diamond / copper composite conductive slurry coated leveling component;

[0068] The diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere for degreasing treatment and sintering treatment in sequence. Specifically, the diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere, heated to 500°C at a heating rate of 2°C / min and then kept warm for 2 hours, and heated to 700°C at a heating rate of 10°C / min and then kept warm for 0.5 hours to obtain a high thermal conductivity diamond / copper composite conductive film material.

[0069] Example 3

[0070] Preparation of high thermal conductivity diamond / copper composite conductive film materials:

[0071] Step 1: Preparation of organic carrier / diamond powder mixture

[0072] A first mixed material is prepared by using terpineol, polyethylene glycol 400, ethyl cellulose and polyoxypropylene according to a ratio, and the prepared first mixed material is subjected to a first water bath stirring treatment. Specifically, the first mixed material is prepared by using 72 parts by weight of terpineol, 22 parts by weight of polyethylene glycol 400, 3 parts by weight of ethyl cellulose and 3 parts by weight of polyoxypropylene, and the prepared first mixed material is stirred in a water bath at a temperature of 100° C. for 2 hours to obtain an organic carrier mixed solution;

[0073] A second mixed material is prepared by using a mixture of diamond powder and an organic carrier according to a ratio, and the prepared second mixed material is subjected to a second water bath stirring treatment. Specifically, 2 parts by weight of diamond powder with an average particle size of 0.2-0.25 μm and 16 parts by weight of an organic carrier mixed solution are used to prepare the second mixed material, and the prepared second mixed material is stirred in a water bath at a temperature of 80° C. for 4 hours to obtain an organic carrier / diamond powder mixed solution;

[0074] Step 2: Preparation of diamond / copper composite conductive slurry

[0075] Silicon dioxide, sodium oxide and calcium oxide are mixed according to a ratio to obtain an inorganic mixed powder, and the obtained inorganic mixed powder is subjected to a vitrification treatment and a refinement treatment in sequence. Specifically, 80 parts by weight of silicon dioxide powder, 15 parts by weight of sodium oxide and 5 parts by weight of calcium oxide powder are mixed to obtain an inorganic mixed powder; the obtained inorganic mixed powder is subjected to a roller milling treatment for 16 hours, and then heated to 1100° C., kept warm for 2 hours and then water-cooled to obtain a vitrified material; the vitrified material is ball-milled for 32 hours at a ball-to-material ratio of 20:1, and the ball-milled material is screened with a 200-mesh sieve to obtain a bonding glass powder;

[0076] A third mixed material is prepared by using copper powder, an organic carrier / diamond powder mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment. Specifically, the third mixed material is prepared by using copper powder, an organic carrier / diamond powder mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment, including: 74 parts by weight of copper powder with an average particle size of 3-5 μm and 8 parts by weight of bonding glass powder are roller-milled for 6 hours, the roller-milled mixed material is mixed with 18 parts by weight of the organic carrier / diamond powder mixed solution, and then stirred in a water bath at a temperature of 80° C. for 4 hours to obtain a diamond / copper composite conductive slurry;

[0077] Step 3: Preparation of high thermal conductivity diamond / copper composite conductive film material

[0078] The diamond / copper composite conductive slurry is coated on the surface of the ceramic substrate, and the ceramic substrate coated with the diamond / copper composite conductive slurry is subjected to vacuum leveling treatment. Specifically, the diamond / copper composite conductive slurry is printed on a ceramic substrate made of an aluminum oxide material with a purity of not less than 99% and a surface average roughness of not more than Ra0.8 using a screen with an aperture of 200 meshes, and the ceramic substrate coated with the diamond / copper composite conductive slurry is placed in a vacuum and heated to 100° C., and kept warm for 30 minutes to obtain a diamond / copper composite conductive slurry coated leveling component;

[0079] The diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere for degreasing treatment and sintering treatment in sequence. Specifically, the diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere, heated to 500°C at a heating rate of 2°C / min and then kept warm for 3 hours, and heated to 700°C at a heating rate of 8°C / min and then kept warm for 1 hour to obtain a high thermal conductivity diamond / copper composite conductive film material.

[0080] Example 4

[0081] Preparation of high thermal conductivity diamond / copper composite conductive film materials:

[0082] Step 1: Preparation of organic carrier / diamond powder mixture

[0083] A first mixed material is prepared by using terpineol, polyethylene glycol 400, ethyl cellulose and polyoxypropylene according to a ratio, and the prepared first mixed material is subjected to a first water bath stirring treatment. Specifically, the first mixed material is prepared by using 70 parts by weight of terpineol, 24 parts by weight of polyethylene glycol 400, 3 parts by weight of ethyl cellulose and 3 parts by weight of polyoxypropylene, and the prepared first mixed material is stirred in a water bath at a temperature of 100° C. for 2.5 hours to obtain an organic carrier mixed solution;

[0084] A second mixed material is prepared by using a mixture of diamond powder and an organic carrier according to a ratio, and the prepared second mixed material is subjected to a second water bath stirring treatment. Specifically, 4 parts by weight of diamond powder with an average particle size of 0.2-0.25 μm and 16 parts by weight of an organic carrier mixed solution are used to prepare the second mixed material, and the prepared second mixed material is stirred in a water bath at a temperature of 80° C. for 4 hours to obtain an organic carrier / diamond powder mixed solution;

[0085] Step 2: Preparation of diamond / copper composite conductive slurry

[0086] Silicon dioxide, sodium oxide and calcium oxide are mixed according to a ratio to obtain an inorganic mixed powder, and the obtained inorganic mixed powder is subjected to a vitrification treatment and a refinement treatment in sequence. Specifically, 75 parts by weight of silicon dioxide powder, 15 parts by weight of sodium oxide and 10 parts by weight of calcium oxide powder are mixed to obtain an inorganic mixed powder; the obtained inorganic mixed powder is roller-milled for 18 hours, heated to 1100° C., kept warm for 2 hours and then water-cooled to obtain a vitrified material; the vitrified material is ball-milled for 36 hours at a ball-to-material ratio of 20:1, and the ball-milled material is screened with a 200-mesh screen to obtain a bonding glass powder;

[0087] A third mixed material is prepared by using copper powder, an organic carrier / diamond powder mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment. Specifically, the third mixed material is prepared by using copper powder, an organic carrier / diamond powder mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment, including: 76 parts by weight of copper powder with an average particle size of 3-5 μm and 10 parts by weight of bonding glass powder are roller-milled for 6 hours, the roller-milled mixed material is mixed with 20 parts by weight of the organic carrier / diamond powder mixed solution, and then stirred in a water bath at a temperature of 80° C. for 4 hours to obtain a diamond / copper composite conductive slurry;

[0088] Step 3: Preparation of high thermal conductivity diamond / copper composite conductive film material

[0089] The diamond / copper composite conductive slurry is coated on the surface of the ceramic substrate, and the ceramic substrate coated with the diamond / copper composite conductive slurry is subjected to vacuum leveling treatment. Specifically, the diamond / copper composite conductive slurry is printed on a ceramic substrate made of an aluminum oxide material with a purity of not less than 99% and a surface average roughness of not more than Ra0.8 using a screen with an aperture of 200 meshes, and the ceramic substrate coated with the diamond / copper composite conductive slurry is placed in a vacuum and heated to 110° C., and kept warm for 40 minutes to obtain a diamond / copper composite conductive slurry coated leveling component;

[0090] The diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere for degreasing treatment and sintering treatment in sequence. Specifically, the diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere, heated to 500°C at a heating rate of 1°C / min and then kept warm for 4 hours, and heated to 800°C at a heating rate of 6°C / min and then kept warm for 1.5 hours to obtain a high thermal conductivity diamond / copper composite conductive film material.

[0091] Example 5

[0092] Preparation of high thermal conductivity diamond / copper composite conductive film materials:

[0093] Step 1: Preparation of organic carrier / diamond powder mixture

[0094] A first mixed material is prepared by using terpineol, polyethylene glycol 400, ethyl cellulose and polyoxypropylene according to a ratio, and the prepared first mixed material is subjected to a first water bath stirring treatment. Specifically, the first mixed material is prepared by using 70 parts by weight of terpineol, 24 parts by weight of polyethylene glycol 400, 3 parts by weight of ethyl cellulose and 3 parts by weight of polyoxypropylene, and the prepared first mixed material is stirred in a water bath at a temperature of 100° C. for 3 hours to obtain an organic carrier mixed solution;

[0095] A second mixed material is prepared by using a mixture of diamond powder and an organic carrier according to a ratio, and the prepared second mixed material is subjected to a second water bath stirring treatment. Specifically, 4 parts by weight of diamond powder with an average particle size of 0.2-0.25 μm and 18 parts by weight of an organic carrier mixed solution are used to prepare the second mixed material, and the prepared second mixed material is stirred in a water bath at a temperature of 80° C. for 4 hours to obtain an organic carrier / diamond powder mixed solution;

[0096] Step 2: Preparation of diamond / copper composite conductive slurry

[0097] Silicon dioxide, sodium oxide and calcium oxide are mixed according to a ratio to obtain an inorganic mixed powder, and the obtained inorganic mixed powder is subjected to a vitrification treatment and a refinement treatment in sequence. Specifically, 70 parts by weight of silicon dioxide powder, 20 parts by weight of sodium oxide and 10 parts by weight of calcium oxide powder are mixed to obtain an inorganic mixed powder; the obtained inorganic mixed powder is subjected to a roller milling treatment for 18 hours, and then heated to 1200° C., kept warm for 3 hours and then water-cooled to obtain a vitrified material; the vitrified material is ball-milled for 36 hours at a ball-to-material ratio of 20:1, and the ball-milled material is screened with a 200-mesh sieve to obtain a bonding glass powder;

[0098] A third mixed material is prepared by using copper powder, an organic carrier / diamond powder mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment. Specifically, the third mixed material is prepared by using copper powder, an organic carrier / diamond powder mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment, including: 78 parts by weight of copper powder with an average particle size of 3-5 μm and 10 parts by weight of bonding glass powder are roller-milled for 6 hours, and the roller-milled mixed material is mixed with 22 parts by weight of the organic carrier / diamond powder mixed solution, and then stirred in a water bath at a temperature of 80° C. for 4 hours to obtain a diamond / copper composite conductive slurry;

[0099] Step 3: Preparation of high thermal conductivity diamond / copper composite conductive film material

[0100] The diamond / copper composite conductive slurry is coated on the surface of the ceramic substrate, and the ceramic substrate coated with the diamond / copper composite conductive slurry is subjected to vacuum leveling treatment. Specifically, the diamond / copper composite conductive slurry is printed on a ceramic substrate made of an aluminum oxide material with a purity of not less than 99% and a surface average roughness of not more than Ra0.8 using a screen with an aperture of 200 meshes, and the ceramic substrate coated with the diamond / copper composite conductive slurry is placed in a vacuum and heated to 120° C., and kept warm for 50 minutes to obtain a diamond / copper composite conductive slurry coated leveling component;

[0101] The diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere for degreasing treatment and sintering treatment in sequence. Specifically, the diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere, heated to 500°C at a heating rate of 1°C / min and then kept warm for 5 hours, and heated to 900°C at a heating rate of 5°C / min and then kept warm for 2 hours to obtain a high thermal conductivity diamond / copper composite conductive film material.

[0102] Example 6 (Comparative Example)

[0103] Preparation of copper conductive film materials:

[0104] Step 1: Preparation of organic carrier mixture

[0105] A first mixed material is prepared by using terpineol, polyethylene glycol 400, ethyl cellulose and polyoxypropylene according to a ratio, and the prepared first mixed material is subjected to a first water bath stirring treatment. Specifically, 80 parts by weight of terpineol, 14 parts by weight of polyethylene glycol 400, 3 parts by weight of ethyl cellulose and 3 parts by weight of polyoxypropylene are used to prepare the first mixed material, and the prepared first mixed material is stirred in a water bath at a temperature of 80° C. for 1 hour to obtain an organic carrier mixed solution;

[0106] Step 2: Preparation of copper conductive paste

[0107] Silicon dioxide, sodium oxide and calcium oxide are mixed according to a ratio to obtain an inorganic mixed powder, and the obtained inorganic mixed powder is subjected to a vitrification treatment and a refinement treatment in sequence. Specifically, 85 parts by weight of silicon dioxide powder, 10 parts by weight of sodium oxide and 5 parts by weight of calcium oxide powder are mixed to obtain an inorganic mixed powder; the obtained inorganic mixed powder is subjected to a roller milling treatment for 12 hours, and then heated to 1000° C., kept warm for 1 hour and then water-cooled to obtain a vitrified material; the vitrified material is ball-milled for 24 hours at a ball-to-material ratio of 20:1, and the ball-milled material is screened with a 200-mesh sieve to obtain a bonding glass powder;

[0108] A third mixed material is prepared by using copper powder, an organic carrier mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment. Specifically, the third mixed material is prepared by using copper powder, an organic carrier mixed solution and a bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment, including: 70 parts by weight of copper powder with an average particle size of 3-5 μm and 6 parts by weight of bonding glass powder are roller-milled for 6 hours, the roller-milled mixed material is mixed with 14 parts by weight of an organic carrier / diamond powder mixed solution, and then stirred in a water bath at 60° C. for 2 hours to obtain a diamond / copper composite conductive slurry;

[0109] Step 3: Preparation of copper conductive film material

[0110] Coating the copper conductive paste on the surface of the ceramic substrate, and performing vacuum leveling treatment on the ceramic substrate coated with the copper conductive paste. Specifically, using a screen with an aperture of 200 meshes to print the copper conductive paste on a ceramic substrate made of an aluminum oxide material with a purity of not less than 99% and a surface average roughness of not more than Ra0.8, placing the ceramic substrate coated with the copper conductive paste in a vacuum and heating it to 80° C., keeping the temperature for 10 minutes, and obtaining a copper conductive paste coated leveling component;

[0111] The copper conductive slurry coated leveling component is placed in a protective atmosphere for degreasing treatment and sintering treatment in sequence. Specifically, the copper conductive slurry coated leveling component is placed in a protective atmosphere, heated to 500°C at a heating rate of 3°C / min and then kept warm for 2 hours, and heated to 700°C at a heating rate of 10°C / min and then kept warm for 0.5 hours to obtain a copper conductive film material.

[0112] Example 7

[0113] The high thermal conductivity diamond / copper composite conductive film materials prepared in Examples 1-5 and the copper conductive film materials prepared in Example 6 (comparative example) were characterized by SEM microscopic morphology and EDS using a Hitachi SU8020 cold field emission scanning electron microscope. The SEM morphology of the high thermal conductivity diamond / copper composite conductive film materials prepared in Examples 1-5 is shown in the table below. Figure 2 , Figure 3 , Figure 4 , Figure 5 and Figure 6 The SEM microstructure of the copper conductive film material prepared in Example 6 (Comparative Example) is shown in Figure 7 ; The local area EDS spectrum of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 3 is shown in Figure 8 The local EDS spectrum of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 5 is shown in Fig. 9 .

[0114] Figure 2 This is a SEM morphology image of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 1 of the present invention; Figure 3 This is a SEM morphology image of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 2 of the present invention; Figure 4 This is a SEM morphology image of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 3 of the present invention; Figure 5 This is a SEM morphology image of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 4 of the present invention; Figure 6 This is a SEM morphology image of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 5 of the present invention; Figure 7 This is a SEM morphology of the copper conductive film material prepared in Example 6 (comparative example) of the present invention; Figure 7 As shown in Figure 2, there are many gaps inside the conductive film without diamond powder doping, which indicates that the conductive and thermal conduction channels of the copper conductive film are imperfect, which is not conducive to improving the electrical and thermal conductivity of the film; Figure 2 As shown in FIG. 1 , after doping with diamond powder, some gaps in the copper film are filled with diamond powder to form a diamond / copper composite conductive film, the thermal conduction channel of the film is improved and the conductive channel of the film is not damaged; Figure 3As shown in FIG. 1 , reducing the heating rate in the degreasing stage is conducive to more complete volatilization of the organic carrier, increasing the proportion of copper in the film, and thus improving the electrical conductivity and thermal conductivity of the conductive film; as shown in FIG. Figure 4 As shown in FIG, after increasing the doping of diamond powder, the gaps in the conductive film are filled with a large amount of diamond powder, and the heat conduction channel of the conductive film is more complete; Figures 5 and 6 As shown in the figure, after continuing to increase the doping of diamond powder, most of the gaps in the conductive film are filled with diamond powder, forming a very complete thermal conduction channel inside the film. At the same time, with the increase of sintering temperature and time, the conductive channel formed by the connection of copper particles becomes denser, which is beneficial to improving the electrical conductivity and thermal conductivity of the conductive film.

[0115] Figure 8 This is a local area EDS spectrum of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 3 of the present invention; Fig. 9 This is a local EDS spectrum of the high thermal conductivity diamond / copper composite conductive film material prepared in Example 5 of the present invention; Figure 8 As shown in the figure, after doping diamond powder in copper conductive paste, the corresponding C element appears in the EDS spectrum of the prepared composite conductive film, and the C element is concentrated in the gaps of Cu, which indicates that the doped diamond powder can effectively supplement the thermal conduction channel of the conductive film, thereby improving the thermal conductivity of the conductive film; Fig. 9 As shown in the figure, as the diamond powder in the conductive paste increases, the gaps in Cu are almost completely filled with C elements, and the C elements are continuously distributed, which indicates that a very complete thermal conduction channel is formed inside the composite conductive film. Therefore, doping diamond powder in copper conductive paste is conducive to the preparation of high thermal conductivity diamond / copper composite conductive film materials.

[0116] The thermal expansion coefficients of the bonding glass powder and the ceramic substrate in Example 5 of the present invention were tested by a German STA 449F3 synchronous thermal analyzer, and the TMA curve was measured. Fig.10 . Fig.10 This is the TMA curve of the bonding glass powder and the ceramic substrate in Example 5 of the present invention. By comparing the thermal expansion coefficients of the bonding glass powder and the ceramic substrate, it can be seen that when the temperature does not exceed 400°C, the thermal expansion coefficient of the bonding glass powder is extremely low, and has a high consistency with the thermal expansion coefficient of the ceramic substrate, which is beneficial to improving the thermal deformation resistance of the copper conductive paste and the thermal stability of the PCB material.

[0117] Table 1 shows the performance parameters of the high thermal conductivity diamond / copper composite conductive film materials prepared by exemplary embodiments 1-5 of the present invention and the copper conductive film materials prepared by Example 6 (comparative example). The resistivity is obtained by four-probe test method, and the measuring instrument is CXT 2516 resistor meter, referring to the test standard "GB / T 17473-2008 Part 3: Square resistance determination", where mΩ / □ represents milliohms per square centimeter; the bonding strength is measured by ZQ-21A tensile testing machine, referring to the test standard "GB / T17473-2008 Part 4: Adhesion determination"; the thermal conductivity is measured by LFA457 laser thermal conductivity meter, referring to the test standard "GB / T 10294-2008 Thermal conductivity test method Thermal conductivity determination method".

[0118] like Figures 2 to 6 As can be seen from the corresponding performance parameters in Table 1, by introducing high thermal conductivity submicron diamond powder, doping it into the gaps of the conductive filler through an organic carrier / diamond powder mixture, and improving the thermal expansion coefficient of the bonding glass powder, the thermal conductivity of the high thermal conductivity diamond / copper composite conductive film material can be significantly improved while maintaining a low square resistance.

[0119] Depend on Figure 4 and Figure 6 As can be seen from the corresponding square resistance in Table 1, the submicron diamond powder inside the film is mainly distributed in the pores between the micron copper particles, without destroying the conductive channel formed by the connection of the copper particles, so that the high thermal conductivity diamond / copper composite conductive film material maintains a low resistivity.

[0120] Depend on Figure 4 and Figure 6 As can be seen from the corresponding thermal conductivity in Table 1, by increasing the weight of diamond powder in the conductive slurry, the thermal conduction channel of the conductive film can be further improved, and the thermal conductivity of the high thermal conductivity diamond / copper composite conductive film material can be improved.

[0121] Table 1

[0122]

[0123]

[0124] A method for preparing a high thermal conductivity diamond / copper composite conductive film material and corresponding materials according to an embodiment of the present invention have the following beneficial technical effects:

[0125] 1. By preparing an organic carrier mixed liquid and mixing it with diamond powder to form an organic carrier / diamond powder mixed liquid, the submicron diamond powder is evenly dispersed in the organic carrier, so that the diamond powder in the conductive film is concentrated in the gap formed after the organic carrier volatilizes, so that the conductive channel of the conductive film is not destroyed;

[0126] 2. By preparing a bonding glass powder with a low thermal expansion coefficient and uniformly mixing it with copper powder and an organic carrier / diamond powder mixture to form a diamond / copper composite conductive slurry, the prepared conductive film has a higher resistance to thermal deformation, thereby improving the thermal stability of the composite conductive film;

[0127] 3. Through vacuum leveling, degreasing and sintering processes, the conductive slurry is prepared into a diamond / copper composite conductive film with high thermal conductivity and low resistivity;

[0128] 4. The prepared high thermal conductivity diamond / copper composite conductive film material has strong heat dissipation, can withstand higher operating temperatures, and is suitable for application in high-precision integrated circuits.

[0129] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.

Claims

1. A method for preparing a high thermal conductivity diamond / copper composite conductive film material, characterized in that: The method comprises: Step 1: Preparation of organic carrier / diamond powder mixture A first mixed material is prepared by using terpineol, polyethylene glycol 400, ethyl cellulose and polyoxypropylene according to a ratio, and the prepared first mixed material is subjected to a first water bath stirring treatment to prepare an organic carrier mixed solution; A second mixed material is prepared by using a mixture of diamond powder and an organic carrier according to a ratio, and the prepared second mixed material is subjected to a second water bath stirring treatment to obtain an organic carrier / diamond powder mixed solution; Step 2: Preparation of diamond / copper composite conductive slurry Mixing silicon dioxide, sodium oxide and calcium oxide according to a ratio to obtain an inorganic mixed powder, and sequentially performing vitrification treatment and refinement treatment on the obtained inorganic mixed powder to obtain a bonding glass powder; A third mixed material is prepared by using copper powder, organic carrier / diamond powder mixed solution and bonding glass powder according to a ratio, and the prepared third mixed material is subjected to a third water bath stirring treatment to obtain a diamond / copper composite conductive slurry; Step 3: Preparation of high thermal conductivity diamond / copper composite conductive film material The diamond / copper composite conductive slurry is coated on the surface of the ceramic substrate, and the ceramic substrate coated with the diamond / copper composite conductive slurry is subjected to vacuum leveling treatment to obtain a diamond / copper composite conductive slurry coated leveling component; The diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere for degreasing treatment and sintering treatment in sequence to obtain a high thermal conductivity diamond / copper composite conductive film material.

2. The method for preparing the high thermal conductivity diamond / copper composite conductive film material according to claim 1, characterized in that: In step one, a first mixed material is prepared using terpineol, polyethylene glycol 400, ethyl cellulose and polyoxypropylene according to a ratio, and the prepared first mixed material is subjected to a first water bath stirring treatment, including: preparing the first mixed material using 70-80 parts by weight of terpineol, 14-24 parts by weight of polyethylene glycol 400, 3 parts by weight of ethyl cellulose and 3 parts by weight of polyoxypropylene, and stirring the prepared first mixed material in a water bath at a temperature of 80-100° C. for 1-3 hours.

3. The method for preparing the high thermal conductivity diamond / copper composite conductive film material according to claim 1, characterized in that: In step one, a second mixed material is prepared by using a mixture of diamond powder and an organic carrier according to a ratio, and the prepared second mixed material is subjected to a second water bath stirring treatment, including: preparing the second mixed material by using 1-4 parts by weight of diamond powder and 14-18 parts by weight of an organic carrier mixed solution, stirring the prepared second mixed material in a water bath at a temperature of 60-80°C for 2-4h, wherein the average particle size of the diamond powder is 0.2-0.25μm.

4. The method for preparing the high thermal conductivity diamond / copper composite conductive film material according to claim 1, characterized in that: In step 2, silica powder, sodium oxide powder and calcium oxide powder are mixed according to a ratio to obtain an inorganic mixed powder, including: mixing 70-85 parts by weight of silica powder, 10-20 parts by weight of sodium oxide and 5-10 parts by weight of calcium oxide powder to obtain an inorganic mixed powder.

5. The method for preparing the high thermal conductivity diamond / copper composite conductive film material according to claim 1, characterized in that: In step 2, the obtained inorganic mixed powder is subjected to vitrification treatment and refinement treatment in sequence. The method comprises preparing a bonding glass powder, comprising: The obtained inorganic mixed powder is roller-milled for 12-18 hours, heated to 1000-1200°C, kept warm for 1-3 hours, and then water-cooled to obtain a vitrified material; The vitrified material is ball-milled for 24-36 hours at a ball-to-material ratio of 20:1, and the ball-milled material is screened to obtain a bonding glass powder.

6. The method for preparing the high thermal conductivity diamond / copper composite conductive film material according to claim 1, characterized in that: In step 2, a third mixed material is prepared according to a ratio of copper powder, an organic carrier / diamond powder mixture and a bonding glass powder, and the prepared third mixed material is subjected to a third water bath stirring treatment, including: roller milling 70-78 parts by weight of copper powder and 6-10 parts by weight of bonding glass powder for 6 hours, mixing the roller-milled mixed material with 15-22 parts by weight of an organic carrier / diamond powder mixture, and then stirring in a water bath at 60-80°C for 2-4 hours, wherein the average particle size of the copper powder is 3-5μm.

7. The method for preparing the high thermal conductivity diamond / copper composite conductive film material according to claim 1, characterized in that: In step three, the diamond / copper composite conductive slurry is coated on the surface of the ceramic substrate, including: using a screen with an aperture of 200 mesh to print the diamond / copper composite conductive slurry on the surface of the ceramic substrate, the ceramic substrate is made of an aluminum oxide material with a purity of not less than 99%, and the average surface roughness of the ceramic substrate is not greater than Ra0.

8.

8. The method for preparing the high thermal conductivity diamond / copper composite conductive film material according to claim 1, characterized in that: In step three, the ceramic substrate coated with the diamond / copper composite conductive slurry is subjected to vacuum leveling treatment, including: placing the ceramic substrate coated with the diamond / copper composite conductive slurry in a vacuum, heating it to 80-120° C., and keeping it warm for 10-50 minutes.

9. The method for preparing the high thermal conductivity diamond / copper composite conductive film material according to claim 1, characterized in that: In step three, the diamond / copper composite conductive slurry coated leveling component is placed in a protective atmosphere for degreasing and sintering treatment in sequence, including: placing the diamond / copper composite conductive slurry coated leveling component in a protective atmosphere, heating it to 500°C at a heating rate of 1-3°C / min and then keeping it warm for 2-5h, heating it to 700-900°C at a heating rate of 5-10°C / min and then keeping it warm for 0.5-2h.

10. A high thermal conductivity diamond / copper composite conductive film material, characterized in that: The high thermal conductivity diamond / copper composite conductive film material is prepared according to any one of the methods described in claims 1-9.

Citation Information

Patent Citations

  • Copper / graphene composite thin film material and preparation method and application thereof

    CN113481491A

  • Graphene composite copper thick film conductive slurry and preparation method thereof

    CN104021842A

  • Preparation method of high-shrinkage copper conductive film and material of high-shrinkage copper conductive film

    CN118136337A

  • Transparent conductive film, manufacturing method thereof, and solar cell / electroluminescence element using transparent conductive film

    JP2012056309A

  • Conductive paste composition

    JP2012226865A