Bimetallic oxide composite nitrogen-doped carbon nanocage and preparation method thereof

ZnO-Co3O4@N-C nanocages were synthesized by hydrothermal method and crystal seed growth method, which solved the problems of poor conductivity and volume expansion of lithium-ion battery anode materials, improved electrochemical performance and reduced preparation costs, and realized efficient lithium-ion batteries. Application of negative electrode materials.

CN118841540APending Publication Date: 2024-10-25BOZHOU SHANGDA ENG TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410838283.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

The poor conductivity and volume expansion effect of existing lithium-ion battery anode materials lead to structural instability and cannot meet the needs of high-energy-density batteries. Moreover, the preparation cost of two-component active metal oxides is high and the process is complex.

Method used

The MOFs material ZIF-8 was prepared by hydrothermal method, and the ZIF-67 shell was coated using the seed growth method to synthesize ZnO-Co3O4@N-C nanocage. The temperature and heating rate were controlled to retain the carbon and nitrogen elements in the organic ligands to form Nitrogen-doped carbon skeleton enables efficient preparation of bimetallic oxide composite materials.

Benefits of technology

It improves the electrochemical performance of the lithium-ion battery anode material, enhances the insertion and diffusion capabilities of lithium ions, buffers volume changes, improves the specific surface area and electrochemical lithium storage performance, and reduces the preparation cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118841540A_ABST
    Figure CN118841540A_ABST
Patent Text Reader

Abstract

The invention provides a bimetallic oxide composite nitrogen-doped carbon nanocage and a preparation method thereof. The special structure of the ZnO-Co3O4 (at) N-C nanocage has a relatively large specific surface area, and the existence of a nitrogen-doped carbon skeleton and mesopores is beneficial to buffering volume change in a lithium ion transfer process and is also beneficial to insertion and diffusion of lithium ions. In addition, the relatively high specific surface area of the ZnO-Co3O4 (at) N-C nanocage is beneficial to electron conduction and ion conduction, and a structural advantage is provided for excellent electrochemical lithium storage performance of the ZnO-Co3O4 (at) N-C nanocage. Besides, due to the synergistic effect of the bimetallic oxide, the framework of the nitrogen-doped carbon provides more active sites for lithium ion deintercalation and intercalation, so that the excellent electrochemical performance of the nitrogen-doped carbon is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new nano materials and electrochemical energy technology, and particularly to a bimetallic oxide composite nitrogen-doped carbon nanocage derived from a metal organic framework (MOFs) material and a preparation method thereof. Background Art

[0002] With the popularity of electronic devices such as electric vehicles and smart phones, lithium-ion batteries, as their core power source, have become the focus of scientific research and industry for performance improvement and cost reduction. Traditional lithium-ion battery negative electrode materials are mainly graphite, but their low theoretical capacity has gradually failed to meet the market demand for high energy density batteries.

[0003] Metal oxides, as a potential negative electrode material for lithium-ion batteries, have attracted widespread attention due to their low cost, natural abundance, and high theoretical specific capacity. However, metal oxides face two major challenges when used as negative electrode materials: first, poor conductivity, which limits the battery's charge and discharge performance at high rates; second, the volume expansion effect during the charge and discharge process, which leads to structural instability and rapid battery capacity decay.

[0004] In order to solve the above problems, researchers have proposed a variety of strategies, including synthesizing metal oxide nanostructures with special morphologies, preparing dual-component active metal oxides, and coating metal oxides with carbon layers or embedding transition metal oxides into ordered porous carbon. These methods have improved the electrochemical properties of metal oxides to a certain extent, but there are still problems such as high cost and complex preparation process.

[0005] As a new type of porous material, MOFs have uniform, continuous and permanent channels, as well as abundant active sites on specific surfaces. Its high specific surface area and pore size provide a suitable environment for lithium ion extraction and embedding, making it an ideal candidate for negative electrode materials for lithium ion batteries. In addition, the abundance of organic ligands in MOFs makes it very suitable as a carbon source for the synthesis of porous carbon, and the large amount of metal cations it contains is also conducive to the derivation of metal oxides with special morphology.

[0006] In recent years, researchers have begun to explore the use of MOFs to prepare lithium-ion battery anode materials with a bimetallic oxide structure. This structure not only combines the advantages of two metal oxides, but also further improves the electrochemical performance of the material through a synergistic effect. However, the current research on the application of MOFs in lithium-ion battery anode materials is still in its early stages. How to efficiently and economically prepare MOFs-based anode materials with a bimetallic oxide structure and promote their application in the field of electrochemical energy conversion is still an urgent problem to be solved. Summary of the invention

[0007] In order to solve the shortcomings of the prior art and improve the electrochemical energy conversion rate of the negative electrode material of lithium-ion batteries, the present invention provides a bimetallic oxide composite nitrogen-doped carbon nanocage and a preparation method thereof. The present invention utilizes the unique structure and characteristics of MOFs, prepares a typical MOFs material ZIF-8 by a hydrothermal method, and uses a seed growth method to coat the surface with a ZIF-67 shell to synthesize a ZIF-8@ZIF-67 core-shell composite structure, and then obtains a bimetallic oxide composite nitrogen-doped carbon nanocage, i.e., a ZnO-Co3O4@NC nanocage composite material, by heat treatment. In this process, the present invention controls the temperature and the heating rate to retain the carbon and nitrogen elements in the organic ligand to form a nitrogen-doped carbon skeleton, and develops an economical and efficient strategy to further promote the development and application of electrochemical energy conversion technology.

[0008] One aspect of the present invention is to provide a bimetallic oxide composite nitrogen-doped carbon nanocage and a preparation method thereof, the steps comprising:

[0009] Providing a ZIF-8;

[0010] ZIF-8 was reacted with cobalt salt (Co 2+ ) and 2-methylimidazole (2-MeIm) are mixed and reacted in a first reaction solvent to obtain ZIF-8@ZIF-67;

[0011] ZIF-8@ZIF-67 was heat treated to obtain a bimetallic oxide composite nitrogen-doped carbon nanocage, namely ZnO-Co3O4@NC.

[0012] In a preferred embodiment, the first reaction solvent includes one or more combinations of water, alcohol, ester, ether, and ketone.

[0013] In a preferred embodiment, the preparation method of ZIF-8 comprises the following steps:

[0014] The zinc salt (Zn 2+ ), polyvinyl pyrrolidone (PVP-K30), and 2-MeIm are mixed and reacted in a second reaction solvent to obtain ZIF-8.

[0015] In a preferred embodiment, the second reaction solvent includes one or more combinations of water, alcohol, ester, ether, and ketone.

[0016] In a preferred embodiment, the cobalt salt is an alcohol-soluble salt.

[0017] Preferably, the cobalt salt is provided in the form of an alcohol solution.

[0018] Preferably, the cobalt salt comprises one or more combinations of CoCl2, CoSO4, and Co(NO3)2.

[0019] Preferably, the zinc salt comprises one or more combinations of ZnCl2, ZnSO4, and Zn(NO3)2.

[0020] In a preferred embodiment, the ZIF-8 and cobalt salt (Co 2+ The reaction temperature of ) and 2-MeIm is 50-180°C, preferably 80-150°C, more preferably 100-120°C.

[0021] In a preferred embodiment, the ZIF-8 and cobalt salt (Co 2+ ) and 2-MeIm, the reaction pressure is 0.01-20 MPa, preferably 0.5-19 MPa, more preferably 1-18 MPa.

[0022] In a preferred embodiment, the ZIF-8 and cobalt salt (Co 2+ The reaction time of ) and 2-MeIm is 2-48h, preferably 5-36h, more preferably 8-24h.

[0023] In a preferred embodiment, the ZIF-8@ZIF-67 is cleaned and dried after preparation.

[0024] Preferably, the cleaning solvent includes one or more combinations of water, alcohol, ester, ether and ketone.

[0025] Preferably, the drying temperature is 30-120°C, preferably 50-100°C, more preferably 60-80°C.

[0026] Preferably, the drying time is 2-48 h, preferably 5-36 h, more preferably 12-24 h.

[0027] In a preferred embodiment, the heat treatment step includes calcination.

[0028] Preferably, the calcining step comprises:

[0029] The ZIF-8@ZIF-67 was heated for the first time under protective gas to obtain the intermediate product of ZIF-8@ZIF-67, namely, ZnO / Co / Co3O4@NC nanocages;

[0030] The ZIF-8@ZIF-67 intermediate product was heated for a second time under air to obtain a bimetallic oxide composite nitrogen-doped carbon nanocage, namely ZnO-Co3O4@NC.

[0031] Preferably, the protective gas includes one or more combinations of nitrogen, argon and helium.

[0032] Preferably, the ZIF-8@ZIF-67 is heated for the first time in a tube furnace.

[0033] Preferably, the temperature of the first heating is 200-800°C, preferably 300-700°C, more preferably 400-600°C.

[0034] Preferably, the heating rate of the first heating is 0.5-5°C / min, preferably 0.8-3°C / min, more preferably 1-2°C / min.

[0035] Preferably, the ZIF-8@ZIF-67 intermediate product is heated a second time in a muffle furnace.

[0036] Preferably, the temperature of the second heating is 200-800°C, preferably 300-700°C, more preferably 350-600°C.

[0037] Preferably, the heating rate of the second heating is 0.5-5°C / min, preferably 0.8-3°C / min, more preferably 1-2°C / min.

[0038] Another aspect of the present invention is to provide a bimetallic oxide composite nitrogen-doped carbon nanocage, namely ZnO-Co3O4@NC, which is obtained based on the preparation method of the present invention.

[0039] In a preferred embodiment, the crystal structure of the ZnO-Co3O4@NC is a regular dodecahedral nanocage.

[0040] In this application specification, "@" means that one material is coated by another material to protect the core material from the external environment, or to control the release of the core material. In MOFs materials, this encapsulation is used to improve the porosity, stability or other physical and chemical properties of the material. In the context of ZIF-8@ZIF-67, "@" means that ZIF-67 is coated by ZIF-8, with ZIF-67 as the core and ZIF-8 as the shell.

[0041] In the present application, "ZIF" refers to a porous crystalline material with a three-dimensional pore structure formed by self-assembly of metal ions (such as Zn2+, Co2+, etc.) and imidazole or its derivatives (such as 2-methylimidazole).

[0042] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0043] The present invention provides a bimetallic oxide composite nitrogen-doped carbon nanocage, namely, ZnO-Co3O4@NC nanocage composite material, and a preparation method thereof. The special structure of the ZnO-Co3O4@NC nanocage of the present invention has a large specific surface area, and the presence of the nitrogen-doped carbon skeleton and mesopores is beneficial to buffering the volume change during lithium ion transfer, and is also beneficial to the insertion and diffusion of lithium ions. In addition, the higher specific surface area of ​​the present invention is beneficial to electronic conduction and ion conduction, providing a structural advantage for the excellent electrochemical lithium storage performance of the ZnO-Co3O4@NC nanocage. In addition, the synergistic effect of the bimetallic oxide of the present invention enables the nitrogen-doped carbon skeleton to provide more active sites for lithium ion extraction and embedding, thereby improving its excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 SEM images of (a) ZIF-8, (b) ZIF-8@ZIF-67 obtained by the implementation of the present invention; (c) TEM image of ZIF-8@ZIF-67; (d) XRD diffraction patterns of ZIF-8, ZIF-67 and ZIF-8@ZIF-67; (e) photos of ZIF-8, (f) ZIF-8@ZIF-67 and (g) ZIF-67 samples.

[0045] Figure 2 This is the XRD diffraction pattern of ZnO / Co / Co3O4@NC obtained by implementing the present invention.

[0046] Figure 3 (a, b) SEM images of ZnO / Co / Co3O4@NC obtained by implementing the present invention; (c, d) TEM images of ZnO / Co / Co3O4@NC.

[0047] Figure 4 XRD diffraction patterns of ZnO@NC, Co3O4@NC and ZnO-Co3O4@NC nanocages obtained by implementing the present invention.

[0048] Figure 5 (a) SEM image, (b, c, f) TEM images, (d) HRTEM image, (e) electron diffraction analysis, and (gk) elemental mapping analysis of the ZnO-Co3O4@NC nanocages obtained for the present invention.

[0049] Figure 6 X-ray energy spectrum analysis of the ZnO-Co3O4@NC nanocage obtained by the implementation of the present invention: (a) full spectrum; high-resolution spectrum (b) Zn 2p, (c) Co 2p, (d) C 1s, (e) N 1s, (f) O 1s.

[0050] Figure 7(a) Nitrogen adsorption-desorption curve and (b) pore size distribution curve of ZnO-Co3O4@NC nanocage obtained by implementing the present invention.

[0051] Figure 8 (a) Cyclic voltammetry curve of ZnO / Co / Co3O4@NC obtained by the implementation of the present invention in the voltage range of 0.01-3V at a scan rate of 0.5mV / s, and (b) charge-discharge curves of 1, 2, 10 and 100 cycles.

[0052] Fig. 9 The cycling performance of ZnO / Co / Co3O4@NC obtained in the present invention at 0.1 A / g.

[0053] Fig.10 Cyclic voltammetry curves of (a) ZnO@NC, (c) Co3O4@NC, and (e) ZnO-Co3O4@NC in the voltage range of 0.01-3 V at a scan rate of 0.5 mV / s. Charge-discharge curves of (b) ZnO@NC, (d) Co3O4@NC, and (f) ZnO-Co3O4@NC after 1, 2, 10, and 100 cycles.

[0054] Fig.11 (a) Cycling performance of ZnO-Co3O4@NC nanocages obtained by implementing the present invention at a current density of 0.1 A / g, (b) rate performance, (c) Cycling performance of ZnO@NC, Co3O4@NC, and ZnO-Co3O4@NC nanocages at a current density of 0.1 A / g, (d) AC impedance spectra of ZnO@NC, Co3O4@NC, and ZnO-Co3O4@NC nanocages. DETAILED DESCRIPTION

[0055] The present invention provides a bimetallic oxide composite nitrogen-doped carbon nanocage and a preparation method thereof. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0056] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged under appropriate circumstances. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0057] Example

[0058] (1) Synthesis of ZIF-8: 3.24 g of Zn(NO3)2·6H2O and 0.80 g of polyvinyl pyrrolidone (PVP-K30) were added to 160 ml of methanol solution and magnetically stirred for 5 minutes to obtain a mixed solution. Then, 2.104 g of 2-MeIm was added to the above solution, and after ultrasonic treatment for 10 minutes, the resulting mixed solution was magnetically stirred at room temperature for 24 hours. Subsequently, the product was collected by centrifugation and washed several times with methanol. The precipitate was dried at 60°C for 12 hours to obtain a sample.

[0059] (2) Synthesis of ZIF-8@ZIF-67: 0.16 g of ZIF-8 was added to 20 ml of methanol solution and ultrasonicated for 30 min to obtain solution A. At the same time, 0.354 g of CoCl2·6H2O was dissolved in 6 ml of methanol solution to obtain solution B, and 1.79 g of 2-MeIm was added to 6 ml of methanol solution to obtain solution C. Solutions B and C were added to solution A at the same time. The mixed solution was stirred for 5 min, then transferred to an autoclave and heated to 100 °C for 24 h. After naturally cooling to room temperature, the resulting precipitate was collected by centrifugation and washed three times with methanol. Finally, the precipitate was dried at 60 °C for 12 h to obtain the sample.

[0060] (3) Synthesis of ZnO-Co3O4@NC dodecahedral nanocages: The ZIF-8@ZIF-67 core-shell structure was calcined in a tube furnace at 600°C in N2 atmosphere at a heating rate of 1°C / min to obtain ZnO / Co / Co3O4@NC nanocages. ZnO-Co3O4@NC dodecahedral nanocages were prepared by further calcining ZnO / Co / Co3O4@NC at 350°C in air in a muffle furnace at a heating rate of 1°C / min. The calcined samples were collected as the final product. As a comparative experiment, ZIF-8 and ZIF-67 nanocrystals were annealed under the same two-step calcination conditions to obtain ZnO@NC and Co3O4@NC nanocages, respectively.

[0061] Figure 1 Field emission scanning electron microscope (SEM) images of ZIF-8 (Fig. a) and ZIF-8@ZIF-67 (Fig. b), transmission electron microscope (TEM) images of ZIF-8@ZIF-67 (Fig. c), XRD diffraction patterns of ZIF-8, ZIF-67 and ZIF-8@ZIF-67 (Fig. d), and ordinary camera photos of ZIF-8, ZIF-67 and ZIF-8@ZIF-67 samples are shown. It can be seen that the obtained ZIF-8@ZIF-67 powder is composed of dispersed rhombic regular dodecahedral crystals with a size of about 1μm, as shown in Fig. b. Compared with ZIF-8, it is found that ZIF-8@ZIF-67 has a similar morphology to ZIF-8 because they have the same topological structure and the ZIF-67 shell is only a few nanometers. Fig. c further proves that the ZIF-8@ZIF-67 core-shell structure presents a hexagonal structure. Figure d shows the XRD diffraction patterns of ZIF-8, ZIF-67 and ZIF-8@ZIF-67. It was found that ZIF-8@ZIF-67 matches well with ZIF-8 and ZIF-67, with similar unit cells and lattices. Figure e g shows that ZIF-8 is white, ZIF-67 is purple, and the color of the obtained ZIF-8@ZIF-67 is between ZIF-8 and ZIF-67. From the above analysis, it can be seen that the obtained product is a core-shell structure of ZIF-8@ZIF-67, indicating the successful synthesis of the ZIF-8@ZIF-67 precursor.

[0062] Figure 2 As shown, the crystal phase of the sample ZnO / Co / Co3O4@NC after one-step calcination was characterized by powder XRD. The XRD diffraction pattern has obvious diffraction peaks at 2θ=34.4° and 36.3°, corresponding to the (002) and (101) crystal planes in ZnO (JCPDS: 36-1451), respectively. The diffraction peaks at 2θ=43.5° and 44.8° correspond to the (111) and (200) crystal planes in Co (JCPDS: 15-0806). In addition, the obvious diffraction peak at 50.8° matches Co3O4 (JCPDS: 42-1467). The crystal phase of ZIF-8@ZIF-67 changes significantly after one-step calcination. This is because the oxidation temperature of Zn is low and it is completely converted into ZnO during the calcination process. The oxidation temperature of Co is high, and Co is completely converted into ZnO under nitrogen protection. 2+ The elemental Co is reduced to form elemental Co, while part of the elemental Co is oxidized to Co3O4. Thus, a ZnO / Co / Co3O4@NC nanocage composite material is formed, which makes it possible to completely oxidize in the air in the second step to form a bimetallic oxide composite material.

[0063] Figure 3The morphological characterization of ZnO / Co / Co3O4@NC composites formed after ZIF-8@ZIF-67 was carbonized under N2 protection in one step is shown. Figure a is a SEM image of the ZnO / Co / Co3O4@NC sample. It can be clearly seen from the figure that the sample size is uniform and its average size is about 800nm, and the sample can be observed to have sharp edges and complete morphology. Figure b is an SEM image at different magnifications. It can be observed that the surface of the ZnO / Co / Co3O4@NC sample is rough compared with ZIF-8@ZIF-67, and the structure of the regular dodecahedron still exists. Figures c and d are TEM images of the ZnO / Co / Co3O4@NC composite at different magnifications. It can be seen that: a clear hollow structure is displayed outside the hexagonal carbon nanocage, and the grooves on the edges of the hexagons are clearly observed in the TEM image, which is caused by volume shrinkage during annealing. Figure d clearly shows that the ZnO / Co / Co3O4@NC sample obtained by carbonizing ZIF-8@ZIF-67 at 600℃ for 2 hours in N2 atmosphere retains the outline and size of the original morphology, and the structure remains intact.

[0064] Figure 4It is shown that ZIF-8, ZIF-67 and ZIF-8@ZIF-67 form ZnO@NC, Co3O4@NC and ZnO-Co3O4@NC nanocages respectively after two-step calcination. There are obvious diffraction peaks at 2θ=31.8°, 34.4°, 36.3°, 47.5°, 56.6°, 62.9°, 68.0°, 69.1° and 77.0°, corresponding to the (100), (002), (101), (102), (110), (103), (112), (201) and (202) crystal planes of ZnO (JCPDS: 36-1451), and the lattice constant is a=b=3.249. The diffraction peaks of the XRD diffraction pattern at 2θ=19.0°, 31.3°, 36.9°, 38.5°, 44.8°, 55.7°, 59.4° and 65.2° correspond to the (111), (220), (311), (222), (400), (422), (511) and (440) crystal planes in Co3O4 (JCPDS: 42-1467), and the lattice constant is a=b=c=8.084. In addition, the diffraction peaks corresponding to the (311) crystal plane of Co3O4 and the (101) crystal plane of ZnO are very close, and the two peaks overlap and are not easy to distinguish. The spinel phase ZnCo2O4 is isostructural with Co3O4, and it is difficult to distinguish the ZnCo2O4 and Co3O4 phases by XRD patterns. According to the XRD spectrum, it can be seen that the sample has the same crystal phase as ZnO and Co3O4 after one-step calcination, Co is completely oxidized to Co3O4, and the peak positions of pure ZIF-8, ZIF-67-derived ZnO and Co3O4 are consistent with those of ZIF-8@ZIF-67-derived ZnO / Co3O4 composite materials. The diffraction peaks of the samples have high intensity and no other impurity peaks, indicating that the samples have high crystallinity. From the above analysis, it can be preliminarily believed that ZIF-8@ZIF-67 successfully synthesized the ZnO-Co3O4@NC composite material after two-step calcination.

[0065] Figure 5(a) SEM image, (b, c, f) TEM image, (d) HRTEM image, (e) electron diffraction analysis, and (gk) element mapping analysis of the ZnO-Co3O4@NC nanocage obtained by the implementation of the present invention. In Figure a, it can be clearly seen that the surface of the regular dodecahedron is very rough and is composed of dense nanoparticles. At the same time, it can be observed that the regular dodecahedron skeleton of ZnO-Co3O4@NC is very similar to ZnO / Co / Co3O4@NC and maintains the original morphology. Figures b and c are TEM images of ZnO-Co3O4@NC nanocages, and the hollow structure of ZnO-Co3O4@NC nanocages can be observed through the TEM images. There is a sharp color contrast between the shell and the inner cavity of the ZnO-Co3O4@NC nanocage. At the same time, the highly symmetrical regular dodecahedron shell framework can be clearly observed, indicating that the nitrogen-doped carbon skeleton of the regular dodecahedron is well retained, and the mesoporous structure formed by the uniform distribution of nanoparticles in the shell can be seen. The porous hollow ZnO-Co3O4@NC nanocage can also maintain its structural integrity after the second oxidation step, and retains a complete nitrogen-doped carbon skeleton. Figure d shows the high-magnification transmission electron microscopy (HRTEM) of the ZnO-Co3O4@NC nanocage. The lattice spacing of 0.467 and 0.247nm was analyzed from the HRTEM image, which corresponds to the (111) crystal plane of Co3O4 and the (101) crystal plane of ZnO, respectively. The regional electron diffraction pattern is shown in Figure e, indicating that the ZnO-Co3O4@NC regular dodecahedral nanocage is polycrystalline, and its diffraction rings match the (111), (220), (400) crystal planes of Co3O4 and the (101), (110), (103) crystal planes of ZnO, which is consistent with the XRD diffraction results. In addition, in order to clearly observe the element distribution of ZnO-Co3O4@NC nanocages, elemental analysis was performed through the white frame area of ​​the TEM dark field image (Figure f). The results show that elements including Zn, Co and O are evenly distributed in the product. However, the content of C and N elements is relatively low because the content of C and N elements in the ZIF-8@ZIF-67 precursor is low and part of them is lost during the oxidation process. The above analysis shows that the ZnO-Co3O4@NC formed after the second step of oxidation well maintains the complete structure of the regular dodecahedral nanocage, and also proves that the nitrogen-doped carbon skeleton is well maintained, further indicating that the ZnO-Co3O4@NC regular dodecahedral nanocage was successfully prepared after two-step calcination.

[0066] Figure 6a is the full XPS spectrum of ZnO-Co3O4@NC nanocage, which confirms the presence of Zn, Co, O, C and N elements. Figures bf analyze the high-resolution XPS of Zn, Co, C, N, etc. The high-resolution XPS spectrum of Zn2p shown in Figure b shows two obvious peaks at 1022.0 and 1045.2eV, which can be assigned to Zn2p3 / 2 and Zn2p1 / 2 respectively. The results show that the Zn in the component has been converted into ZnO. For Co2p, the peak of Co2p3 / 2 at 780eV and the peak of Co 2p1 / 2 at 795eV are fitted and decomposed into four peaks, whose binding energies are equivalent to 779.4, 780.0, 794.3 and 795.5eV respectively (Figure c), proving that Co ions exist in two valence states of +2 and +3. After fitting, C1s (Figure d) corresponds to CC at 284.5eV, CO at 286.2eV, and C=O at 288.5eV. The N1s spectrum has two peaks at 398.8 and 400.5eV, corresponding to pyridine and pyrrole nitrogen, respectively (Figure e). The results confirm that the carbon framework in the ZnO-Co3O4@NC nanocage is successfully doped with nitrogen. The O1s spectrum (Figure f) shows two bonding characteristics. The peak at 529.1eV binding energy is a typical peak position of metal-oxygen bond, while the peak at 531.4eV is usually associated with defects, chemically adsorbed oxygen or under-coordinated lattice oxygen. According to XPS analysis, the peak area is proportional to its molar content through peak area calculation. The molar ratio of Zn to Co is calculated to be 3.87, indicating that the molar ratio of ZnO to Co3O4 is 11.61, and the molar contents of C and N are 25.14% and 3.66%, respectively. The above analysis confirmed the presence of ZnO, Co3O4, C, and N in the final sample, which once again confirmed the successful synthesis of ZnO-Co3O4@NC nanocage composite materials.

[0067] Figure 7 The (a) nitrogen adsorption-desorption curve and (b) pore size distribution curve of ZnO-Co3O4@NC nanocage are presented. By analyzing the nitrogen adsorption-desorption curve of ZnO-Co3O4@NC nanocage, the Brunauer-Emmett-Teller (BET) surface area and pore size distribution are obtained. It can be seen that the sample exhibits typical IV-type characteristics. The adsorption and desorption curves do not overlap at 0.4-1.0P / P0, and belong to the H3-type hysteresis loop. This adsorption-desorption curve is usually seen in the structure of slit pores, indicating that the prepared ZnO-Co3O4@NC nanocage has a macroporous or microporous structure with a pore range of 2-42nm and an average pore size of 10.9nm (Figure b). According to BJH theoretical calculations, the BET specific surface area of ​​ZnO-Co3O4@NC nanocage is calculated to be 65.9m 2 g -1 , the pore volume is 0.217 cm 3 g-1 .

[0068] Figure 8 The cyclic voltammetry (CV) and constant current charge-discharge curves of ZnO / Co / Co3O4@NC are shown. Figure a shows the first three cyclic voltammetry tests of ZnO / Co / Co3O4@NC nanocages under the conditions of a test voltage range of 0.01-3V and a scan rate of 0.1mV / s. During the discharge process, a reduction reaction occurred at the electrode, and the reduction peak around 1.53V corresponds to Zn 2+ Reduced to Zn element, in the subsequent cycle process, 1.44V and 2.14V correspond to the oxidation peaks of Zn and Co, respectively, and the reduction peak of about 0.7V corresponds to the irreversible reduction of the electrolyte and the formation of the solid electrolyte intermediate phase SEI film. After the first cycle, the CV curve showed good repeatability, indicating that ZnO / Co / Co3O4@NC has good reversibility during the charge and discharge cycle. Figure b is the constant current charge and discharge curve of ZnO / Co / Co3O4@NC nanocage in the voltage range of 0.01-3.0V and the current density of 0.1A / g for 1, 2, 10, and 100 times. It can be seen that the ZnO / Co / Co3O4@NC nanocage shows good stability during the cycle, and still maintains a discharge capacity of 807mAh / g after 100 cycles, indicating that the ZnO / Co / Co3O4@NC nanocage has good electrochemical performance.

[0069] Fig. 9 The constant current cycling performance curves of ZnO / Co / Co3O4@NC at a current density of 0.1A / g are listed in detail. The ZnO / Co / Co3O4@NC electrode shows excellent cycling stability. Although the first coulombic efficiency is only 56.4%, the capacity decays during the cycle, but then gradually stabilizes. After 100 constant current cycles at a current density of 0.1A / g, the specific capacity can be stabilized at 807mAh / g, and the coulombic efficiency is as high as 98.7%. Analysis shows that the attenuation of reversible capacity is mainly caused by the decomposition of the electrolyte and the formation of the SEI film. In the ZnO / Co / Co3O4@NC electrode, ZnO and Co3O4 provide the main theoretical capacity, but due to the presence of some elemental cobalt, its electrochemical performance is not optimal. At the same time, the incomplete oxidation makes its mesoporous structure unclear, and it cannot provide more channels for lithium ion transfer during the cycle. Therefore, the cycling performance of the ZnO / Co / Co3O4@NC electrode is good, but there is still room for improvement. This is the significance of the second step oxidation and provides a good foundation for the excellent electrochemical performance after complete oxidation.

[0070] Fig.10a shows the CV curves of the first three cycles of the ZnO@NC electrode. It can be seen that the oxidation peak around 1.0 V during the first charge corresponds to the Zn 0 Oxidation to Zn 2+ . Figure 6 c It can be seen that the first three cycle CV curves of the Co3O4@NC electrode show that the broad reduction peak near 0.72 V in the first discharge process is attributed to the irreversible reduction of the electrolyte and the formation of the SEI film at the solid electrolyte interface. The oxidation peak around 2.19 V during the charge process corresponds to the Co 0 Figure e shows the first three consecutive CV curves of the ZnO-Co3O4@NC sample. It can be clearly seen that the weak reduction peak observed at 0.9 V is related to the reduction of Co3+ to Co2+, while the other peak below 0.3 V is related to the reduction of Co 2+ The reduction of ZnO to Co0 and the formation of Li2O also indicate the irreversible reduction of electrolyte and the formation of solid electrolyte interphase SEI film. In addition, the reduction peak around 1.3V in the first discharge process corresponds to the Zn 2+ Reduction to Zn 0 In the subsequent charging process, the oxidation peaks at 1.73 V and 2.16 V correspond to Zn0 and Co, respectively. 0 Oxidation reaction. It is worth noting that Figure e clearly shows that the oxidation and reduction peaks in the CV curve of ZnO-Co3O4@NC maintain their original peak positions and shapes during subsequent cycles, almost overlapping with the first cycle, especially compared with the ZnO@NC and Co3O4@NC samples, which means that ZnO-Co3O4@NC has the most excellent stability and reversibility after the first cycle. Figures b, d and f show the constant current charge and discharge curves of ZnO@NC, Co3O4@NC and ZnO-Co3O4@NC samples at a current density of 0.1A / g for 1, 2, 10 and 100 times. The results show intuitively that the stability of ZnO@NC and Co3O4@NC during the cycle is poor, and only remains at 610mAh / g and 746mAh / g after 100 charge and discharge cycles. The ZnO-Co3O4@NC nanocage derived from the composite maintained a high discharge specific capacity of 1102 mAh / g after 100 cycles. The results once again proved the significance of using ZIF-8 and ZIF-67 composites to provide Zn and Co sources respectively. It has higher and better electrochemical performance than pure ZnO and Co3O4, reflecting the advantages of designed materials.

[0071] Fig.11a lists in detail the constant current cycling performance curves of ZnO-Co3O4@NC at a current density of 0.1A / g and the changes in coulombic efficiency (CE) during the cycling process. When ZnO-Co3O4@NC is used as an anode material, the discharge capacity can still be maintained at about 1305mAh / g after 300 cycles, and it has a high coulombic efficiency of about 98% after the first few cycles. The first charge and discharge capacity is about 1495 and 2373mAh / g, and the first coulombic efficiency is 62.9%. The initial irreversible capacity loss is usually caused by the formation of SEI film and the decomposition of electrolyte. It can be seen from the figure that the charge and discharge capacity decays rapidly during the first 60 cycles, which may be caused by the presence of irreversible substances. However, it can be clearly observed that the specific capacity shows an upward trend during the subsequent cycles. Figure b clearly shows the rate performance of the ZnO-Co3O4@NC electrode, with discharge specific capacities of 1458, 1398, 1165, 1056, 880 and 716 mAh / g at 0.1, 0.2, 0.5, 1, 2 and 5 A / g, respectively. When the current density returns to 0.1 A / g, ZnO-Co3O4@NC is still able to recover to a discharge specific capacity of 1460 mAh / g. When the current density increases from the initial 0.1 A / g to 1 A / g, the discharge specific capacity remains stable at about 72% of the original value. In addition, when the current density returns to the original 0.1 A / g, the cycle remains stable and the specific capacity increases slightly after several cycles, which may be due to the reduced impedance of the anode material after high current density discharge. Among them, ZnO@NC and Co3O4@NC are compared with ZnO-Co3O4@NC, as shown in Figure c. The results show that compared with ZnO@NC and Co3O4@NC samples, the ZnO-Co3O4@NC sample maintains a higher capacity of 1179mAh / g after 200 charge and discharge cycles, while the discharge specific capacities of ZnO@NC and Co3O4@NC samples are only 610mAh / g and 746mAh / g respectively after 100 cycles. ZnO-Co3O4@NC nanocages show significant advantages in capacity retention and stability in long-term cycles.

[0072] In summary, the special structure of the ZnO-Co3O4@NC nanocage in the embodiment of the present invention enables it to have a large specific surface area. The presence of the nitrogen-doped carbon skeleton and mesopores is beneficial to buffering the volume change during lithium ion transfer, and is also beneficial to the insertion and diffusion of lithium ions. The higher specific surface area is beneficial to electronic conduction and ion conduction, providing a structural advantage for the excellent electrochemical lithium storage performance of the ZnO-Co3O4@NC nanocage. The synergistic effect of the bimetallic oxide and the nitrogen-doped carbon skeleton provide more active sites for the extraction and insertion of lithium ions, thereby improving its excellent electrochemical performance.

[0073] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.

Claims

1. A method for preparing bimetallic oxide composite nitrogen-doped carbon nanocages, It is characterized in that the steps include: Providing a ZIF-8; The ZIF-8 is mixed with cobalt salt and 2-MeIm in a first reaction solvent and reacted to obtain ZIF-8@ZIF-67; the ZIF-8@ZIF-67 is heat-treated to obtain a bimetallic oxide composite nitrogen-doped carbon nanocage, i.e., ZnO-Co 3 O 4 @NC.

2. The preparation method according to claim 1, It is characterized in that The preparation method of ZIF-8 comprises the following steps: Zinc salt, polyvinyl pyrrolidone and 2-MeIm are mixed and reacted in a second reaction solvent to obtain ZIF-8.

3. The preparation method according to claim 1, It is characterized in that The cobalt salt includes CoCl 2 、CoSO 4 、Co(NO 3 ) 2 One or more combinations of .

4. The preparation method according to claim 1, It is characterized in that The reaction temperature of ZIF-8, cobalt salt and 2-MeIm is 50-180°C, preferably 80-150°C, and more preferably 100-120°C.

5. The preparation method according to claim 1, It is characterized in that The reaction pressure of the ZIF-8, cobalt salt and 2-MeIm is 0.01-20 MPa, preferably 0.5-19 MPa, and more preferably 1-18 MPa.

6. The preparation method according to claim 1, It is characterized in that The heat treatment step includes calcining; the calcining step includes: The ZIF-8@ZIF-67 was heated for the first time under protective gas to obtain the intermediate product of ZIF-8@ZIF-67, namely ZnO / Co / Co 3 O 4 @NC nanocage; The ZIF-8@ZIF-67 intermediate product was heated for the second time under air to obtain a double metal oxide composite nitrogen-doped carbon nanocage, namely ZnO-Co 3 O 4 @NC.

7. The preparation method according to claim 6, It is characterized in that The ZIF-8@ZIF-67 is subjected to the first heating in a tube furnace; and / or The temperature of the first heating is 200-800° C., preferably 300-700° C., more preferably 400-600° C.; and / or The heating rate of the first heating is 0.5-5°C / min, preferably 0.8-3°C / min, more preferably 1-2°C / min.

8. The preparation method according to claim 6, It is characterized in that Heating the ZIF-8@ZIF-67 intermediate product a second time in a muffle furnace; and / or The temperature of the second heating is 200-800°C, preferably 300-700°C, more preferably 350-600°C; and / or The heating rate of the second heating is 0.5-5°C / min, preferably 0.8-3°C / min, more preferably 1-2°C / min.

9. A double metal oxide composite nitrogen-doped carbon nanocage, namely ZnO-Co 3 O 4 @NC, It is characterized in that Obtained based on the preparation method according to any one of claims 1 to 8.

10. The ZnO-Co according to claim 9 3 O 4 @NC, It is characterized in that The ZnO-Co 3 O 4 The crystal structure of @NC is a regular dodecahedral nanocage.

Citation Information

Cited By

  • Preparation method of bimetallic nanoparticles and application of bimetallic nanoparticles in lithium-sulfur battery

    CN119858920A