Positive electrode slurry, preparation method thereof and positive plate

By using additives such as polyacrylic acid and lithium silicate in the positive electrode slurry, the solubility and dispersion of the binder are improved, the problem of poor flexibility of the electrode sheet is solved, the adhesion and stability of the electrode sheet are improved, and the production costs.

CN118841571APending Publication Date: 2024-10-25ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410766401.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Excessive use of existing cathode binders results in poor flexibility of lithium-ion battery electrode sheets, which are prone to falling powder and breakage, affecting the stability and energy density of the battery.

Method used

Polyacrylic acid is used as the binder, and lithium silicate and copolymers with phosphate groups, ether bonds and ester groups are used as additives to improve the solubility and dispersion of the binder through hydrogen bonds and other interaction forces. Increase the flexibility and adhesion of the pole pieces.

Benefits of technology

It effectively reduces the amount of binder, improves the flexibility and bonding force of the electrode piece, improves the stability and processing performance of the electrode piece, reduces production costs, and avoids the gel-like and high viscosity problems of the slurry. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004892636920000021
    Figure BDA0004892636920000021
  • Figure BDA0004892636920000141
    Figure BDA0004892636920000141
  • Figure BDA0004892636920000151
    Figure BDA0004892636920000151
Patent Text Reader

Abstract

The invention provides a positive electrode slurry and a preparation method thereof, and a positive plate, the positive electrode slurry comprises a positive electrode active material, a binder, a conductive agent and an additive, the binder comprises at least one of a first additive and a second additive, the first additive is lithium silicate, and the second additive is lithium silicate. The second additive is a copolymer with a phosphate group, an ether bond and an ester group. Compared with the prior art, the polyacrylic acid is used as the binder and is matched with the positive electrode material lithium iron phosphate and the additive, so that the dispersity in the slurry can be improved, the slurry does not generate gel and is good in dispersity, and meanwhile, the prepared positive plate is good in flexibility and conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of secondary batteries, and in particular to a positive electrode slurry and a preparation method thereof, and a positive electrode sheet. Background Art

[0002] As an inactive component in lithium-ion battery electrode sheets, binder is one of the important materials that must be used in the preparation of lithium-ion battery electrode sheets. The main function of the binder is to connect the electrode active material, the conductive agent and the electrode current collector so that they have overall connectivity, thereby reducing the impedance of the electrode and better stabilizing the electrode sheet structure. At present, the general positive electrode binder (PVDF) is added in large amounts, which affects the overall energy density of the battery. When using some highly adhesive modified PVDF, the slurry is often unstable, resulting in agglomeration between materials, and the slurry shows high viscosity, gel-like, and poor fluidity, which is not conducive to subsequent coating and drying processes. The produced electrode sheets are harder and more brittle, and the electrode sheets are not flexible. They are prone to powder loss and breakage during winding and bending, resulting in short circuits and other defects.

[0003] Therefore, it is necessary to provide a method for improving the quality rate of the electrode by improving the positive electrode binder. Summary of the invention

[0004] One of the purposes of the present invention is to provide a positive electrode slurry to address the deficiencies of the prior art, reduce the amount of binder used, and at the same time improve the bonding strength of the electrode piece, thereby improving the problem of easy powder loss and poor flexibility of the electrode piece.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A positive electrode slurry comprises a positive electrode active material, a binder, a conductive agent and an additive, wherein the binder comprises polyacrylic acid, and the additive comprises at least one of a first additive and a second additive, wherein the first additive is lithium silicate, and the second additive is a copolymer with a phosphoric acid group, an ether bond and an ester group.

[0007] Preferably, the structural formula of the second additive is as follows:

[0008]

[0009] Preferably, the number of ether group segments and ester group segment segments in the second additive is 15 to 25, and the molecular weight of the second additive is 6,000 to 10,000.

[0010] Preferably, the mass fraction of the first additive in the positive electrode slurry is 0.01-0.5%, and the mass fraction of the second additive in the positive electrode slurry is 0.01-0.3%.

[0011] Preferably, the preparation method of the second additive comprises the following steps:

[0012] A1. Under anhydrous and oxygen-free conditions, dissolve 1,12-dodecanediol in an organic solvent, add a strong base, and stir in an ice bath for 20 to 40 minutes; dissolve dodecanedioic acid in an organic solvent, add it at 0°C, and react at 90 to 100°C for 22 to 26 hours; add toluene, a white substance precipitates, filter, wash, and dry to obtain compound A;

[0013] A2. Under anhydrous and oxygen-free conditions, dissolve 1,12-dodecanediol in an organic solvent, add a strong base, and stir in an ice bath for 20 to 40 minutes; dissolve 1,12-dibromododecane in an organic solvent, add slowly at 0°C, and stir at room temperature for 1 to 3 hours after all the addition; add toluene, a white substance precipitates, filter, wash, and dry to obtain compound B;

[0014] A3. Under anhydrous and oxygen-free conditions, add an organic solvent to n-hexadecyl phosphoric acid, add a strong base, and stir in an ice bath for 20 to 40 minutes; dissolve compound B in an organic solvent, add slowly at 0°C, and stir at room temperature for 2 to 4 hours after all are added; dissolve compound A in an organic solvent, add slowly at 0°C, and stir at room temperature for 2 to 4 hours; after the reaction is completed, add methanol, and react at 60 to 100°C for 22 to 24 hours. Solution C is obtained;

[0015] A4. At 0°C, acetic acid was added to solution C until it became weakly acidic, and toluene was added to cause white matter to precipitate. The matter was filtered, washed, dried, and recrystallized to obtain a second additive.

[0016] Preferably, the positive electrode active material includes at least one of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, lithium nickel cobalt manganese oxide and lithium nickel cobalt aluminum oxide; and the particle size Dv50 of the positive electrode active material is 0.5 to 1.0 μm.

[0017] Preferably, the conductive agent includes at least one of conductive carbon black, graphene and carbon nanotubes.

[0018] Preferably, the weight content ratio of the positive electrode active material, the binder, the conductive agent and the additive is (93-97wt%): (1-3wt%): (1.88-5%wt%): (0.02-0.8wt%).

[0019] The second object of the present invention is to provide a method for preparing a positive electrode slurry, the preparation steps comprising:

[0020] 1) Add the binder to the solvent and stir evenly;

[0021] 2) Adding a conductive agent and an additive to the solution in step 1) in sequence and stirring evenly;

[0022] 3) First, add 50-70 wt% of the positive electrode active material to the solution stirred evenly in step 2), stir evenly, then add the remaining 30-50 wt% of the positive electrode active material, stir evenly, and obtain the positive electrode slurry.

[0023] The third object of the present invention is to provide a positive electrode sheet, comprising a current collector and a positive electrode slurry layer coated on at least one surface of the current collector, wherein the positive electrode slurry layer comprises the positive electrode slurry described in any one of the above items.

[0024] Compared with the prior art, the beneficial effects of the present invention are as follows: the positive electrode slurry provided by the present invention adopts polyacrylic acid as a binder, and is matched with the first additive and the second additive. The silicate in the lithium silicate in the first additive is easily combined with polyacrylic acid through hydrogen bonds, thereby increasing the solubility of lithium silicate. The polyacrylic acid is indirectly connected through the hydrogen bonds formed with the silicate, thereby alleviating the rigidity between the molecules, thereby increasing the flexibility of the pole piece; the second additive contains a phosphate group, an ether bond, and an ester group, and the above groups can generate hydrogen bonds with the carboxyl group, which can be adsorbed on the surface of the positive electrode active material and dispersed in the glue, and at the same time play the role of a dispersant and a softener. Among them, the ether bond is conducive to the extension of the chain segment and increases the flexibility; the intermolecular force of the ester group is strong, the crystallinity is good, which is conducive to the improvement of the bonding property and improves the cracking of the pole piece during coating; the carbon chain connected between the ether bond and the ester group is selected to be longer than 10 to 14 carbon atoms, which can make the additive molecule stretch, improve the stability of the slurry, and effectively improve the powdering, cracking and flexibility of the pole piece in the subsequent coating and drying processes. DETAILED DESCRIPTION

[0025] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be further described in detail below in conjunction with specific implementation methods, but the implementation methods of the present invention are not limited thereto.

[0026] The terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0027] According to the first aspect of the present application, the present application provides a positive electrode slurry, including a positive electrode active material, a binder, a conductive agent and an additive, wherein the binder includes polyacrylic acid, and the additive includes at least one of a first additive and a second additive, wherein the first additive is lithium silicate, and the second additive is a copolymer with a phosphate group, an ether bond and an ester group. Among them, the binder is polyacrylic acid (PAA), which contains a large number of carboxyl groups, can produce more hydrogen bonds, has good adhesion, has a high degree of anchoring to the positive electrode active material particles, and has a stronger cohesive force on the prepared pole piece. At the same time, PAA does not contain fluorine, so HF will not be removed, and the slurry will not produce gel, thereby affecting the slurry. However, the excessive hydrogen bonds contained in PAA result in greater rigidity of the PAA chain, which will make the pole piece brittle and poor in flexibility.

[0028] The silicate in the first additive lithium silicate is easily combined with PAA through hydrogen bonds, increasing the solubility of lithium silicate. PAA is indirectly connected through the hydrogen bonds formed between the silicate, which alleviates the rigidity between the molecules and increases the flexibility of the pole piece. Therefore, the first additive can improve the rigidity of the binder PAA, thereby improving the flexibility of the pole piece. In addition, when lithium iron phosphate is used in the positive electrode active material, the phosphate group in the lithium iron phosphate has more PO bonds, and the hydrogen bonds with the carboxyl groups in the binder PAA are stronger, so that the positive electrode active material particles are evenly dispersed in the glue, and PAA also improves rigidity and increases flexibility.

[0029] The second additive contains phosphate groups, ether bonds, and ester groups, all of which can generate hydrogen bonds with carboxyl groups. Therefore, the second additive can be adsorbed on the surface of the positive electrode active material and evenly dispersed in the glue, and can play the role of a dispersant and a softener at the same time.

[0030] The preparation method of the second additive specifically comprises the following steps:

[0031] A1. Under anhydrous and oxygen-free conditions, dissolve 1,12-dodecanediol in an organic solvent, add a strong base, and stir in an ice bath for 20 to 40 minutes; dissolve dodecanedioic acid in an organic solvent, add it at 0°C, and react at 90 to 100°C for 22 to 26 hours; add toluene, a white substance precipitates, filter, wash, and dry to obtain compound A;

[0032] A2. Under anhydrous and oxygen-free conditions, dissolve 1,12-dodecanediol in an organic solvent, add a strong base, and stir in an ice bath for 20 to 40 minutes; dissolve 1,12-dibromododecane in an organic solvent, add slowly at 0°C, and stir at room temperature for 1 to 3 hours after all the addition; add toluene, a white substance precipitates, filter, wash, and dry to obtain compound B;

[0033] A3. Under anhydrous and oxygen-free conditions, add an organic solvent to n-hexadecyl phosphoric acid, add a strong base, and stir in an ice bath for 20 to 40 minutes; dissolve compound B in an organic solvent, add slowly at 0°C, and stir at room temperature for 2 to 4 hours after all are added; dissolve compound A in an organic solvent, add slowly at 0°C, and stir at room temperature for 2 to 4 hours; after the reaction is completed, add methanol, and react at 60 to 100°C for 22 to 24 hours. Solution C is obtained;

[0034] A4. At 0°C, acetic acid was added to solution C until it became weakly acidic, and toluene was added to cause white matter to precipitate. The matter was filtered, washed, dried, and recrystallized to obtain a second additive.

[0035] The mass fraction of the first additive in the positive electrode slurry is 0.01-0.5%, and the mass fraction of the second additive in the positive electrode slurry is 0.01-0.3%. The mass fraction of the first additive in the positive electrode slurry can be 0.01wt%, 0.02wt%, 0.03wt%, 0.04wt%, 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, 0.35wt%, 0.4wt%, 0.45wt%, 0.85wt%, and can include but are not limited to the values ​​listed above, preferably 0.1wt%. The mass fraction of the second additive in the positive electrode slurry may be 0.01wt%, 0.02wt%, 0.03wt%, 0.04wt%, 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt%, 0.1wt%, 0.15wt%, 0.2wt%, 0.25wt%, 0.3wt%, and preferably 0.15wt%.

[0036] Wherein, the positive electrode active material includes at least one of lithium iron phosphate, lithium cobaltate, lithium manganate, nickel cobalt manganate and nickel cobalt aluminum lithium, preferably lithium iron phosphate. Lithium iron phosphate has good lattice stability, and the insertion and extraction of lithium ions have little effect on the lattice, so it has good reversibility and a long cycle life. However, lithium iron phosphate has poor electronic conductivity and ion transport properties, and is not suitable for large current charging and discharging. In order to solve this problem, the size of lithium iron phosphate particles is usually reduced, so the lithium iron phosphate has a large specific surface area, strong adsorption between particles, and difficulty in dispersion during pulping. By using multiple PO bonds in lithium iron phosphate, combined with binder PAA and additives, the hydrogen bonds generated between the phosphate group and the carboxyl group can solve the problem of difficulty in dispersing lithium iron phosphate, and can improve the processing performance and electrical properties of the pole piece. In this way, the use of binders and solvents can be reduced, the properties of the pole piece can be improved, and the cost can be reduced.

[0037] Wherein, the conductive agent is at least one of conductive carbon black, graphene and carbon nanotubes, preferably a mixture of conductive carbon black and carbon nanotubes.

[0038] The particle size Dv50 of the positive electrode active material is 0.5-1.0 μm, specifically 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, including but not limited to the values ​​listed above, preferably 0.7 μm.

[0039] The weight content ratio of the positive electrode active material, the binder, the conductive agent and the additive is (93-97wt%): (1-3wt%): (1.88-5wt%): (0.02-0.8wt%).

[0040] According to a second aspect of the present application, the present application provides a method for preparing a positive electrode slurry, comprising the following steps:

[0041] 1) Add the binder to the solvent and stir evenly;

[0042] 2) Adding a conductive agent and an additive to the solution in step 1) in sequence and stirring evenly;

[0043] 3) First, add 50-70 wt% of the positive electrode active material to the solution stirred evenly in step 2), stir evenly, then add the remaining 30-50 wt% of the positive electrode active material, stir evenly, and obtain the positive electrode slurry.

[0044] In some embodiments, the solvent includes a polar solvent, such as one or more selected from pyrrolidone, amide, water, ether, alcohol and ketone solvents. Specifically, the solvent may be N-methylpyrrolidone (NMP), N,N-dimethylformamide, N,N-dimethylacetamide, N,N-diethylformamide (DEF), dimethyl sulfoxide (DMSO), tetrahydrofuran (THF), triethyl phosphate, water, methanol, ethanol, ether and acetone, or any combination thereof, preferably N-methylpyrrolidone.

[0045] The inventors found that the binder polyacrylic acid (PAA) is a linear long-chain structure with a large number of carboxyl groups. The carboxyl groups form hydrogen bonds between the molecular chains of PAA itself, resulting in a certain degree of cross-linking, so the bonding performance is good, and it can form ester bonds and hydrogen bond structures with the hydroxyl groups on the surface of the active material particles or conductive agent particles, thereby enhancing the adhesion and facilitating the stability of the electrode. At the same time, PAA has lithium transfer properties, so that lithium ions can jump between adjacent carboxyl positions, thereby increasing the diffusion rate of lithium ions. The silicon in the additive lithium silicate has a strong affinity for oxygen, and oxygen is easy to form hydrogen bonds, so it can interact with lithium iron phosphate and PVDF through ionic bonds, covalent bonds or hydrogen bonds to make them have stronger adhesion. In this way, the use of binders and solvents can be reduced, the properties of the pole pieces can be improved, and the cost can be reduced. At the same time, the components are added in multiple times, and the intermolecular forces in the lithium silicate are combined with the solvent and the conductive agent respectively, so that the conductive agent particles are prevented from forming large agglomerations in the dispersed solution, thereby improving the dispersion uniformity of the conductive agent. Since the conductive agent is evenly dispersed in the positive electrode slurry, the chance of forming large agglomerations is reduced.

[0046] According to the third aspect of the present application, the present application also provides a positive electrode sheet, comprising a current collector and a positive electrode slurry layer coated on at least one surface of the current collector, wherein the positive electrode slurry layer comprises the positive electrode slurry described above.

[0047] The positive electrode slurry layer is coated on the current collector surface with a thickness of 230 to 270 μm, specifically 230 μm, 235 μm, 240 μm, 245 μm, 250 μm, 255 μm, 260 μm, 265 μm, 270 μm, including but not limited to the above-mentioned values, preferably 250 μm.

[0048] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be further described in detail below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto.

[0049] Example 1

[0050] The positive electrode slurry composition is: 94.99wt% lithium iron phosphate, 2wt% PAA, 2wt% SP, 1wt% CNT and 0.01wt% lithium silicate, and the D50 of the lithium iron phosphate is 0.7μm.

[0051] Preparation of positive electrode slurry:

[0052] 1) Add 2 wt% of polyacrylic acid (PAA) into N-methylpyrrolidone (NMP) and stir evenly;

[0053] 2) 1 wt% CNT, 2 wt% SP and 0.01 wt% lithium silicate were added to the solution in step 1) in sequence and stirred evenly;

[0054] 3) First, add 50% of lithium iron phosphate with a Dv50 of 0.7 μm to the solution stirred evenly in step 2), stir evenly, and then add the remaining 50% of lithium iron phosphate, stir evenly, to obtain the positive electrode slurry.

[0055] Preparation of positive electrode:

[0056] The positive electrode slurry prepared above is evenly coated on the aluminum foil by an extrusion coater with a coating thickness of 250 μm, and then baked at a baking temperature of 134°C. The baked electrode sheet is then cooled to room temperature and rolled and cut to obtain the positive electrode sheet.

[0057] Example 2

[0058] The difference from Example 1 is that the mass fraction of lithium iron phosphate in the positive electrode slurry is 94.98wt%, and the mass fraction of lithium silicate is 0.02wt%.

[0059] The rest is the same as in Example 1 and will not be described again here.

[0060] Example 3

[0061] The difference from Example 1 is that the mass fraction of lithium iron phosphate in the positive electrode slurry is 94.97wt%, and the mass fraction of lithium silicate is 0.03wt%.

[0062] The rest is the same as in Example 1 and will not be described again here.

[0063] Example 4

[0064] The difference from Example 1 is that the mass fraction of lithium iron phosphate in the positive electrode slurry is 94.95wt%, and the mass fraction of lithium silicate is 0.05wt%.

[0065] The rest is the same as in Example 1 and will not be described again here.

[0066] Example 5

[0067] Different from Example 1, the mass fraction of lithium iron phosphate in the positive electrode slurry is 94.92wt%, and the mass fraction of lithium silicate is 0.08wt%.

[0068] The rest is the same as in Example 1 and will not be described again here.

[0069] Example 6

[0070] The difference from Example 1 is that the mass fraction of lithium iron phosphate in the positive electrode slurry is 94.90wt%, the mass fraction of lithium silicate is 0.1wt%,

[0071] The rest is the same as in Example 1 and will not be described again here.

[0072] Example 7

[0073] The difference from Example 1 is that the mass fraction of lithium iron phosphate in the positive electrode slurry is 94.85wt%, and the mass fraction of lithium silicate is 0.15wt%.

[0074] The rest is the same as in Example 1 and will not be described again here.

[0075] Example 8

[0076] The difference from Example 1 is that the mass fraction of lithium iron phosphate in the positive electrode slurry is 94.80wt%, and the mass fraction of lithium silicate is 0.2wt%.

[0077] The rest is the same as in Example 1 and will not be described again here.

[0078] Example 9

[0079] The difference from Example 1 is that the mass fraction of lithium iron phosphate in the positive electrode slurry is 94.70wt%, and the mass fraction of lithium silicate is 0.3wt%.

[0080] The rest is the same as in Example 1 and will not be described again here.

[0081] Example 10

[0082] The difference from Example 1 is that the mass fraction of lithium iron phosphate in the positive electrode slurry is 94.50wt%, and the mass fraction of lithium silicate is 0.5wt%.

[0083] The rest is the same as in Example 1 and will not be described again here.

[0084] Embodiment 11

[0085] The difference from Example 1 is that the additive in the positive electrode slurry composition is the second additive, and its mass fraction is 0.01wt%.

[0086] The preparation method of the second additive comprises the following steps:

[0087] A1. Under anhydrous and oxygen-free conditions, 1,12-dodecanediol (10.12 g, 50 mmol) was dissolved in DMSO (200 ml), KOH (168.5 mg, 3 mmol) was added, and the mixture was stirred in an ice bath for 30 min; dodecanedioic acid (11.98 g, 52 mmol) was dissolved in DMSO (50 ml), added at 0°C, and reacted at 100°C for 24 h; toluene was added, and a white substance was precipitated, which was filtered, washed, and dried to obtain compound A;

[0088] A2. Under anhydrous and oxygen-free conditions, 1,12-dodecanediol (10.17 g, 50 mmol) was dissolved in DMSO (500 ml), KOH (5.89 g, 105 mmol) was added, and the mixture was stirred in an ice bath for 30 min; 1,12-dibromododecane (17.06 g, 52 mmol) was dissolved in DMSO (50 ml), and the mixture was slowly added at 0°C. After all the mixture was added, the mixture was stirred at room temperature for 2 h; toluene was added, and a white substance was precipitated. The mixture was filtered, washed, and dried to obtain compound B;

[0089] A3. Under anhydrous and oxygen-free conditions, add DMSO (20 ml) to n-hexadecyl phosphoric acid (1.53 g, 5 mmol), add KOH (337 mg, 6 mmol), and stir in an ice bath for 30 min. Dissolve compound B in DMSO (20 ml), add slowly at 0°C, and stir at room temperature for 2 h after all are added. Dissolve compound A in DMSO (50 ml), add slowly at 0°C, and stir at room temperature for 2 h; after the reaction is complete, add 5 ml of methanol and react at 80°C for 24 h. Obtain solution C;

[0090] A4. At 0°C, acetic acid was added to solution C until it became weakly acidic, and toluene was added to cause white matter to precipitate. The matter was filtered, washed, dried, and recrystallized to obtain a second additive.

[0091] The rest is the same as in Example 1 and will not be described again here.

[0092] Example 12

[0093] The difference from Example 2 is that the additive in the positive electrode slurry composition is the second additive, and its mass fraction is 0.02wt%.

[0094] The rest is the same as in Example 2 and will not be described again here.

[0095] Embodiment 13

[0096] The difference from Example 3 is that the additive in the positive electrode slurry composition is the second additive, and its mass fraction is 0.03wt%.

[0097] The rest is the same as in Example 3 and will not be described again here.

[0098] Embodiment 14

[0099] The difference from Example 4 is that the additive in the positive electrode slurry composition is the second additive, and its mass fraction is 0.05wt%.

[0100] The rest is the same as in Example 4 and will not be described again here.

[0101] Embodiment 15

[0102] The difference from Example 5 is that the additive in the positive electrode slurry composition is the second additive, and its mass fraction is 0.08wt%.

[0103] The rest is the same as in Example 5 and will not be described again here.

[0104] Example 16

[0105] The difference from Example 6 is that the additive in the positive electrode slurry composition is the second additive, and its mass fraction is 0.1wt%.

[0106] The rest is the same as in Example 6 and will not be described again here.

[0107] Embodiment 17

[0108] The difference from Example 7 is that the additive in the positive electrode slurry composition is the second additive, and its mass fraction is 0.15wt%,

[0109] The rest is the same as in Example 7 and will not be described again here.

[0110] Embodiment 18

[0111] The difference from Example 8 is that the additive in the positive electrode slurry composition is the second additive, and its mass fraction is 0.2wt%.

[0112] The rest is the same as in Example 8 and will not be described again here.

[0113] Embodiment 19

[0114] The difference from Example 9 is that the additive in the positive electrode slurry composition is the second additive, and its mass fraction is 0.3wt%.

[0115] The rest is the same as in Example 9 and will not be described again here.

[0116] Embodiment 20

[0117] Different from Example 1, the additives in the positive electrode slurry composition are 0.15 wt % lithium silicate and 0.15 wt % of the second additive, and the mass fraction of the lithium iron phosphate is 94.7 wt %.

[0118] The rest is the same as in Example 1 and will not be described again here.

[0119] Embodiment 21

[0120] Different from Example 1, the additives in the positive electrode slurry composition are 0.1 wt % lithium silicate and 0.2 wt % of the second additive, and the mass fraction of the lithium iron phosphate is 94.7 wt %.

[0121] The rest is the same as in Example 1 and will not be described again here.

[0122] Embodiment 22

[0123] Different from Example 1, the additives in the positive electrode slurry composition are 0.2 wt % lithium silicate and 0.1 wt % of the second additive, and the mass fraction of the lithium iron phosphate is 94.7 wt %.

[0124] The rest is the same as in Example 1 and will not be described again here.

[0125] Embodiment 23

[0126] Different from Example 1, the additives in the positive electrode slurry composition are 0.01 wt % lithium silicate and 0.01 wt % of the second additive, and the mass fraction of the lithium iron phosphate is 94.98 wt %.

[0127] The rest is the same as in Example 1 and will not be described again here.

[0128] Embodiment 24

[0129] Different from Example 1, the additives in the positive electrode slurry composition are 0.01 wt % lithium silicate and 0.3 wt % of the second additive, and the mass fraction of the lithium iron phosphate is 94.69 wt %.

[0130] The rest is the same as in Example 1 and will not be described again here.

[0131] Embodiment 25

[0132] Different from Example 1, the additives in the positive electrode slurry composition are 0.3 wt % lithium silicate and 0.01 wt % of the second additive, and the mass fraction of the lithium iron phosphate is 94.69 wt %.

[0133] The rest is the same as in Example 1 and will not be described again here.

[0134] Embodiment 26

[0135] Different from Example 1, the additives in the positive electrode slurry composition are 0.05 wt % lithium silicate and 0.05 wt % of the second additive, and the mass fraction of the lithium iron phosphate is 94.90 wt %.

[0136] The rest is the same as in Example 1 and will not be described again here.

[0137] Embodiment 27

[0138] Different from Example 1, the additives in the positive electrode slurry composition are 0.1 wt % lithium silicate and 0.1 wt % of the second additive, and the mass fraction of the lithium iron phosphate is 94.80 wt %.

[0139] The rest is the same as in Example 1 and will not be described again here.

[0140] Embodiment 28

[0141] Different from Example 1, the additives in the positive electrode slurry composition are 0.3 wt % lithium silicate and 0.3 wt % of the second additive, and the mass fraction of the lithium iron phosphate is 94.40 wt %.

[0142] The rest is the same as in Example 1 and will not be described again here.

[0143] Embodiment 29

[0144] Different from Example 1, the additives in the positive electrode slurry composition are 0.5 wt % lithium silicate and 0.3 wt % of the second additive, and the mass fraction of the lithium iron phosphate is 94.20 wt %.

[0145] The rest is the same as in Example 1 and will not be described again here.

[0146] Comparative Example 1

[0147] The difference from Example 1 is that the binder in the positive electrode slurry composition is 2.0 wt% polyvinylidene fluoride (PVDF).

[0148] The rest is the same as in Example 1 and will not be described again here.

[0149] Comparative Example 2

[0150] Different from Example 1, no additives were added to the positive electrode slurry, and the positive electrode slurry consisted of 95wt% lithium iron phosphate, 2wt% PAA, 2wt% SP and 1wt% CNT.

[0151] The rest is the same as in Example 1 and will not be described again here.

[0152] Comparative Example 3

[0153] The difference from Example 1 is that the additive in the positive electrode slurry composition is 0.1wt% lithium phosphate;

[0154] The rest is the same as in Example 1 and will not be described again here.

[0155] The positive electrode slurries and positive electrode sheets of the above-mentioned Examples 1 to 29 and Comparative Examples 1 to 3 were subjected to the following performance tests. The test results are shown in Tables 1 and 2 below.

[0156] (1) Film performance test:

[0157] Take pure PVDF glue, pure PAA glue and ten parts of glue in Examples 1-10. All adhesive solutions were cast into a dumbbell-shaped mold with a length of 100 mm, a width of 10 mm and a thickness of 5 mm. After being placed at room temperature for 48 hours, they were demoulded and trimmed, and then baked in an oven at 85°C for 4 hours to obtain an adhesive film. Mechanical properties were tested using an electronic universal testing machine. At room temperature, the lower fixture was kept stationary, and the upper fixture was stretched upward at a tensile rate of 5 mm / min. The elastic modulus and elongation at break measured in the elastic deformation section were recorded.

[0158] Table 1

[0159]

[0160]

[0161] (2) Let the slurry stand and observe its state after 2 hours; bend the electrode inward to observe its flexibility.

[0162] (3) Adhesion test: Stick about 10 cm of double-sided tape on one side of the electrode prepared above, leave 15 cm of free space on the other side of the double-sided tape, and roll it with a roller 3 times to make the electrode and the double-sided tape fit tightly. Cut the electrode into strips about 25 cm long, with double-sided tape on one end and a blank electrode on the other end. Prepare 6 strips. Stick the electrode with double-sided tape on a clean glass plate and roll it with a roller 3 times. Use an electronic universal tensile testing machine to test the adhesion. Fix one end of the electrode on the glass plate upwards and fix the other end with a clamp. Turn the free end of the electrode upwards and fix it with the upper clamp. Keep the lower clamp stationary, stretch the upper clamp at a speed of 250 mm / min, and test for about 20 seconds. Test 6 times and take the average value.

[0163] (4) Cohesion test: Apply a 50μm thick layer of PVDF glue evenly on the surface of the aluminum foil, dry it, apply a 250μm thick slurry on the dried film, and bake it dry. The subsequent test process is the same as the adhesion test. Since there is a layer of PVDF between the aluminum foil and the slurry layer, the interfacial force is strong. During the test, the interface between the aluminum foil and the PVDF layer, and the interface between the PVDF layer and the slurry layer will not break. The measured result is the force of tearing the slurry layer, that is, the cohesion.

[0164] (5) Diaphragm resistance test: Test the resistance at 5 different positions of the electrode and take the average value.

[0165] Table 2

[0166]

[0167]

[0168] From the test results of the analytical films in Table 1, it can be seen that the rigidity of the embodiment in which PAA is selected as the adhesive is stronger than that of PVDF in the comparative example, the PAA film is more brittle than PVDF, and the intramolecular bonding force of PAA is stronger than that of PVDF. The addition of lithium silicate in Examples 1 to 10 reduces the elastic modulus, weakens the rigidity of PAA, increases flexibility, and increases the intramolecular bonding force to a certain extent. In Comparative Example 3, the addition of lithium phosphate to PAA can well reduce the elastic modulus, but because the acidity of phosphoric acid is stronger than that of silicic acid, the force of phosphoric acid on hydrogen is less than that of silicic acid, resulting in a weaker elongation at break than that of silicic acid and a weaker tensile strength. The addition of the second additive in Examples 11 to 19 can also reduce the elastic modulus well. This is because the phosphate group and the carboxyl group have a stronger force, while the ether bond and the ester group are weaker. The molecular chain will stretch out in the glue and disperse between the PAA chains. The oxygen and hydrogen in the ether bond and the ester group form hydrogen bonds, separating the PAA molecular chains, reducing the contact between the carboxyl groups, and thus reducing the rigidity of the PAA; because the second additive increases the crosslinking degree of the molecular chains between the glue, the elongation at break and the tensile strength are both improved. When lithium silicate and the second additive are added at the same time in Examples 20 to 29, it can be found that the two have a mutually reinforcing effect, but when the total amount of the two additives is large, a deterioration effect will occur.

[0169] From the performance test results of the slurry and the pole piece in Table 2, it can be seen from Comparative Examples 1 and 2 that the adhesive PAA has better adhesion. Due to the high rigidity of PAA, the pole piece is hard and brittle, which causes the pole piece to crack and fall off when it is wound. After adding a small amount of lithium silicate to the PAA slurry, the carboxyl groups and silicate groups in the PAA are connected together by hydrogen bonds, which separates the contact between the PAAs, weakens the interaction between the PAAs, and reduces the rigidity of the PAA. The flexibility of the pole piece is the magnitude of the force between the PAA molecular chains. PAA has many carboxyl groups, and the mutual force between them is very large, so it is easy to aggregate and form crystals. Therefore, when pure PAA is used, the pole piece is very brittle.

[0170] From Examples 1 to 10, the additive lithium silicate is added to the positive electrode slurry. Lithium silicate weakens the contact between PAA molecules and reduces the crystallinity of PAA, thereby improving flexibility. Adhesion and cohesion are the adsorption forces of PAA on the current collector and PAA on the active material, respectively. There are some oxygen elements or metal ions on the surface of the current collector and the surface of the active material. The addition of lithium silicate makes PAA more dispersed. These oxygen elements or metal ions can form more hydrogen bonds or ionic bonds with the carboxyl group, so the adhesion and cohesion will increase, and the conductivity will also improve due to the improvement of dispersion.

[0171] It can be seen from Examples 6 to 10 that when the lithium silicate content exceeds 0.1wt%, the bonding force of the pole piece begins to decrease and the resistance begins to increase, indicating that the dispersibility of the slurry begins to decrease. It can be found from Examples 9 and 10 that when the lithium silicate content exceeds 0.3wt%, the slurry begins to gel, the binder in the slurry is cross-linked, and the PAA does not cross-link, indicating that a strong interaction occurs between the lithium silicate and the PAA at this time, limiting the fluidity of the slurry.

[0172] It can be found from the examples and comparative example 3 that the effect of adding lithium phosphate to PAA is similar to that of lithium silicate. Since the acidity of phosphoric acid is stronger than that of silicic acid, the hydrogen bond formed between phosphate and hydrogen is weaker than that between silicate, resulting in that the adhesive force and cohesive force of comparative example 3 are both less than those of lithium silicate with the same content.

[0173] From Examples 11 to 19, after adding the synthesized second additive to PAA, the ether bonds and ester chain segments of the second additive stretch into NMP, reducing the contact of carboxyl groups between PAA, increasing the distance between PAA molecules, improving the dispersibility of the slurry, and allowing more carboxyl groups to contact the current collector and active materials. The changes in electrode adhesion, cohesion and conductivity are similar to those when lithium silicate is added, and are therefore improved.

[0174] From Examples 20 to 29, when lithium silicate and additives are added to PAA at the same time, the two have a promoting effect and have a promoting relationship on the adhesion and cohesion. When the total amount of the two additives is large, the adhesion and cohesion will be deteriorated, such as in Examples 28 and 29, the slurry gels and has poor performance.

[0175] In summary, the present invention improves the dispersibility of the slurry by forming hydrogen bonds with the carboxyl groups of PAA through the first additive lithium silicate and the synthesized second additive in the positive electrode slurry, separating the direct contact of the carboxyl groups, increasing the distance between PAA molecules, and weakening the interaction between PAA. However, the interaction between lithium silicate and carboxyl groups is relatively strong, and adding too much lithium silicate will worsen the dispersion of the slurry; the interaction between the phosphate group, ether bond and ester group in the additive and the carboxyl group is weaker than that of lithium silicate, and the slurry will not produce gel, and the alkyl segment is also conducive to the dispersion of the slurry and the flexibility of the electrode; in addition, the second additive and PAA are not sensitive to moisture, which can reduce the requirements for the production environment.

[0176] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.

Claims

1. A positive electrode slurry comprising a positive electrode active material, a binder, a conductive agent and an additive, It is characterized in that The binder includes polyacrylic acid, and the additive includes at least one of a first additive and a second additive, wherein the first additive is lithium silicate, and the second additive is a copolymer with a phosphoric acid group, an ether bond, and an ester group.

2. A positive electrode slurry according to claim 1, It is characterized in that The structural formula of the second additive is as follows:

3. The positive electrode slurry according to claim 1, It is characterized in that The number of ether group and ester group segments in the second additive is 15 to 25, the length of the carbon chain connecting the ether bond and the ester group is 10 to 14 carbon atoms, and the molecular weight of the second additive is 6000 to 10000.

4. The positive electrode slurry according to claim 1, It is characterized in that The mass fraction of the first additive in the positive electrode slurry is 0.01-0.5%, and the mass fraction of the second additive in the positive electrode slurry is 0.01-0.3%.

5. The positive electrode slurry according to claim 1, It is characterized in that The preparation method of the second additive comprises the following steps: A1. Under anhydrous and oxygen-free conditions, dissolve 1,12-dodecanediol in an organic solvent, add a strong base, and stir in an ice bath for 20 to 40 minutes; dissolve dodecanedioic acid in an organic solvent, add it at 0°C, and react at 90 to 100°C for 22 to 26 hours; add toluene, a white substance precipitates, filter, wash, and dry to obtain compound A; A2. Under anhydrous and oxygen-free conditions, dissolve 1,12-dodecanediol in an organic solvent, add a strong base, and stir in an ice bath for 20 to 40 minutes; dissolve 1,12-dibromododecane in an organic solvent, add slowly at 0°C, and stir at room temperature for 1 to 3 hours after all the addition; add toluene, a white substance precipitates, filter, wash, and dry to obtain compound B; A3. Under anhydrous and oxygen-free conditions, add an organic solvent to n-hexadecyl phosphoric acid, add a strong base, and stir in an ice bath for 20 to 40 minutes; dissolve compound B in an organic solvent, add slowly at 0°C, and stir at room temperature for 2 to 4 hours after all are added; dissolve compound A in an organic solvent, add slowly at 0°C, and stir at room temperature for 2 to 4 hours; after the reaction is completed, add methanol, and react at 60 to 100°C for 22 to 24 hours. Solution C is obtained; A4. At 0°C, acetic acid was added to solution C until it became weakly acidic, and toluene was added to cause white matter to precipitate. The matter was filtered, washed, dried, and recrystallized to obtain a second additive.

6. The positive electrode slurry according to claim 1, It is characterized in that The positive electrode active material includes at least one of lithium iron phosphate, lithium cobaltate, lithium manganate, lithium nickel cobalt manganate and lithium nickel cobalt aluminum oxide; the particle size Dv50 of the positive electrode active material is 0.5-1.0 μm.

7. The positive electrode slurry according to claim 1, It is characterized in that The conductive agent includes at least one of conductive carbon black, graphene and carbon nanotubes.

8. The positive electrode slurry according to claim 1, It is characterized in that The weight content ratio of the positive electrode active material, the binder, the conductive agent and the additive is (93-97wt%): (1-3wt%): (1.88-5%wt%): (0.01-0.8wt%).

9. A method for preparing a positive electrode slurry according to any one of claims 1 to 8, It is characterized in that The following steps are involved: 1) Add the binder to the solvent and stir evenly; 2) Adding a conductive agent and an additive to the solution in step 1) in sequence and stirring evenly; 3) First, add 50-70 wt% of the positive electrode active material to the solution stirred evenly in step 2), stir evenly, then add the remaining 30-50 wt% of the positive electrode active material, stir evenly, and obtain the positive electrode slurry.

10. A positive electrode sheet comprising a current collector and a positive electrode slurry layer coated on at least one surface of the current collector, It is characterized in that The positive electrode slurry layer comprises the positive electrode slurry according to any one of claims 1 to 8.

Citation Information

Cited By

  • Lithium ion secondary battery, preparation method thereof and electric device

    CN119153702A

  • Lithium ion secondary battery, method for manufacturing the same, and electric device

    CN119153702B

  • Positive electrode slurry and preparation method and application thereof

    CN119495744A