Zinc ion doped cerium oxide nano composite material as well as preparation method and application thereof
By optimizing the preparation process of zinc ion-doped cerium oxide and using acetic acid and a combination of zinc ions and ethylene glycol, zinc ion-doped cerium oxide nanocomposites with unique nanomorphology and excellent performance were successfully prepared, solving the existing problems. The technology improves the appearance and performance problems and achieves more efficient antioxidant and antibacterial effects.
Patent Information
- Application Number
- CN202410849068.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
AI Technical Summary
The preparation process of zinc ion doped cerium oxide in the existing technology has problems in morphology control and performance improvement, especially when selecting the cerium oxide precursor, pH adjuster and dispersant, which affects the morphology and performance of the final product.
By fully dissolving cerium nitrate hexahydrate with water, adding pH adjuster acetic acid and zinc ion preparation, adding dispersion medium ethylene glycol after mixing, heating reaction and washing with water, zinc ion doping with unique nano-morphology is prepared Cerium oxide nanocomposites.
The special "hollow" morphology and smaller nanosphere diameter of zinc ion-doped cerium oxide nanocomposites have been achieved, which improves the antioxidant and antibacterial properties. At the same time, the amount of zinc ions added has been optimized, reducing costs and enhancing market competitiveness.
Smart Images

Figure CN118845495A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a composite material for cosmetics, in particular to a zinc ion doped cerium oxide nanocomposite material and a preparation method and application thereof, belonging to the technical field of cosmetics. Background Art
[0002] Cerium (Ce) is a lanthanide element in the periodic table and belongs to the rare earth metals. It is relatively cheap and has greater production and economic advantages than other rare earth elements. The characteristic of single Ce is that it has high reactivity and will oxidize in the air. There are two valence states of cerium oxide, trivalent cerium and tetravalent cerium, which can be reversibly transformed between these two valence states, accompanied by the generation and elimination of oxygen vacancies, thus having good antioxidant or antibacterial activity.
[0003] Oxidative stress in cells is a mediator of many diseases, including cellular aging, atherosclerosis, arthritis, and neurodegenerative diseases such as Parkinson's disease and Alzheimer's disease. Cerium oxide is generally considered to limit cellular aging by reducing free radicals formed within cells. This scavenging ability can be achieved by adding Ce 3+ Oxidation to Ce 4+ In addition, nano-cerium oxide can show activities such as peroxidase, superoxide dismutase or catalase, which may be involved in biological processes that interfere with bacterial growth and metabolism. For example, researchers have synthesized a cerium oxide nanoparticle with phosphatase-like activity, which has catalytic selectivity for phosphate bonds and can specifically catalyze the cleavage of the PO bond of the RO-PO3 molecule, significantly reducing the formation of the LPS-t lr4 complex, the activation of NF-κB and the release of pro-inflammatory cytokines, potentially preventing the growth of Gram-negative bacteria.
[0004] How to improve the performance of cerium oxide and achieve synergistic effects through technical means is still a hot topic in this field. Those skilled in the art have found that doping is a powerful means to improve the performance of cerium oxide in the fields of catalysis, photocatalysis, biomedicine and energy. This is because doping can increase the Ce in cerium oxide. 3+ratio and oxygen vacancy content. To this end, technicians have found through first-principles calculations that doping with elements such as Mn, Pr, Sn, and Zr can reduce the formation energy of oxygen vacancies in cerium oxide, but there are differences in their mechanisms. Among them, when cerium is doped, external defects are introduced into its crystal structure, oxygen vacancies are generated, and the migration of oxygen is improved, all of which lead to enhanced performance. The advantages of doping include, but are not limited to, enhanced catalytic activity. One way to achieve this goal is to dope metals with high ion mobility, which act as shallow electron traps to suppress electron-hole recombination processes. In addition, the doping of rare earth metals leads to weaker metal-oxygen bonds, which is also conducive to better catalytic performance. In addition, the oxygen vacancies in doped cerium oxide can be used as probes to detect the free radicals generated when they are transferred through a jumping mechanism. At the same time, the addition of dopants will also destroy the chemical bonds on the surface of cerium oxide, thereby generating new active centers, thereby improving the selectivity and stability of the resulting doped catalyst.
[0005] There are reports on zinc ion doped cerium oxide in the prior art, but the inventors found in their research that there are many technical problems in the preparation process of zinc ion doped cerium oxide, and the selection and adjustment of cerium oxide precursors, pH regulators, dispersants and preparation process parameters are crucial, which can directly affect the target morphology of the final product and thus affect the product performance. For example, a variety of cerium-containing precursors such as commercially available CeCl3·7H2O cannot prepare the target morphology of the composite material of the present invention, resulting in poor performance of the final product. This is because the decomposition reaction process and products of different Ce-containing salts are different, and different anions have different effects on morphology control. Second, the pH regulator will also directly affect the morphology of the target product. For example, after the pH regulator is selected as formic acid, the synthesized cerium oxide is severely aggregated and has an irregular morphology. In the selection of acids, organic acids involving safety issues also need to be excluded. Third, in the selection of organic solvents such as dispersants, organic solutions such as propylene glycol will cause changes in product results and degradation of performance.
[0006] In summary, how to provide a zinc ion-doped cerium oxide that has both a unique nanomorphology and synergistic effects to improve material performance to solve the above-mentioned problems in the prior art is of great significance for the wide application of cerium oxide as an antioxidant or preservative in biomedicine and cosmetics. Summary of the invention
[0007] Based on the above problems in the prior art, the primary technical problem to be solved by the present invention is to provide a method for preparing a zinc ion-doped cerium oxide nanocomposite material which can be used as a cosmetic, a cosmetic additive, an external medicine or an external medicine additive, and has a unique nano morphology and better antioxidant and antibacterial properties, comprising the following steps:
[0008] (1) fully dissolving a cerium-containing precursor in water to prepare a precursor solution; the cerium-containing precursor is cerium nitrate hexahydrate;
[0009] (2) adding a pH adjuster to prepare a first solution;
[0010] (3) adding a zinc ion-containing preparation to the first solution and mixing thoroughly to prepare a second solution doped with zinc ions;
[0011] (4) adding a dispersion medium to the second solution and stirring the mixture to obtain a third solution;
[0012] (5) heating the third solution to react;
[0013] (6) Wash the product obtained in step (5) with water, centrifuge, and dry.
[0014] In some embodiments, the mass volume ratio of the cerium-containing precursor to water in step (1) is intended to allow the cerium-containing precursor to be completely dissolved in water.
[0015] In some embodiments, the concentration of the cerium-containing precursor in step (1) is 0.5 g / mL to 1.5 g / mL.
[0016] In some embodiments, the pH adjuster in step (2) is one or more of acetic acid and propionic acid.
[0017] In some embodiments, the mass ratio of the cerium-containing precursor to the pH adjuster is (16-19.9): (16-20).
[0018] In some embodiments, the zinc ion-containing agent in step (3) is one or more of zinc chloride and zinc nitrate hexahydrate.
[0019] In some embodiments, the molar ratio of zinc ions to cerium ions in the second solution of step (3) is 0.1 mol% to 40 mol%.
[0020] In some embodiments, the dispersion medium in step (4) is ethylene glycol.
[0021] In some embodiments, the mass volume ratio of the cerium-containing precursor to ethylene glycol is (16-19.9) g: (600-700) mL.
[0022] In some embodiments, the heating reaction in step (5) comprises one or more of the following conditions a) to b):
[0023] a) the temperature of the heating reaction is 160°C to 190°C;
[0024] b) The heating reaction time is 120 min to 200 min.
[0025] In some embodiments, the centrifugation condition in step (6) is 8000-10000 rpm for 10-20 minutes.
[0026] Another technical problem to be solved by the present invention is to provide a zinc ion-doped cerium oxide nanocomposite material, wherein the nanocomposite material is prepared by the above method.
[0027] Another technical problem to be solved by the present invention is to provide a new use of the zinc ion-doped cerium oxide nanocomposite material prepared by the above method in the preparation of cosmetics, cosmetic additives, external medicines and / or external medicine additives.
[0028] Another technical problem to be solved by the present invention is to provide a cosmetic comprising the zinc ion-doped cerium oxide nanocomposite material prepared by the above method.
[0029] The composite material prepared by the present invention can be mainly used in the following types of cosmetics, including but not limited to: emulsion products such as cleansing cream, moisturizing cream, moisturizing lotion, etc.; powder products such as scented powder, talcum powder, etc.; block products such as pressed powder, rouge, etc.; suspended products such as liquid foundation, etc.; surfactant solvent products such as shampoo, hand sanitizer, etc.; gel products such as cleansing gel, sleeping mask, etc.; paste products such as shampoo cream, paste mask, etc.
[0030] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0031] (1) The present invention has conducted creative research on the selection and compatibility of raw materials such as cerium-containing precursors, pH regulators and dispersants, which can achieve the "hollow" special morphology of zinc ion-doped cerium oxide nanocomposites and further reduce the diameter of zinc ion-doped cerium oxide nanospheres, thereby solving the problem in the prior art of poor morphology and structure of target particles of composite materials due to material selection and compatibility issues, resulting in reduced product performance.
[0032] (2) The present invention improves the preparation process and condition parameters, and works synergistically with the raw materials and compatibility relationship to achieve the improvement of the morphology and performance of the target product. The present invention can obtain more excellent antibacterial performance without affecting the antioxidant capacity of cerium oxide.
[0033] (3) The present invention optimizes the amount of zinc ions added, achieves better product performance with less zinc ions added, and reduces product costs and increases market competitiveness. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1Transmission electron microscope images of pure CeO2 nanospheres and Zn / CeO2 nanospheres;
[0035] Figure 2A is the diameter distribution diagram of pure CeO2 nanospheres;
[0036] Figure 2B is the diameter distribution diagram of Zn / CeO2 nanospheres;
[0037] Figure 3 The bar graph of DPPH removal rate of cerium oxide samples under different zinc ion doping amounts;
[0038] Figure 4 The bar graph of hydroxyl radical scavenging rate of cerium oxide samples under different zinc ion doping amounts;
[0039] Figure 5 The bar graph of superoxide anion radical scavenging rate of cerium oxide samples under different zinc ion doping amounts;
[0040] Figure 6 The remaining colonies after pure CeO2 nanospheres and Zn / CeO2 nanospheres were co-cultured with Staphylococcus aureus for 24 hours;
[0041] Fig. 7A The bar graph shows the antibacterial rate of pure CeO2 nanospheres and Zn / CeO2 nanospheres after co-culture with Staphylococcus aureus for 24 hours;
[0042] Figure 7B A bar graph of the antibacterial rate of cerium oxide with different zinc doping amounts was set up when the cerium oxide concentration was 0.03125%;
[0043] Figure 8 The remaining colonies after pure CeO2 nanospheres and Zn / CeO2 nanospheres were co-cultured with Escherichia coli for 24 hours;
[0044] Fig.9A The bar graph shows the antibacterial rate of pure CeO2 nanospheres and Zn / CeO2 nanospheres after co-culture with Escherichia coli for 24 hours;
[0045] Fig. 9B A bar graph of the antibacterial rate of cerium oxide with different zinc doping amounts was set up when the cerium oxide concentration was 0.0625%;
[0046] Fig. 10A It is a comparison diagram of Comparative Example 8 before and after the synthesis reaction;
[0047] Fig. 10B This is a comparison diagram of Comparative Example 10 before and after the synthesis reaction. DETAILED DESCRIPTION
[0048] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described in the present invention. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0049] Unless otherwise defined, all technical and scientific terms used in the present invention have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention.
[0050] In the present invention, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0051] In the present invention, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed in the present invention should be understood to include any and all subranges included therein.
[0052] The present invention only specifically discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.
[0053] The temperature parameters in the present invention, if not specifically limited, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument.
[0054] In the description of the invention, “plurality” means at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0055] If there is no special description, all embodiments and optional embodiments of the present invention can be combined with each other to form a new technical solution. If there is no special description, all technical features and optional technical features of the present invention can be combined with each other to form a new technical solution.
[0056] If not specifically stated, all steps of the present invention may be performed sequentially or randomly, but are preferably performed sequentially.
[0057] The raw materials and equipment used in the present invention are well known to those skilled in the art. The raw materials used in the present invention can be prepared by themselves according to the prior art or purchased commercially, and the equipment used in the present invention can also be purchased commercially. The following lists the ways to obtain the raw materials and equipment of the present invention.
[0058] The raw materials and sources of the present invention are shown in Table 1.
[0059] Table 1
[0060]
[0061] The equipment and sources in the present invention are shown in Table 2.
[0062] Table 2
[0063]
[0064] The technical solution of the present invention is described in detail in conjunction with specific embodiments as follows.
[0065] Example 1
[0066] (1) Weigh 1.99 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0067] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0068] (3) adding 0.5 mol % zinc chloride to the first solution and mixing uniformly by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0069] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0070] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0071] (6) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 0.5 mol % Zn / CeO2 nanospheres.
[0072] Example 2
[0073] (1) Weigh 1.98 g of cerium sulfate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0074] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0075] (3) adding 1 mol % zinc chloride to the first solution and mixing uniformly by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0076] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0077] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0078] (6) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 1 mol % Zn / CeO 2 nanospheres.
[0079] Example 3
[0080] (1) Weigh 1.96 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0081] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0082] (3) adding 2 mol % zinc chloride to the first solution and mixing uniformly by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0083] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0084] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0085] (6) The suspension after the reaction was centrifuged at 10,000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 2 mol % Zn / CeO 2 nanospheres.
[0086] Example 4
[0087] (1) Weigh 1.90 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0088] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0089] (3) adding 5 mol % zinc chloride to the first solution and mixing by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0090] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0091] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0092] (6) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 5 mol % Zn / CeO 2 nanospheres.
[0093] Example 5
[0094] (1) Weigh 1.80 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0095] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0096] (3) adding 10 mol % zinc chloride to the first solution and mixing uniformly by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0097] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0098] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0099] (6) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 10 mol % Zn / CeO 2 nanospheres.
[0100] Example 6
[0101] (1) Weigh 1.60 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0102] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0103] (3) adding 20 mol % zinc chloride to the first solution and mixing uniformly by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0104] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0105] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0106] (6) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 20 mol % Zn / CeO 2 nanospheres.
[0107] Example 7
[0108] Except that the 0.5 mol % zinc chloride in step (3) is replaced by 0.5 mol % zinc nitrate hexahydrate, other contents are consistent with those in Example 1.
[0109] Example 8
[0110] Except that the amount of ethylene glycol was changed to 70 ml, other contents were consistent with those in Example 1.
[0111] Example 9
[0112] Except that the amount of acetic acid is changed to 1.6 g, other contents are consistent with Example 1.
[0113] Example 10
[0114] Except that the reaction temperature of step (5) was changed to 160° C., other contents were consistent with those of Example 1.
[0115] Embodiment 11
[0116] Except that the reaction temperature of step (5) was changed to 190° C., other contents were consistent with those of Example 1.
[0117] Example 12
[0118] Except that the reaction time of step (5) was changed to 120 min, other contents were consistent with Example 1.
[0119] Embodiment 13
[0120] Except that the centrifugation condition in step (6) was changed to 8000 rpm, 20 min, all other contents were consistent with Example 1.
[0121] Embodiment 14
[0122] Except that the acetic acid in step (2) is replaced by propionic acid, other contents are consistent with those in Example 1.
[0123] Embodiment 15
[0124] Except that the 1.99 g of cerium nitrate hexahydrate in step (1) is replaced by 1 g of cerium nitrate hexahydrate, other contents are consistent with those in Example 1.
[0125] Example 16
[0126] Except that 1.99 g of cerium nitrate hexahydrate in step (1) is replaced with 3 g of cerium nitrate hexahydrate, other contents are consistent with those in Example 1.
[0127] Comparative Examples used in the present invention
[0128] Comparative Example 1 Pure CeO2 Nanospheres
[0129] (1) Weigh 2 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0130] (2) adding 2 g of acetic acid to the precursor solution and mixing by ultrasonication for 10 min to obtain a first solution;
[0131] (3) adding 60 ml of ethylene glycol to the first solution and stirring at 400 rpm for 30 min to prepare a second solution;
[0132] (4) The second solution was transferred into an autoclave and reacted in an oven at 180°C for 200
[0133] min;
[0134] (5) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of pure CeO2 nanospheres.
[0135] Comparative Example 2 0.1mol% Zn / CeO2 nanospheres:
[0136] (1) Weigh 1.998 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0137] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0138] (3) adding 0.1 mol % zinc chloride to the first solution and mixing uniformly by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0139] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0140] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0141] (6) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 0.1 mol % Zn / CeO2 nanospheres.
[0142] Comparative Example 3 0.2mol% Zn / CeO2 nanospheres
[0143] (1) Weigh 1.996 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0144] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0145] (3) adding 0.2 mol % zinc chloride to the first solution and mixing uniformly by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0146] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0147] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0148] (6) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 0.2 mol % Zn / CeO2 nanospheres.
[0149] Comparative Example 4 0.3mol% Zn / CeO2 nanospheres
[0150] (1) Weigh 1.994 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0151] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0152] (3) adding 0.3 mol % zinc chloride to the first solution and mixing uniformly by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0153] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0154] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0155] (6) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 0.3 mol % Zn / CeO2 nanospheres.
[0156] Comparative Example 5 0.4mol% Zn / CeO2 nanospheres
[0157] (1) Weigh 1.992 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0158] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0159] (3) adding 0.4 mol % zinc chloride to the first solution and mixing uniformly by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0160] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0161] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0162] (6) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 0.4 mol % Zn / CeO2 nanospheres.
[0163] Comparative Example 6 30mol% Zn / CeO2 nanospheres
[0164] (1) Weigh 1.40 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0165] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0166] (3) adding 30 mol % zinc chloride to the first solution and mixing uniformly by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0167] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0168] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0169] (6) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 30 mol % Zn / CeO2 nanospheres.
[0170] Comparative Example 7 40mol% Zn / CeO2 nanospheres
[0171] (1) Weigh 1.20 g of cerium nitrate hexahydrate and dissolve it in 2 g of water until it is fully dissolved to prepare a precursor solution;
[0172] (2) adding 2 g of acetic acid to the precursor solution and mixing evenly to obtain a first solution;
[0173] (3) adding 40 mol % zinc chloride to the first solution and mixing uniformly by ultrasonication for 10 min to obtain a second solution doped with zinc ions;
[0174] (4) adding 60 ml of ethylene glycol to the second solution and stirring at 400 rpm for 30 min to prepare a third solution;
[0175] (5) The third solution was transferred into an autoclave and reacted in an oven at 180° C. for 200 min;
[0176] (6) The suspension after the reaction was centrifuged at 10000 rpm for 10 min, washed with water three times, and dried at 45° C. overnight to obtain a solid powder of 40 mol % Zn / CeO2 nanospheres.
[0177] Comparative Example 8
[0178] Except that the cerium nitrate hexahydrate in step (1) is replaced by CeCl3·7H2O, the other contents are consistent with those in Example 1. The synthesis results are shown in FIG. Fig. 10A As shown, Fig. 10A On the left is a picture of all the raw materials mixed before the reaction; Fig. 10A The right side is a picture of the product after the reaction. It can be seen that there is no obvious change before and after the reaction, and it is found that no product is synthesized.
[0179] Comparative Example 9
[0180] Except for replacing acetic acid with formic acid in step (2), other contents are consistent with Example 1. It is found that after adding formic acid, the synthesized cerium oxide is severely aggregated and irregular in morphology, which is quite different from the uniform nanospheres in Example 1, and the antioxidant property is poor.
[0181] Comparative Example 10
[0182] Except that the ethylene glycol in step (4) is replaced by propylene glycol, the other contents are consistent with those in Example 1. Fig. 10B As shown, Fig. 10B On the left is a picture of all the raw materials mixed before the reaction; Fig. 10B The right side shows the product after the reaction. It can be seen that only the color changes after the reaction, but no precipitate is produced, that is, no cerium oxide is generated.
[0183] Efficacy experiments of the present invention
[0184] 1. Transmission electron microscopy results of cerium oxide
[0185] 1. Test method: In order to observe the morphology and size of the synthesized pure CeO2 of comparative example 1 and Zn / CeO2 of embodiment 5, a JEOL JEM-F200 transmission electron microscope was used for transmission electron microscopy (TEM) characterization. After the sample was ultrasonically dispersed in ethanol, it was dripped onto a copper mesh with a carbon film by a capillary pipette, and the transmission electron microscope effect diagram of the sample was observed. In the transmission electron microscope effect diagram of each sample, 100 nanospheres with clear outlines were selected, and after the diameter of the nanospheres was annotated with Image J software, the diameter distribution diagram of the nanospheres was statistically analyzed and drawn.
[0186] 2. Transmission electron microscopy results: Figure 1 , Figure 2A and Figure 2B As shown, Figure 1 a is pure CeO2 nanosphere, which can be seen as a solid sphere, and b is the Zn / CeO2 prepared by the present invention, which is a hollow sphere morphology; the particle size of pure CeO2 nanosphere is mainly concentrated around 115nm. The particle size of Zn / CeO2 prepared by the present invention is mainly concentrated around 90nm, and it is observed that the particle size of cerium oxide nanospheres is significantly reduced after doping.
[0187] 2. Cerium Oxide I CP Results
[0188] 1. Test method: In order to test the mass concentration of zinc ions actually doped into cerium oxide after the reaction under different addition amounts of anhydrous zinc chloride, the concentration is determined by plasma emission spectrometer. Before the test, the sample needs to be digested. A certain amount of sample dispersion is transferred into a 10mL colorimetric tube, and 2mL nitric acid and a few drops of 30% hydrogen peroxide are added to it. Slightly shake and mix evenly. After mixing, place it in a water bath and gradually heat it to boiling, and digest it for about 2 hours. After the digestion is completed, cool it to room temperature and then dilute it to 10mL for standby use.
[0189] 2. Test results: It can be seen from the test results in Table 3 that the addition of zinc ions in the range of 0.1mol% to 40mol% is feasible. When the amount of zinc ion added is small, the actual zinc doping amount gradually increases. When the zinc ion is added at 5mol%, the actual zinc doping amount growth rate is significantly improved. At this time, the actual zinc doping amount is 0.746wt%. After that, the actual zinc doping amount increases slowly, and the maximum actual zinc doping amount is about 1wt%. This shows that with the increase of the doping amount, the actual doping amount tends to saturation, especially after the zinc ion addition amount is 30mol%, the actual doping amount does not increase significantly, and is still about 1wt%, which can be approximately regarded as the maximum doping amount of 1wt%. This also shows that the amount of anhydrous zinc chloride and the actual zinc doping amount are not monotonically increasing. When the zinc ion addition amount exceeds 40mol%, simply increasing the amount of anhydrous zinc chloride cannot increase the actual zinc doping amount infinitely, and the actual zinc doping amount has a saturation value. From the perspectives of raw material cost control and actual doping amount, it is more appropriate to select the range of zinc ion addition as 0.1mol% to 40mol%.
[0190] Table 3 ICP results of Zn / CeO2 nanospheres
[0191]
[0192] 3. DPPH free radical scavenging effect
[0193] DPPH (1,1-disphenyl-2-picryl-hydrazyl), chemically named 1,1-diphenyl-2-trinitrophenylhydrazine, has a molecular formula of (C6H5)2N-NC6H2(NO2)3. In this compound, there is an unpaired valence electron on one atom of the nitrogen bridge, and the orbital motion of this electron is almost offset by the molecular structure. The capture of DPPH free radicals is usually used as an indicator for assessing antioxidant capacity. DPPH is a stable organic free radical with a maximum absorption peak of 517nm in the visible light region. In ethanol solution, each DPPH molecule can generate a stable nitrogen-containing free radical in the solution with a typical purple color. When it acts with a free radical scavenger that provides 1 electron (for example, cerium oxide dispersion), a yellow product is generated, which makes the typical purple color of the solution lighter. The degree of fading is stoichiometrically related to the number of paired electrons. Therefore, spectrophotometry can be used for quantitative analysis to detect the free radical scavenging situation, thereby evaluating the free radical scavenging ability of the sample. The reaction process of cerium oxide dispersion to scavenging DPPH is as follows:
[0194]
[0195] 1. Instruments and Reagents
[0196] Note: ① The brands and models marked in brackets for equipment are those used during laboratory method development, and are not exclusive. ② The brands, specifications, and other information commonly used in laboratories are marked in brackets for reagents and consumables, and are not exclusive.
[0197] (1) Analytical balance (d = 0.1 mg, Sartorius, BSA2202S-CW, Max 220 g);
[0198] (2) Constant temperature water bath (Gongyi Hua Instrument Co., Ltd., HH-S2);
[0199] (3) Ultraviolet spectrophotometer (Agilent, Cary 60UV-Vis) and matching cuvette;
[0200] (4) Pipette (5 mL, 200 μL, 1000 μL, Eppendorf) and matching tips;
[0201] (5) DPPH (sigma, analytical grade, C 18 H 12 N5O6, molecular weight 394.32);
[0202] (6) Centrifuge (ThermoFisher, Pico 21);
[0203] (7) Anhydrous ethanol (Sinopharm Chemical Reagent Co., Ltd., analytical grade);
[0204] (8) Deionized water.
[0205] 2. Experimental Preparation
[0206] 2.1 Reagent preparation
[0207] (1) 0.2mmol / L DPPH solution
[0208] Weigh 0.0200 g of DPPH, add anhydrous ethanol to dissolve and dilute to volume in a 250 mL volumetric flask, and shake well.
[0209] (2) Pure cerium oxide dispersion
[0210] Take 50 mg of pure cerium oxide sample, disperse it in 10 mL of deionized water, and disperse it by ultrasonic for 30 minutes. Shake it well to obtain a 0.5 wt % cerium oxide dispersion, which is diluted to 0.3 wt % and 0.1 wt % concentration for later use.
[0211] (3) Zinc ion doped cerium oxide dispersion
[0212] Take 50 mg of zinc ion-doped cerium oxide sample, disperse it in 10 mL of deionized water, and ultrasonically disperse it for 60 minutes. Shake it well to obtain a 0.5 wt % cerium oxide dispersion, which is diluted to 0.3 wt % and 0.1 wt % concentrations for later use.
[0213] 2.2 Preparation of reagents and consumables
[0214] Before starting the test, prepare the prepared test solution, anhydrous ethanol, DPPH diluent, pipette and pipette tip in front of the EP tube rack. Turn on the UV spectrophotometer and preheat it for more than 30 minutes in advance to allow the instrument to reach a stable state.
[0215] 3. Test operation
[0216] Mix the same amount of the test solution with the DPPH solution as group A (sample group); mix the same amount of anhydrous ethanol with the DPPH solution as group B (control group); mix the same amount of anhydrous ethanol with the test solution as group C (blank group). After reacting for 30 minutes at room temperature and in the dark, measure the absorbance of each group of solutions at 517nm. Note: In order to exclude the possible influence of CeO2 particles on the absorbance measurement, all solutions in the experimental group (group A) and the blank group (group C) were centrifuged at 10,000 rpm for 10 minutes, and then the absorbance of the supernatant was measured.
[0217] 4. Result processing
[0218] DPPH free radical scavenging rate calculation formula: Scavenging rate = [(B + C) - A] / B * 100%
[0219] Where:
[0220] A—Absorbance value after mixing the sample solution with the DPPH solution
[0221] B—Absorbance value after mixing anhydrous ethanol and DPPH solution
[0222] C—Absorbance value after mixing anhydrous ethanol and sample solution.
[0223] 5. Results Analysis
[0224] In order to compare the DPPH radical scavenging ability of pure CeO2 nanospheres and Zn / CeO2 nanospheres, we tested the DPPH radical scavenging rate of zinc ion-doped cerium oxide at three concentrations: pure cerium oxide (Comparative Example 1), 1 mol% (Example 2), 5 mol% (Example 4), 10 mol% (Example 5) and 20 mol% (Example 6).
[0225] Depend on Figure 3As can be seen from the results of Table 4, with the increase of cerium oxide concentration, the DPPH radical scavenging rates of pure cerium oxide and cerium oxide doped with zinc ions gradually increase. When the cerium oxide concentration is 0.1wt%, the DPPH radical scavenging rates of pure cerium oxide, 1mol%, 5mol%, 10mol% and 20mol% zinc ion doped cerium oxide are 50.64%, 48.67%, 47.40%, 57.23% and 47.96% respectively, and when the cerium oxide concentration is 0.3wt%, the scavenging rate has approached the peak value, which is 95.14%, 91.75%, 92.49%, 93.88% and 92.90% respectively. By comparing the DPPH radical scavenging rates of pure cerium oxide and cerium oxide doped with zinc ions, it can be found that doping with zinc ions does not affect the scavenging of DPPH radicals by cerium oxide. After doping with zinc ions, cerium oxide still has good antioxidant capacity. A suitable concentration of 0.25% was selected to compare the DPPH scavenging rates of all the examples and the comparative examples as the main criterion for judging the antioxidant capacity. It was found that the DPPH free radical scavenging rates of the comparative examples 1 to 7 were slightly lower than those of the examples, and the scavenging rate of the comparative example 9 was very low, and the antioxidant effect was weak.
[0226] Table 4 DPPH free radical scavenging results of 0.25% dispersion of Examples and Comparative Examples
[0227]
[0228] 4. Hydroxyl free radical scavenging effect
[0229] Hydroxyl radical (·OH) is an important reactive oxygen species that can react quickly with other molecules to become a more stable form. This method uses the reaction of FeSO4·7H2O and H2O2 to generate hydroxyl radical (·OH). The reaction of salicylic acid with the hydroxyl radical (·OH) generated by the Fenton reaction will generate 2.3-dihydroxybenzoic acid with a maximum absorption wavelength at 510nm. If a substance with the ability to scavenge hydroxyl radicals is added to the reaction system, the formation of 2,3-dihydroxybenzoic acid can be inhibited. The fixed reaction time method is used to detect the change in absorbance at 510nm using an enzyme marker to detect the antioxidant capacity of the added substance.
[0230] 1. Instruments and Reagents
[0231] Note: ① The brands and models marked in brackets for equipment are those used during laboratory method development, and are not exclusive. ② The brands, specifications, and other information commonly used in laboratories are marked in brackets for reagents and consumables, and are not exclusive.
[0232] (1) Analytical balance (d = 0.1 mg, Sartorius, BSA2202S-CW, Max 220 g);
[0233] (2) Vortex mixer (MX-F);
[0234] (3) Multifunctional microplate reader (Thermo scientific), 96-well plate (Corning);
[0235] (4) Pipette (5 mL, 200 μL, 1000 μL, Eppendorf);
[0236] (5) High-speed centrifuge (Thermo scientific);
[0237] (6) Salicylic acid (MACKLIN);
[0238] (7) Anhydrous ethanol (Tianjin Damao Chemical Reagent Factory);
[0239] (8) Ferrous sulfate (Sinopharm Chemical Reagent Co., Ltd.);
[0240] (9) Hydrogen peroxide (MREDA).
[0241] 2. Experimental Preparation
[0242] 2.1 Reagent preparation
[0243] (1) 9mmol / L salicylic acid-ethanol solution
[0244] Take 0.124 g of salicylic acid, dissolve it in anhydrous ethanol and make up to 100 mL.
[0245] (2) 9mmol / L ferrous sulfate solution
[0246] Take 0.2502 g of ferrous sulfate heptahydrate, dissolve it in distilled water and make up to 100 mL.
[0247] (3) 8.8mmol / L hydrogen peroxide solution
[0248] Take 9.926g of 30% H2O2 solution and add distilled water to make up to 100mL; then take 1mL of the solution after the volume is adjusted to a 100mL volumetric flask and add water to make up to 100mL.
[0249] (4) Sample solution
[0250] Take 100 mg of the sample to be tested, disperse it in 10 mL of deionized water, disperse it by ultrasonic for 60 minutes, and shake it well to obtain a 1 wt% sample solution, which is then diluted to 0.5 wt%, 0.25 wt%, and 0.125 wt% concentrations for later use.
[0251] 2.2 Preparation of reagents and consumables
[0252] Before starting the test, prepare the prepared test solution, 9mmol / L ferrous sulfate solution, 9mmol / L salicylic acid-ethanol solution, 8.8mmol / L hydrogen peroxide solution, distilled water, pipette and pipette tip in front of the EP tube rack.
[0253] 3. Test operation
[0254] Different solutions were added to a 1.5 mL centrifuge tube in the order from top to bottom in the following table, as shown in Table 5.
[0255] Table 5
[0256]
[0257] After adding in order, mix and shake well, heat in a 37℃ water bath for 15 minutes and then take out. Pipette 200μL of each solution and measure the absorbance at 510nm. Note: In order to prevent the CeO2 particles in the solution from affecting the absorbance measurement, A X and A X0 All the solutions were centrifuged at 10,000 rpm for 10 min, and the absorbance of the supernatant was measured. The scavenging rate (R, %) of hydroxyl radicals was calculated according to the following formula.
[0258] 4. Result processing
[0259] The calculation formula of hydroxyl free radical scavenging rate is: scavenging rate R = 1-(A X -A X0 ) / A0×100%
[0260] Where:
[0261] A0—Absorbance value after mixing ferrous sulfate solution, salicylic acid-ethanol solution and H2O2 solution
[0262] A X —Absorbance value after the sample solution is mixed with ferrous sulfate solution, salicylic acid-ethanol solution, H2O2 solution and distilled water
[0263] A X0 —Absorbance value after the sample solution is mixed with ferrous sulfate solution, salicylic acid-ethanol solution and distilled water.
[0264] 5. Results Analysis
[0265] In order to compare the hydroxyl radical scavenging ability of pure CeO2 nanospheres and Zn / CeO2 nanospheres, we tested the hydroxyl radical scavenging rate of zinc ion-doped cerium oxide at four concentrations: pure cerium oxide (Comparative Example 1), 1 mol% (Example 2), 5 mol% (Example 4), 10 mol% (Example 5) and 20 mol% (Example 6).
[0266] Depend on Figure 4 The results show that with the increase of cerium oxide concentration, the hydroxyl radical scavenging rates of pure cerium oxide and cerium oxide doped with zinc ions gradually increase. When the cerium oxide concentration is 0.125wt%, the hydroxyl radical scavenging rates of pure cerium oxide, 1mol%, 5mol%, 10mol% and 20mol% zinc ion doped cerium oxide are 44.59%, 39.44%, 50.16%, 48.63% and 49.90%, respectively, while when the cerium oxide concentration is 1wt%, the scavenging rates are 67.81%, 64.18%, 65.04%, 65.61% and 61.17%, respectively. By comparing the hydroxyl radical scavenging rates of pure cerium oxide and cerium oxide doped with zinc ions, it can be found that doping with zinc ions does not affect the scavenging of hydroxyl radicals by cerium oxide. After doping with zinc ions, cerium oxide still has good antioxidant capacity.
[0267] 5. Superoxide anion free radical scavenging effect
[0268] Superoxide anion (O 2- ) is a kind of reactive oxygen, which is the product of oxygen molecules in cells being reduced by a single electron. It can diffuse through cells, participate in numerous physiological activities such as cell proliferation and apoptosis, and play an important role in the redox metabolism of cells. This method utilizes pyrogallol to undergo self-oxidation under alkaline conditions. When superoxide anions are produced, a characteristic absorption peak will appear near 325nm, and superoxide anions can further promote the oxidation of pyrogallol. As the oxidation reaction goes deeper, the absorption of this peak gradually becomes stronger. After the superoxide anions produced are removed, the reaction is suppressed, and its absorption near 325nm will be reduced. Therefore, the amount of superoxide anions in the solution can be judged according to the change of the characteristic absorption peak near 325nm, thereby judging the scavenging effect of antioxidants on superoxide anions.
[0269] 1. Instruments and Reagents
[0270] Note: ① The brands and models marked in brackets for equipment are those used during laboratory method development, and are not exclusive. ② The brands, specifications, and other information commonly used in laboratories are marked in brackets for reagents and consumables, and are not exclusive.
[0271] (1) Analytical balance (d = 0.1 mg, Sartorius, BSA2202S-CW, Max 220 g);
[0272] (2) Vortex mixer (MX-F);
[0273] (3) Multifunctional microplate reader (Thermo scientific), 96-well plate (jet)
[0274] (4) Pipette (5 mL, 200 μL, 1000 μL, Eppendorf);
[0275] (5) High-speed centrifuge (Thermo scientific);
[0276] (6) Pyrogallol (Beijing Bio-Toda Technology Co., Ltd., analytical grade, C6H6O3, molecular weight 126.11);
[0277] (7) Tris (Beijing Bio-Toda Technology Co., Ltd., analytical grade, C4H 11 NO3, molecular weight 121.14);
[0278] (8) Concentrated hydrochloric acid (Modern Oriental (Beijing) Science and Technology Development Co., Ltd., analytical grade).
[0279] 2. Experimental Preparation
[0280] 2.1 Reagent preparation
[0281] (1) 0.1 mol / L HCl solution
[0282] Weigh 2.1 ml of concentrated hydrochloric acid, add deionized water to a 250 mL volumetric flask, and shake well.
[0283] (2) 50mmol / L Tris-HCl solution
[0284] Weigh 0.6057g Tris and dissolve it in deionized water. Add 22.9ml 0.1mol / L HCL solution and dilute to 100mL volumetric flask with deionized water and shake well.
[0285] (3) 0.3mmol / L pyrogallol solution
[0286] Take 7.5666 mg of pyrogallol solution, add 0.01 mol / L HCL solution to dissolve, make up to volume in a 100 mL volumetric flask, and shake well.
[0287] (4) Sample solution
[0288] Take 25 mg of the sample to be tested, disperse it in 10 mL of deionized water, ultrasonically disperse it for 60 minutes, and shake it well to obtain a 0.25 wt% sample solution, which is then diluted to 0.125 wt%, 0.0625 wt%, and 0.03125 wt% concentrations for later use.
[0289] 2.2 Preparation of reagents and consumables
[0290] Before starting the experiment, prepare the prepared test solution, 0.1mol / L HCL solution, 50mmol / L Tris-HCL solution, 0.3mmol / L pyrogallol solution, pipette and pipette tip in front of the EP tube rack.
[0291] 3. Test operation
[0292] Add 500 μL Tris-HCl buffer and 100 μL pyrogallol solution to a 1.5 mL centrifuge tube, mix and shake, and place in a 37°C water bath for 10 min. Then add 100 μL sample solution, react for 5 min, and terminate the reaction with 100 μL 0.1 mol / L HCL solution. Measure the absorbance of each group of solutions at 320 nm. Note: In order to prevent the CeO2 particles in the solution from affecting the absorbance measurement, A i and A j All the solutions were centrifuged at 10,000 rpm for 10 min, and the absorbance of the supernatant was measured. The clearance rate (R, %) of superoxide anions was calculated according to the following formula.
[0293] 4. Result processing
[0294] The calculation formula of superoxide anion free radical scavenging rate is: scavenging rate R = 1-(A i -A j ) / A0*100%
[0295] Where:
[0296] A i —Absorbance value after the sample solution is mixed with Tris-HCl solution, pyrogallol solution and 0.1 mol / L HCl solution
[0297] A j —Absorbance value after the sample solution is mixed with Tris-HCl solution, deionized water and 0.1 mol / L HCl solution
[0298] A0—Absorbance value after mixing deionized water with Tris-HCL solution, pyrogallol solution and 0.1 mol / L HCL solution.
[0299] 5. Results Analysis
[0300] In order to compare the superoxide anion radical scavenging ability of pure CeO2 nanospheres and Zn / CeO2 nanospheres, we tested the superoxide anion radical scavenging rate of pure cerium oxide (Comparative Example 1), 1 mol% (Example 2), 5 mol% (Example 4), 10 mol% (Example 5) and 20 mol% (Example 6) zinc ion-doped cerium oxide at four concentrations.
[0301] Depend on Figure 5 The results show that with the increase of cerium oxide concentration, the superoxide anion radical scavenging rate of pure cerium oxide and cerium oxide doped with zinc ions gradually increases. When the cerium oxide concentration is 0.03125wt%, the superoxide anion radical scavenging rates of pure cerium oxide, 1mol%, 5mol%, 10mol% and 20mol% zinc ion doped cerium oxide are 79.77%, 75.59%, 74.85%, 82.42% and 77.37%, respectively. When the cerium oxide concentration is 0.125wt%, the scavenging rate approaches the peak value, and the scavenging rates are 97.98%, 93.69%, 95.25%, 97.49% and 99.85%, respectively. By comparing the superoxide anion radical scavenging rates of pure cerium oxide and cerium oxide doped with zinc ions, it can be found that doping with zinc ions does not affect the scavenging of superoxide anion radicals by cerium oxide. After doping with zinc ions, cerium oxide still has good antioxidant capacity.
[0302] VI. Study on Antibacterial Activity
[0303] 1. Instruments and Reagents
[0304] Note: The test site, test instruments, bacterial strains and culture media used in this experiment were all provided by the Beijing Beinong Testing Center of Beijing Beinong Technology Co., Ltd.
[0305] (1) Bacterial strains: Escherichia coli (ATCC 25922) and Staphylococcus aureus (ATCC 6538) were purchased from China Industrial Microbiological Culture Collection Center;
[0306] (2) Culture medium: nutrient agar (Qingdao Haibo Biotechnology Co., Ltd.);
[0307] (3) Instruments: biological safety cabinet, clean bench, analytical balance, vortex mixer, 1000 μL pipette and matching tips, centrifuge tubes, test tubes (with matching rubber stoppers), culture dishes, alcohol lamps, 1L conical flasks, biochemical incubators, water baths, shakers, tweezers, and medicine spoons;
[0308] (4) Reagents: sodium chloride (aladdin), McFarland turbidimetric tube (Beekman).
[0309] 2. Test preparation and operation
[0310] 2.1 Culture medium preparation
[0311] Weigh 4.6 g of NA dry powder into a conical flask, add 200 mL of distilled water and disperse evenly, sterilize the conical flask with high-pressure steam (121°C, 15 min), and then pour the solid culture medium into disposable culture dishes (90 mm in diameter) at 50°C in a biological safety cabinet. After cooling, it becomes an agar plate; seal it with sealing film and refrigerate at 4°C for later use.
[0312] 2.2 Bacterial recovery
[0313] Take out the frozen Staphylococcus aureus and Escherichia coli and thaw them in a 37°C constant temperature incubator. Heat the bacterial inoculation loop on an alcohol lamp until it turns red, dip it in the bacterial solution after cooling, and make continuous "Z"-shaped lines on the agar plate. Mark the two agar plates with lines and transfer them to a 37°C constant temperature incubator for incubation for 24 hours. Take out the streaked agar plate, and after obvious colony formation is observed, transfer it to a biosafety cabinet and continue to subculture overnight. Afterwards, prepare two 20mL test tubes, add 3mL of normal saline to each, pick up a single colony with a pipette tip and add it to a centrifuge tube, mix it thoroughly with a rotary mixer to obtain the initial bacterial solution. The bacterial concentration of the bacterial solution is on the order of 10 8 cfu / mL (McFarland turbidity).
[0314] 2.3 Preparation of bacterial suspension
[0315] Take 1 mL of the initial bacterial solution in a 20 mL test tube, add 9 mL of saline, mix thoroughly and record as 10 7 cfu / mL bacterial solution, prepared in the same way, and diluted to 10 5 cfu / mL for future use.
[0316] 2.4 Sample preparation and sterilization
[0317] Prepare dispersions of different concentrations for the samples: weigh 25 mg of the sample to be tested, disperse it in 10 mL of physiological saline, ultrasonically disperse it for 60 minutes, and shake it well to obtain a 0.25 wt% sample solution. Dilute it to 0.125 wt%, 0.0625 wt%, 0.03125 wt% and 0.0156 wt% concentrations for later use. Sterilize the samples of the required concentrations with high-pressure steam (121°C, 15 min). After sterilization is completed and the solution is cooled to room temperature, transfer it to a biosafety cabinet. Transfer all samples to test tubes in order, and add 5 mL to each test tube.
[0318] 2.5 Add bacterial solution for co-cultivation
[0319] The prepared 10 5 cfu / mL bacterial solution was thoroughly mixed with a rotary mixer and repeatedly pipetted. 250uL bacterial solution was added to each sample in the test tube, and a control group (bacterial solution + saline) was set up at the same time. All test tubes were transferred to a 37℃ constant temperature incubator and incubated for 24h.
[0320] 2.6 Preparation of secondary culture medium
[0321] Weigh 4.6 g of NA dry powder into a conical flask, add 200 mL of distilled water to disperse evenly, sterilize the conical flask with high-pressure steam (121°C, 15 min), and immediately put it in a 46°C water bath to keep the agar in a liquid state.
[0322] 2.7 Dilution after incubation
[0323] After the incubation is completed, disinfect the surface of the well plate with alcohol and transfer it to the biosafety cabinet. Take 1ml from each tube of the sample group and the positive control group, and dilute it with 9ml of saline. Pipette 1ml from each test tube into a blank culture dish, pour in appropriate nutrient agar and mix well. Make three parallel groups for each test tube. After the mixed agar plate cools down, invert it in a 37℃ constant temperature incubator and culture it for 24h to 40h.
[0324] 2.8 Colony count and antibacterial rate calculation
[0325] Take out the agar plate and observe the colonies with naked eyes. Count the colonies according to the corresponding sample number and dilution multiple. The formula for calculating the antibacterial rate is as follows:
[0326]
[0327] 3. Results Analysis
[0328] In order to compare the antibacterial properties of pure CeO2 nanospheres and Zn / CeO2 nanospheres against Staphylococcus aureus, we selected three sample concentrations (0.0156%, 0.03125%, 0.0625%) and co-cultured with Staphylococcus aureus for 24 hours. After that, the bacterial solution was diluted and plated, and the number of remaining colonies was counted to calculate the antibacterial rate.
[0329] Depend on Figure 6 It can be seen that after the sample was co-cultured with Staphylococcus aureus for 24 hours, compared with the control group without cerium oxide, the number of remaining colonies in the pure cerium oxide group gradually decreased with the increase of cerium oxide concentration, indicating that it has an antibacterial effect and the antibacterial effect gradually increases; while 10 mol% Zn 2+ The number of residual colonies in the cerium oxide-doped group was less, and the antibacterial effect was better than that in the pure cerium oxide group. Fig. 7A The antibacterial rate bar graph shown in Figure 2 can also verify this. At the same time, the cerium oxide concentration was set to 0.03125% to compare the antibacterial rates of cerium oxide with different zinc doping amounts. The results are as follows: Figure 7B shown. Figure 7B It shows that doping with different concentrations of zinc ions will affect its antibacterial rate. As the concentration of doped zinc ions increases, the antibacterial rate tends to increase. 2+ The antibacterial effect of cerium oxide is the best, with an antibacterial rate of 99.52%.
[0330] In addition, in order to compare the antibacterial properties of pure CeO2 nanospheres and Zn / CeO2 nanospheres against Escherichia coli, we selected three sample concentrations (0.03125%, 0.0625%, 0.125%) and co-cultured them with Escherichia coli for 24 hours. After that, the bacterial solution was diluted and plated, and the number of remaining colonies was counted to calculate the antibacterial rate.
[0331] Depend on Figure 8 It can be seen that after the sample was co-cultured with Escherichia coli for 24 hours, compared with the control group without cerium oxide, the number of remaining colonies in the pure cerium oxide group gradually decreased with the increase of cerium oxide concentration, indicating that it has an antibacterial effect and the antibacterial effect gradually increases; while 10 mol% Zn 2+ The number of remaining colonies in the cerium oxide-doped group was less and the antibacterial effect was better than that in the pure cerium oxide group. Fig.9A The antibacterial rate bar graph can also verify this. At the same time, the cerium oxide concentration was set to 0.0625% to compare the antibacterial rates of cerium oxide with different zinc doping amounts. The results are as follows: Fig. 9B As shown, Fig. 9B It shows that doping with different concentrations of zinc ions will affect its antibacterial rate. As the concentration of doped zinc ions decreases, the antibacterial rate tends to decrease. 2+ The antibacterial effect of cerium oxide is the best, with an inhibition rate of 99.46%.
[0332] From the antibacterial experiments on Escherichia coli and Staphylococcus aureus of the control group and the embodiment, it can be seen that the zinc ion doping concentration in cerium oxide shows antibacterial efficacy above 0.2 mol%, and the antibacterial rate is greater than 80% when it is 0.5 mol% to 20 mol%, and the antibacterial effect is better than that of the control group (undoped). Therefore, considering the influence of four aspects, namely, the actual doping amount, raw material cost control, antioxidant capacity and antibacterial capacity, the doping amount of zinc ions is finally selected to be more appropriate in the range of 0.1 mol% to 40 mol%, among which 0.5 mol% to 20 mol% is better.
Claims
1. A method for preparing a zinc ion-doped cerium oxide nanocomposite material, characterized in that The steps include: (1) fully dissolving a cerium-containing precursor in water to prepare a precursor solution; the cerium-containing precursor is cerium nitrate hexahydrate; the concentration of the cerium-containing precursor is 0.5 g / mL to 1.5 g / mL; (2) adding a pH adjuster to prepare a first solution; (3) adding a zinc ion-containing preparation to the first solution and mixing thoroughly to prepare a second solution doped with zinc ions; (4) adding a dispersion medium to the second solution and stirring the mixture to obtain a third solution; (5) heating the third solution to react; (6) Wash the product obtained in step (5) with water, centrifuge, and dry.
2. The method for preparing the zinc ion-doped cerium oxide nanocomposite material according to claim 1, wherein: In the step (2), the pH adjuster is one or more of acetic acid and propionic acid.
3. The method for preparing the zinc ion-doped cerium oxide nanocomposite material according to claim 2, characterized in that: The mass ratio of the cerium-containing precursor to the pH adjuster is 16-19.9:16-20.
4. The method for preparing the zinc ion-doped cerium oxide nanocomposite material according to claim 1, characterized in that: In the step (3), the zinc ion-containing agent is one or more of zinc chloride and zinc nitrate hexahydrate, and the molar ratio of zinc ions to cerium ions in the second solution is 0.1 mol% to 40 mol%.
5. The method for preparing the zinc ion-doped cerium oxide nanocomposite material according to claim 1, characterized in that: The dispersion medium in step (4) is ethylene glycol.
6. The method for preparing the zinc ion-doped cerium oxide nanocomposite material according to claim 5, characterized in that: The mass volume ratio of the cerium-containing precursor to ethylene glycol is 16-19.9 g: 600-700 mL.
7. The method for preparing the zinc ion-doped cerium oxide nanocomposite material according to claim 1, characterized in that: In the step (5), the heating reaction includes one or more of the following conditions a) to b): a) the temperature of the heating reaction is 160°C to 190°C; b) The heating reaction time is 120 min to 200 min.
8. A zinc ion doped cerium oxide nanocomposite material, characterized in that Prepared by the method according to any one of claims 1 to 7.
9. Use of the zinc ion-doped cerium oxide nanocomposite material according to claim 8 in the preparation of cosmetics, cosmetic additives, external medicines and / or external medicine additives.
10. A cosmetic, characterized in that A zinc ion-doped cerium oxide nanocomposite material comprising the zinc ion-doped cerium oxide nanocomposite material according to claim 8.