Developable soft tissue repair patch as well as preparation method and application thereof
Through the combination of polypropylene, modified bismuth trioxide and xanthan gum, a developable soft tissue repair patch with high mechanical properties is prepared, which solves the problems of difficult evaluation and insufficient mechanical properties of existing materials after implantation, and achieves Improved imaging performance and safety, suitable for soft tissue repair and regeneration support.
Patent Information
- Application Number
- CN202410886331.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-29
AI Technical Summary
It is difficult to evaluate the later state of existing soft tissue repair materials after implantation. They have poor mechanical properties and are prone to fracture and recurrence, affecting patient safety and efficacy.
Polypropylene, methylcellulose-modified bismuth trioxide and trace amounts of xanthan gum are used to control the proportion and particle size of the components through the preparation method, improve the dispersion and cross-linking of the developer, enhance the mechanical properties of the patch, and A porous network patch is prepared through a weaving process.
A developable soft tissue repair patch with high bursting strength, high tensile strength, and high safety has been obtained. The development effect is clear and non-cytotoxic. It is suitable for soft tissue repair and supports tissue regeneration and rapid recovery.
Smart Images

Figure BDA0004926152950000071 
Figure BDA0004926152950000081 
Figure BDA0004926152950000082
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of medical materials, and in particular to a developable soft tissue repair patch and a preparation method and application thereof. Background Art
[0002] Soft tissue is a relatively important human tissue, which refers to the human skin, subcutaneous tissue, muscles, tendons, ligaments, joint capsules, synovial capsules, nerves, blood vessels, etc. At present, soft tissue damage caused by pathological changes or trauma seriously threatens human health and has become one of the common clinical diseases.
[0003] In recent years, the use of soft tissue repair materials to repair and replace damaged soft tissues in the body and to restore or partially restore the original tissue morphology and function has become an important method for treating soft tissue injuries.
[0004] However, it is impossible to observe the later state of soft tissue repair materials after implantation in patients, making it difficult to evaluate surgical positioning and postoperative degradation and healing effects. Therefore, it is urgent to provide a developable soft tissue repair material. In addition, the existing patches have poor mechanical properties, and the patches are prone to breakage and recurrent tearing, which is not conducive to the patient's postoperative safety and long-term efficacy. Summary of the invention
[0005] In order to obtain a developable soft tissue repair patch with excellent mechanical properties, the present application provides a developable soft tissue repair patch and a preparation method and application thereof.
[0006] In a first aspect, the present application provides a developable soft tissue repair patch.
[0007] A developable soft tissue repair patch adopts the following technical solution: A developable soft tissue repair patch is composed of the following components in parts by weight: 80-90 parts of polypropylene; 8-14 parts of modified bismuth trioxide; 0.2-0.4 parts of xanthan gum; Wherein, the modified bismuth trioxide is obtained by modifying bismuth trioxide with methyl cellulose.
[0008] The present application utilizes polypropylene as the main body, adds methylcellulose-modified bismuth trioxide as a developer, and simultaneously adds a trace amount of xanthan gum as a functional additive, so as to obtain a developable soft tissue repair patch with high bursting strength, high tensile strength, high safety, and clear developing effect.
[0009] The polypropylene used in this application has good flexibility and durability, is suitable for preparing medical soft tissue repair patches, and can provide excellent mechanical properties for developable soft tissue repair patches. The methylcellulose used in this application has rich methoxy groups. After modifying bismuth trioxide, the dispersibility of the developer is improved, the surface energy of the developer is reduced, and it is beneficial to reduce the agglomeration of the developer; at the same time, the developer is given a certain cross-linking property, which is beneficial to the bonding strength between the developer and the polypropylene, and enhances the mechanical properties of the soft tissue repair patch. Xanthan gum has a certain viscosity, which is beneficial to further enhance the mechanical properties of the soft tissue repair patch. In addition, the methylcellulose and xanthan gum used in this application are both biomaterials, which are used to prepare soft tissue repair patches and are non-cytotoxic.
[0010] Preferably, the developable soft tissue repair patch is composed of the following components in parts by weight: 85-90 parts of polypropylene; 8-12 parts of modified bismuth trioxide; and 0.25-0.35 parts of xanthan gum.
[0011] In a specific embodiment, the added amount of the polypropylene can be 80 parts, 85 parts, or 90 parts.
[0012] In some specific embodiments, the added amount of the polypropylene can also be 80-85 parts.
[0013] In a specific embodiment, the added amount of the modified bismuth trioxide can be 8 parts, 12 parts, or 14 parts.
[0014] In some specific embodiments, the added amount of the modified bismuth trioxide can also be 12-14 parts.
[0015] In a specific embodiment, the added amount of xanthan gum can be 0.2 parts, 0.25 parts, 0.3 parts, 0.35 parts, or 0.4 parts.
[0016] In some specific embodiments, the added amount of xanthan gum can also be 0.2-0.25 parts, 0.2-0.3 parts, 0.2-0.35 parts, 0.25-0.3 parts, 0.25-0.4 parts, 0.3-0.35 parts, 0.3-0.4 parts, 0.35-0.4 parts.
[0017] Through experimental analysis, it can be known that when the addition amount of each raw material component is controlled within the above range, the mechanical properties of the developable soft tissue repair patch can be further improved without reducing the developing effect of the soft tissue repair patch.
[0018] Preferably, in the modified bismuth trioxide, the weight ratio of the methyl cellulose to the bismuth trioxide is (2-6):20.
[0019] In a specific embodiment, the weight ratio of the methyl cellulose to the bismuth trioxide can be 2:20, 4:20, or 6:20.
[0020] In some specific embodiments, the weight ratio of the methyl cellulose to the bismuth trioxide can also be (2-4):20 or (4-6):20.
[0021] Through experimental analysis, it can be known that when the addition amount of each raw material component is controlled within the above range, the mechanical properties of the developable soft tissue repair patch can be further improved, and a better development effect can be achieved.
[0022] Preferably, the viscosity of the methyl cellulose is 400-4000 cp.
[0023] Furthermore, the viscosity of the methyl cellulose is 1000-2000cp.
[0024] In some specific embodiments, the viscosity of the methylcellulose may be 400 cp, 1000 cp, 1500 cp, 2000 cp, or 4000 cp.
[0025] In a specific embodiment, the viscosity of the methyl cellulose may also be 400-1000 cp, 400-1500 cp, 400-2000 cp, 1000-1500 cp, 1000-4000 cp, 1500-2000 cp, 1500-4000 cp, or 2000-4000 cp.
[0026] Through experimental analysis, it can be known that when the addition amount of each raw material component is controlled within the above range, the mechanical properties of the developable soft tissue repair patch can be further improved, and a better development effect can be achieved.
[0027] Preferably, the particle size of the bismuth trioxide is 100-600 nm.
[0028] Through experimental analysis, it can be known that when the particle size of bismuth trioxide is controlled within the above range, the mechanical properties of the developable soft tissue repair patch can be further improved.
[0029] Preferably, the preparation method of the modified bismuth trioxide is: The methyl cellulose is dissolved in a mixed solvent of toluene and water at a temperature of 100-120° C. to obtain a methyl cellulose solution with a concentration of 3-5wt%; then the bismuth trioxide is added to the methyl cellulose solution and stirred and refluxed for 60-90 minutes; after the reaction is completed, the reaction solution is vacuum dried to obtain the modified bismuth trioxide.
[0030] Preferably, the volume ratio of the toluene to the water is 1:(0.8-1.4).
[0031] The modified bismuth trioxide obtained by the above-mentioned preparation method can be used in the present application to further improve the mechanical properties of the developable soft tissue repair patch by screening the reaction solvent and process temperature.
[0032] In a second aspect, the present application provides a method for preparing the above-mentioned developable soft tissue repair patch, which specifically comprises the following steps: The polypropylene is dissolved in an organic solvent to obtain a polypropylene solution, and then the modified bismuth trioxide and the xanthan gum are added, and stirred until the mixture is uniform to obtain a mixed slurry; The mixed slurry is added into a coagulation bath for phase inversion solidification, and then washed, vacuum dried, extruded, granulated and spun to obtain a fiber raw material; The fiber raw materials are mixed and woven to prepare the developable soft tissue repair patch.
[0033] Preferably, the process conditions of the extrusion granulation are: temperature of 200-230° C. and screw speed of 150-250 r / min.
[0034] Preferably, the spinning temperature is 160-200°C.
[0035] The present application uses the above-mentioned preparation process to prepare a developable soft tissue repair patch. The preparation method is simple and easy to operate, and a developable soft tissue repair patch with excellent mechanical properties, high safety and good developing effect can be obtained at a low cost.
[0036] Preferably, the mixing temperature of the mixed slurry is 90-120°C.
[0037] Preferably, the organic solvent is selected from any one of toluene, xylene and decalin.
[0038] Preferably, the coagulation bath is selected from any one of petroleum ether, ethyl acetate and dichloromethane.
[0039] Through experimental analysis, it can be known that compared with anhydrous ethanol as a coagulation bath, the present application selects any one of petroleum ether, ethyl acetate, and dichloromethane as a coagulation bath for phase inversion, which can further improve the mechanical properties of the developable soft tissue repair patch. Furthermore, the present application selects petroleum ether as a coagulation bath.
[0040] Optionally, the specific method for mixed weaving of the fiber raw materials is: using a Raschel warp knitting machine to mixed weave the fiber raw materials, the specific process is: machine number 12, pulling density 10 / cm, warp let-off 3000mm / rack, weaving into a square mesh patch, and the woven product is heat-set at 130°C to obtain a developable soft tissue repair patch.
[0041] Through the above weaving method, the surface of the developable soft tissue repair patch product is porous network-like, with pores of different sizes, many and obvious interconnected channels, a porosity of 12-45%, a pore size of 50-300um, and a unit area weight of 100-200g / m 2 The thickness is 0.6-1.5mm, which can meet the requirements of cell growth on the scaffold material structure and pore size, is conducive to the infiltration and growth of tissue cells, and realizes rapid tissue regeneration.
[0042] In a third aspect, the present application provides the application of the above-mentioned developable soft tissue repair patch in medical materials.
[0043] In summary, the technical solution of this application has the following effects: The present application utilizes polypropylene as the main body, adds bismuth trioxide modified with methylcellulose and a trace amount of xanthan gum, and controls the addition amount of each raw material component, so as to obtain a developable soft tissue repair patch with high bursting strength, high tensile strength, high safety, and clear developing effect.
[0044] The present application can further improve the mechanical properties of the developable soft tissue repair patch by controlling the weight ratio of methyl cellulose and bismuth trioxide in the modified bismuth trioxide, the viscosity of methyl cellulose and the particle size of bismuth trioxide.
[0045] The raw materials used in this application are all safe and non-toxic materials, and the degradation products are safe and non-toxic. No toxic reagents are used in the production process. The developable soft tissue repair patch is non-cytotoxic, which gives the developable soft tissue repair patch good cell compatibility and has broad clinical application prospects.
[0046] The composite material has simple manufacturing process, low cost and is convenient for industrial production. DETAILED DESCRIPTION
[0047] In a first aspect, the present application provides a developable soft tissue repair patch, comprising the following components in parts by weight: 80-90 parts of polypropylene; 8-14 parts of modified bismuth trioxide; 0.2-0.4 parts of xanthan gum; The modified bismuth trioxide is obtained by modifying bismuth trioxide with methyl cellulose, the weight ratio of methyl cellulose to bismuth trioxide is (2-6):20; the viscosity of methyl cellulose is 400-4000cp; and the particle size of bismuth trioxide is 100-600nm.
[0048] Specifically, the developable soft tissue repair patch is composed of the following components in parts by weight: 85-90 parts of polypropylene; 8-12 parts of modified bismuth trioxide; and 0.25-0.35 parts of xanthan gum.
[0049] Furthermore, the viscosity of methylcellulose is 1000-2000 cp.
[0050] Wherein, the preparation method of modified bismuth trioxide is: The methyl cellulose is dissolved in a mixed solvent of toluene and water at a temperature of 100-120° C. to obtain a methyl cellulose solution with a concentration of 3-5wt%; then bismuth trioxide is added to the methyl cellulose solution and stirred and refluxed for 60-90 minutes; after the reaction is completed, the reaction solution is vacuum dried to obtain modified bismuth trioxide; the volume ratio of toluene to the water is 1:(0.8-1.4).
[0051] In a second aspect, the present application provides a method for preparing the above-mentioned developable soft tissue repair patch, which specifically comprises the following steps: Dissolving polypropylene in an organic solvent at 90-120° C. to obtain a polypropylene solution, then adding modified bismuth trioxide and xanthan gum, stirring until the mixture is uniform, and obtaining a mixed slurry; The mixed slurry is added into a coagulation bath for phase inversion solidification, and then washed, vacuum dried, extruded into granules and spun to obtain fiber raw materials; The fiber raw materials are mixed and woven to prepare a developable soft tissue repair patch.
[0052] Specifically, the process conditions for extrusion granulation are: temperature of 200-230° C. and screw speed of 150-250 r / min.
[0053] The spinning temperature is 160-200°C.
[0054] Meanwhile, the organic solvent is selected from any one of toluene, xylene and decalin.
[0055] The coagulation bath is selected from any one of petroleum ether, ethyl acetate and dichloromethane.
[0056] The specific method for mixed weaving of fiber raw materials is: using a Raschel warp knitting machine to mixed weave the fiber raw materials, the specific process is: machine number 12, pulling density 10 / cm, warp let-off 3000mm / rack, weaving into a square mesh patch, and the woven product is heat-set at 130°C to obtain a developable soft tissue repair patch.
[0057] In a third aspect, the present application provides the application of the above-mentioned developable soft tissue repair patch in medical materials.
[0058] The present application is further described in detail below in conjunction with examples, comparative examples and performance testing experiments. These examples should not be construed as limiting the scope of protection claimed in the present application.
[0059] Preparation Example Preparation Example 1 This preparation example provides a modified bismuth trioxide.
[0060] The preparation method of modified bismuth trioxide in this preparation example is: 1 g of methyl cellulose with a viscosity of 1500 cP (purchased from Merck) was dissolved in 100 ml of a mixed solvent of toluene and water (the volume ratio of toluene to water was 1:1) at a temperature of 110° C. to obtain a methyl cellulose solution; then 20 g of bismuth trioxide was slowly added to the methyl cellulose solution, and the mixture was stirred and refluxed for 75 minutes; after the reaction was completed, the reaction solution was placed at 120° C. and vacuum dried to obtain modified bismuth trioxide.
[0061] Preparation Example 2 This preparation example provides a modified bismuth trioxide.
[0062] The difference between this preparation example and preparation example 1 is that the amount of methyl cellulose used is 2 g.
[0063] Preparation Example 3 This preparation example provides a modified bismuth trioxide.
[0064] The difference between this preparation example and preparation example 1 is that the amount of methyl cellulose used is 4 g.
[0065] Preparation Example 4 This preparation example provides a modified bismuth trioxide.
[0066] The difference between this preparation example and preparation example 1 is that the amount of methyl cellulose used is 6 g.
[0067] Preparation Example 5 This preparation example provides a modified bismuth trioxide.
[0068] The difference between this preparation example and preparation example 1 is that the amount of methyl cellulose used is 7 g.
[0069] Preparation Example 6 This preparation example provides a modified bismuth trioxide.
[0070] The difference between this preparation example and preparation example 1 is that the viscosity of methylcellulose is 400 cP (purchased from Merck).
[0071] Preparation Example 7 This preparation example provides a modified bismuth trioxide.
[0072] The difference between this preparation example and preparation example 1 is that the viscosity of methyl cellulose is 4000 cP (purchased from Merck).
[0073] Preparation Example 8 This preparation example provides a modified bismuth trioxide.
[0074] The difference between this preparation example and preparation example 1 is that the particle size of bismuth trioxide is 50 nm.
[0075] Preparation Example 9 This preparation example provides a modified bismuth trioxide.
[0076] The difference between this preparation example and preparation example 1 is that the particle size of bismuth trioxide is 800 nm.
[0077] Preparation Example 10 This preparation example provides a modified bismuth trioxide.
[0078] The difference between this preparation example and preparation example 1 is that the reaction temperature is 90°C.
[0079] Preparation Example 11 This preparation example provides a modified bismuth trioxide.
[0080] The difference between this preparation example and preparation example 1 is that the reaction temperature is 100°C.
[0081] Preparation Example 12 This preparation example provides a modified bismuth trioxide.
[0082] The difference between this preparation example and preparation example 1 is that the reaction temperature is 120°C.
[0083] Preparation Example 13 This preparation example provides a modified bismuth trioxide.
[0084] The difference between this preparation example and preparation example 1 is that the reaction temperature is 130°C.
[0085] Preparation Example 14 This preparation example provides a modified barium sulfate.
[0086] The preparation method of modified barium sulfate in this preparation example is: 1 g of methyl cellulose with a viscosity of 1500 cP (purchased from Merck) was dissolved in 100 ml of a mixed solvent of toluene and water (the volume ratio of toluene to water was 1:1) at a temperature of 110° C. to obtain a methyl cellulose solution; then 20 g of barium sulfate was slowly added to the methyl cellulose solution, and the mixture was stirred and refluxed for 75 minutes; after the reaction was completed, the reaction solution was placed at 120° C. and vacuum dried to obtain modified barium sulfate. Example
[0087] Examples 1-5 Embodiments 1-5 each provide a developable soft tissue repair patch.
[0088] The difference between the above embodiments is that the addition amount of each component in the developable soft tissue repair patch is specifically shown in Table 1.
[0089] The method for preparing the developable soft tissue repair patch in the above embodiment specifically comprises the following steps: S1: According to Table 1, add 100 mL of xylene to the reactor, adjust the temperature to 100°C, the stirring speed to 250 r / min, and then add the corresponding weight of polypropylene. After the polypropylene is completely dissolved, add the modified bismuth trioxide in Preparation Example 3 to the reactor, and add xanthan gum; then maintain the temperature and speed unchanged, continue stirring for 30 minutes, and obtain a mixed slurry.
[0090] S2: The mixed slurry is slowly poured into a 100mL petroleum ether coagulation bath at room temperature and a stirring rate of 50r / min for phase inversion solidification, washed with petroleum ether and vacuum dried; put into a twin-screw extruder at a temperature of 220°C and a screw speed of 180r / min for extrusion granulation; and single-screw melt spinning at a temperature of 180°C is performed to obtain a fiber raw material.
[0091] S3: The fiber raw materials are mixed and woven using a Raschel warp knitting machine. The specific process is: machine number 12, pulling density 10 / cm, warp let-off 3000mm / rack, and square mesh patches are woven. The woven products are heat-set at 130°C to obtain developable soft tissue repair patches.
[0092] Table 1 Addition amount of each component in the developable soft tissue repair patch in Examples 1-5 Embodiment 6-17 Examples 6-17 each provide a developable soft tissue repair patch.
[0093] The difference between the above embodiment and embodiment 2 is that the sources of modified bismuth trioxide are different, as shown in Table 2.
[0094] Table 2 Sources of modified bismuth trioxide in Examples 2, 6-17 Embodiment 18 This embodiment provides a developable soft tissue repair patch.
[0095] The difference between this embodiment and embodiment 2 is that in step S2, 100 mL of ethyl acetate is used instead of petroleum ether as the coagulation bath.
[0096] Embodiment 19 This embodiment provides a developable soft tissue repair patch.
[0097] The difference between this embodiment and embodiment 2 is that in step S2, 100 mL of dichloromethane is used as the coagulation bath instead of petroleum ether.
[0098] Embodiment 20 This embodiment provides a developable soft tissue repair patch.
[0099] The difference between this embodiment and embodiment 2 is that in step S2, 100 mL of anhydrous ethanol is used instead of petroleum ether as the coagulation bath.
[0100] Comparative Example Comparative Example 1 This comparative example provides a developable soft tissue repair patch.
[0101] The difference between this comparative example and Example 2 is that bismuth trioxide is used instead of modified bismuth trioxide.
[0102] Comparative Example 2 This comparative example provides a developable soft tissue repair patch.
[0103] The preparation method of the developable soft tissue repair patch in this comparative example is: S1: Add 100 mL of xylene to the reactor, adjust the temperature to 100°C, stir at 250 r / min, then add 85 g of polypropylene. After the polypropylene is completely dissolved, add 2 g of methyl cellulose with a viscosity of 1500 cP, 10 g of bismuth trioxide and 0.3 g of xanthan gum to the reactor; then maintain the temperature and speed unchanged, continue stirring for 30 min, and obtain a mixed slurry.
[0104] S2: The mixed slurry is slowly poured into a 100mL petroleum ether coagulation bath at room temperature and a stirring rate of 50r / min for phase inversion solidification, washed with petroleum ether and vacuum dried; put into a twin-screw extruder at a temperature of 220°C and a screw speed of 180r / min for extrusion granulation; and single-screw melt spinning at a temperature of 180°C is performed to obtain a fiber raw material.
[0105] S3: The fiber raw materials are mixed and woven using a Raschel warp knitting machine. The specific process is: machine number 12, pulling density 10 / cm, warp let-off 3000mm / rack, and square mesh patches are woven. The woven products are heat-set at 130°C to obtain developable soft tissue repair patches.
[0106] Comparative Example 3 This comparative example provides a developable soft tissue repair patch.
[0107] The difference between this comparative example and Example 2 is that the modified barium sulfate prepared in Preparation Example 14 is used instead of the modified bismuth trioxide.
[0108] Comparative Example 4 This comparative example provides a developable soft tissue repair patch.
[0109] The difference between this comparative example and Example 2 is that no xanthan gum is added.
[0110] Comparative Example 5 This comparative example provides a developable soft tissue repair patch.
[0111] The difference between this comparative example and Example 2 is that carob bean gum (purchased from Merck) is used instead of xanthan gum.
[0112] Performance testing The performance of the developable soft tissue repair patches prepared in the examples and comparative examples was tested.
[0113] (1) Bursting strength: According to the test method specified in YY0500-2004, the developable soft tissue repair patch to be tested is cut into a 5×5 cm square and then placed on a universal tensile testing machine to test the bursting strength of the sample to be tested.
[0114] Test results: as shown in Table 3.
[0115] (2) Tensile strength: Tested in accordance with the method specified in GB / T 3923.1-2013 “Tensile Properties of Textile Fabrics”.
[0116] Test results: as shown in Table 3.
[0117] (3) Cytotoxicity: Cytotoxicity test was performed according to ISO10993-5, 1999: Biological evaluation of medical devices - Part 5: In vitro cytotoxicity test.
[0118] The cytotoxicity evaluation method is as follows: 0 - no cytotoxicity; 1 - mild cytotoxicity; 2 - moderate cytotoxicity; 3 - severe cytotoxicity.
[0119] Test results: as shown in Table 3.
[0120] (4) Detection of X-ray development Place the developable soft tissue repair patch on A4 paper and take a photo with an X-ray developer to observe the clarity of the developed image of the suture (the clarity is from high to low: high definition, relatively clear, relatively fuzzy, and fuzzy).
[0121] Test results: as shown in Table 3.
[0122] Table 3 Performance test results of the developable soft tissue repair patches in Examples 1-20 and Comparative Examples 1-5 Combined with the test results in Table 3, the present application uses methylcellulose to modify bismuth trioxide, and prepares a developable soft tissue repair patch with polypropylene and xanthan gum. The bursting strength of the developable soft tissue repair patch is ≥236N, and the tensile strength is ≥92Kpa. The above test results show that the developable soft tissue repair patch prepared by the present application has better mechanical properties. After the tissue patch is implanted in the body, it can provide sufficient mechanical support, which is conducive to preventing recurrence of tearing of the affected area caused by the breakage of the repair patch. It is suitable for the repair of joint soft tissue and can ensure the success rate of the operation. In addition, the developable soft tissue repair patch prepared by the present application is non-cytotoxic and has a clear development effect, which is conducive to checking the position, shape and state of the soft tissue repair patch in vitro, which is helpful for doctors to diagnose and follow up after surgery, and is conducive to patient recovery.
[0123] By comparing the test results of Example 2 with those of Comparative Examples 1-3, when the preparation method of unmodified bismuth trioxide is selected as the developer and no methyl cellulose is added, the mechanical properties of the developable soft tissue repair patch prepared are poor; when the preparation method of adding unmodified bismuth trioxide and methyl cellulose respectively is selected, the mechanical properties and developing effect of the developable soft tissue repair patch prepared are poor; when barium sulfate modified by methyl cellulose is selected as the developer, the developable soft tissue repair patch prepared has moderate cytotoxicity and the development is fuzzy; and the present application selects methyl cellulose to modify bismuth trioxide as the developer, which can effectively improve the mechanical properties of the developable soft tissue repair patch, and has high safety and good developing effect.
[0124] At the same time, by comparing the test results of Examples 1-3, when the addition amount of modified bismuth trioxide is controlled to be 8-14 parts, the mechanical properties of the developable soft tissue repair patch can be further improved, and the soft tissue repair patch has higher safety and better developing effect.
[0125] By comparing the test results of Examples 2 and 6-9, in the process of preparing modified bismuth trioxide, when the weight ratio of methyl cellulose and bismuth trioxide is controlled to be (2-6):20, the mechanical properties of the developable soft tissue repair patch can be further improved without affecting the development effect.
[0126] By comparing the test results of Examples 2 and 10-13, in the process of preparing modified bismuth trioxide, when the viscosity of methyl cellulose is controlled to be 800-3000cp and the particle size of bismuth trioxide is controlled to be 100-600nm, the mechanical properties of the developable soft tissue repair patch can be further improved.
[0127] By comparing the test results of Examples 2 and 14-17, in the process of preparing modified bismuth trioxide, when the reaction temperature is 100-120°C, the mechanical properties of the developable soft tissue repair patch can be further improved without affecting the developing effect of the soft tissue repair patch.
[0128] By comparing the test results of Example 2 with those of Comparative Examples 4-5, when no xanthan gum is added, the mechanical properties of the developed soft tissue repair patch prepared are poor; when carob bean gum is used instead of xanthan gum, the mechanical properties of the developed soft tissue repair patch prepared are not well improved, and it has severe cytotoxicity and poor development effect; and the present application selects xanthan gum as the raw material, which can significantly improve the mechanical properties of the developable soft tissue repair patch, and has no cytotoxicity and will not affect the development effect.
[0129] At the same time, by comparing the test results of Examples 2 and 4-5, when the addition amount of xanthan gum is controlled to be 0.2-0.4 parts, the mechanical properties of the developable soft tissue repair patch can be further improved, and the soft tissue repair patch has higher safety and better developing effect.
[0130] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A developable soft tissue repair patch, characterized in that: The invention comprises the following components in parts by weight: 80-90 parts of polypropylene; 8-14 parts of modified bismuth trioxide; 0.2-0.4 parts of xanthan gum; Wherein, the modified bismuth trioxide is obtained by modifying bismuth trioxide with methyl cellulose.
2. The developable soft tissue repair patch according to claim 1, characterized in that: The invention is composed of the following components in parts by weight: 85-90 parts of polypropylene; 12-14 parts of modified bismuth trioxide; and 0.25-0.35 parts of xanthan gum.
3. The developable soft tissue repair patch according to claim 1, characterized in that: In the modified bismuth trioxide, the weight ratio of the methyl cellulose to the bismuth trioxide is (2-6):
20.
4. The developable soft tissue repair patch according to claim 1, characterized in that: The viscosity of the methyl cellulose is 400-4000 cp.
5. The developable soft tissue repair patch according to claim 1, characterized in that: The particle size of the bismuth trioxide is 100-600nm.
6. The developable soft tissue repair patch according to claim 1, characterized in that: The preparation method of the modified bismuth trioxide is: The methyl cellulose is dissolved in a mixed solvent of toluene and water at a temperature of 100-120° C. to obtain a methyl cellulose solution with a concentration of 3-5wt%; then the bismuth trioxide is added to the methyl cellulose solution and stirred and refluxed for 60-90 minutes; after the reaction is completed, the reaction solution is vacuum dried to obtain the modified bismuth trioxide. The volume ratio of the toluene to the water is 1: (0.8-1.4).
7. The method for preparing a developable soft tissue repair patch according to any one of claims 1 to 6, characterized in that: The specific steps include: The polypropylene is dissolved in an organic solvent to obtain a polypropylene solution, and then the modified bismuth trioxide and the xanthan gum are added, and stirred until the mixture is uniform to obtain a mixed slurry; The mixed slurry is added into a coagulation bath for phase inversion solidification, and then washed, vacuum dried, extruded, granulated and spun to obtain a fiber raw material; The fiber raw materials are mixed and woven to prepare the developable soft tissue repair patch.
8. The method for preparing a developable soft tissue repair patch according to claim 7, characterized in that: The organic solvent is selected from any one of toluene, xylene and decalin.
9. The method for preparing a developable soft tissue repair patch according to claim 7, characterized in that: The coagulation bath is selected from any one of petroleum ether, ethyl acetate and dichloromethane.
10. Use of the developable soft tissue repair patch according to any one of claims 1 to 6 in medical materials.