Material with developing function and preparation method thereof
By modifying barium sulfate with a modifying liquid and using a polymer surfactant, the problem of poor dispersion of the developer in the material and reduced mechanical properties is solved, and the mechanical properties and development effect of the developing material are significantly improved.
Patent Information
- Application Number
- CN202410886327.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-29
AI Technical Summary
The mechanical properties of existing polymer materials used in interventional medical devices decrease after adding a developer, which limits the application of the developer material. Moreover, the developer barium sulfate is not easily dispersed in the material, affecting the development effect.
The surface of barium sulfate is modified with a modification liquid and combined with trimethylene carbonate and hyperbranched polyphosphate to improve the toughness and stability of the developer; 4-hydroxybutyl acrylate and polydioxanone are introduced to Enhance the stability and mechanical properties of the material; use polymer surfactants as dispersants to improve the dispersion and compatibility of the developer in polyglycolic acid.
The tensile strength, elongation at break, flexural modulus and impact strength of the development material are significantly improved, and the mechanical properties are optimized while ensuring the development performance. The material produced has good mechanical properties and development effect.
Smart Images

Figure BDA0004926151970000071
Abstract
Description
Technical Field
[0001] The present application relates to the field of developable materials, and more specifically, to a material with a developing function and a preparation method thereof. Background Art
[0002] Medical polymer materials refer to polymer materials used to manufacture human internal organs, external organs, drug dosage forms and medical devices. Their sources include natural biopolymer materials and synthetic biopolymer materials. Natural medical polymer materials come from nature, including cellulose, chitin, hyaluronic acid, collagen, gelatin and sodium alginate; synthetic medical polymer materials are polymer materials for medical use that are artificially synthesized by chemical methods. Currently commonly used ones are polyurethane, silicone rubber, polyester fiber, polyetheretherketone, polymethyl methacrylate, polyvinyl alcohol, polylactic acid, polyethylene, etc.
[0003] For polymer materials used in interventional medical devices, medical polymers are required to be resistant to biological aging, have stable physical and mechanical properties, be easy to process and form, and have easy access to materials. At the same time, in order to have X-ray development, a certain amount of developer needs to be added to the polymer matrix. Barium sulfate is a type of low molecular weight substance that can be developed under X-rays, and has the characteristics of being developable under X-rays and being biologically inert. At the same time, polyetheretherketone materials do not degrade in the human body, have good toughness and high strength. The bone repair and reconstruction materials made by mixing the two have the characteristics of being developable, high strength, and low barium sulfate release. By adjusting the distribution density of barium sulfate per unit volume, its development effect can be effectively adjusted, thereby meeting the needs of implants in different parts for X-ray transmittance. However, the addition of barium sulfate will cause the hardness and toughness of the material to decrease, limiting the application of development materials. Summary of the invention
[0004] In order to improve the mechanical properties of a developing material, the present application provides a material with a developing function and a preparation method thereof.
[0005] In a first aspect, the present application provides a material with a developing function, which adopts the following technical solution: A material with a developing function comprises the following raw materials in parts by weight: 75-90 parts of polyglycolic acid, 5-15 parts of a modified developer, 2-8 parts of a dispersant, 1-4 parts of 4-hydroxybutyl acrylate, 2-6 parts of polydioxanone, 1-4 parts of polyethylene carbonate and 0.5-2 parts of a hyperbranched polyphosphate; the modified developer is prepared from barium sulfate and a modifying liquid.
[0006] By adopting the above technical scheme, the present application modifies the surface of the developer barium sulfate by a modifying liquid, and then utilizes the synergistic effect of trimethylene carbonate and hyperbranched polyphosphate to improve the toughness of the composite material when the developer is added; then utilizes the composite effect of 4-hydroxybutyl acrylate and polydioxanone to improve the stability of the material with a developing function by introducing a hydroxyl group, and can slow down the degradation rate of the material; then, by adding a certain amount of dispersant to the raw material of the material with a developing function, the dispersibility of the modified developer in the raw material can be further improved, so that it is evenly dispersed in polyglycolic acid, and the compatibility of the developer and polyglycolic acid is improved, so that the developing performance is ensured while obtaining the material with a developing function having strong mechanical properties.
[0007] Preferably, the material with developing function comprises the following raw materials in parts by weight: 80-85 parts of polyglycolic acid, 8-12 parts of modified developer, 4-6 parts of dispersant, 2-3 parts of 4-hydroxybutyl acrylate, 4-5 parts of polydioxanone and 1-1.5 parts of hyperbranched polyphosphate.
[0008] By adopting the above technical solution, the present application optimizes the ratio between the raw materials of the materials with developing function, so that the tensile strength, elongation at break, bending modulus and impact strength of the prepared material with developing function are better.
[0009] Preferably, the mass ratio of barium sulfate to the modified liquid in the modified developer is (1-4):20.
[0010] By adopting the above technical solution, the present application limits the mass ratio of barium sulfate and modifying liquid in the modified developer, so that the modifying liquid can modify the surface of barium sulfate more completely, and the prepared modified developer can be added to a material with a developing function.
[0011] Preferably, the modified developer is prepared by adding barium sulfate to the modified solution, stirring at 65-85°C for 0.5-1h, then washing repeatedly with ethanol and deionized water for 3-5 times, and drying at a constant temperature of 65-85°C for 1-2h to obtain the modified developer.
[0012] By adopting the above technical solution, the present application modifies the surface of barium sulfate through the above preparation method, so that the developer barium sulfate can be more fully modified, and the obtained modified developer can have better compatibility when added to materials with developing function.
[0013] Preferably, the average particle size of the barium sulfate is 100-200 nm.
[0014] By adopting the above technical solution, when the particle size of the barium sulfate powder particles is less than 100 nm, the barium sulfate powder has a large specific surface area, is easy to agglomerate, and is not easy to disperse in the thermoplastic polymer main material. The present application limits the average particle size of barium sulfate to make it have better dispersibility in the raw material, so that the final material with development function has better mechanical properties.
[0015] Preferably, the modified liquid is one or more of aminosilane, acryloxysilane, isopropyl dioleyl acyloxy titanate or isopropyl trititanate.
[0016] By adopting the above technical solution, the present application adopts the above modifying liquid to modify the surface of barium sulfate powder, and the modifying liquid contains two different types of chemical functional groups, one end of which can react with inorganic materials to form hydrogen bonds, and condense, dehydrate and solidify under certain conditions to form covalent bonds; the other end can combine with polyglycolic acid, so that a good interface bonding force is generated between the two, and the two materials with large differences in properties are firmly combined. Thus, the material has a certain development effect, and the mechanical properties of the material are also improved.
[0017] Preferably, the raw materials further include 4-10 parts by weight of tricalcium phosphate.
[0018] By adopting the above technical solution, tricalcium phosphate is widely present in bones and has a good bone-forming effect, and appropriately mixing tricalcium phosphate into polymer materials is beneficial to enhancing their mechanical strength.
[0019] Preferably, the dispersant is a polymer surfactant; the dispersant is one or more of polyethylene glycol, polyethylene oxide, and sodium polyacrylate.
[0020] By adopting the above technical solution, the developer barium sulfate used in this application is a polar substance, and the main material used is a non-polar polymer, so the developer barium sulfate is not easy to disperse in the main material. The polymer surfactant molecular chain contains polar groups such as carboxyl, hydroxyl, and ether bonds, which can be adsorbed or chemically reacted with the surface of inorganic filler particles; at the same time, the main component of its molecular chain is a carbon-carbon structure, so it is compatible with the main material at the same time. The dispersant covers the surface of the polymer, and its polar end is inwardly combined with the barium sulfate. At the same time, its carbon-carbon structure end (lipophilic end) faces outward, so that a layer of lipophilic structure is formed on the surface of the barium sulfate powder, which improves its compatibility with the main polymer, thereby improving its dispersibility in the main material.
[0021] In a second aspect, the present application provides a method for preparing a material having a developing function, using the following technical solution: A method for preparing a material with a developing function comprises the following steps: 1) melt-blending polyglycolic acid, 4-hydroxybutyl acrylate, polydioxanone and hyperbranched polyphosphate to obtain a first mixture; 2) Adding a modified developer, a dispersant and other raw materials to the first mixture, melt blending for 10-15 minutes, and then extruding to obtain a material with a developing function.
[0022] By adopting the above technical solution, the material with developing function prepared in the present application has readily available raw materials, a simple and easy preparation method, and can effectively improve production efficiency.
[0023] In summary, this application has the following beneficial effects: 1. The present application modifies the surface of the developer barium sulfate by a modifying liquid, and then utilizes the synergistic effect of trimethylene carbonate and hyperbranched polyphosphate to improve the toughness of the composite material when the developer is added; then utilizes the composite effect of 4-hydroxybutyl acrylate and polydioxanone to improve the stability of the material with a developing function by introducing a hydroxyl group, thereby slowing down the degradation rate of the material; and then by adding a certain amount of dispersant to the raw material of the material with a developing function, the dispersibility of the modified developer in the raw material can be further improved, so that it is evenly dispersed in polyglycolic acid, and the compatibility of the developer and polyglycolic acid is improved, thereby ensuring the developing performance while obtaining a material with a developing function having strong mechanical properties.
[0024] 2. In this application, the above-mentioned modifying liquid is used to modify the surface of barium sulfate powder. The modifying liquid contains two different types of chemical functional groups. One end of it can react with inorganic materials to form hydrogen bonds, and condense, dehydrate and solidify under certain conditions to form covalent bonds; the other end can combine with polyglycolic acid, so that a good interface bonding force is generated between the two, and the two materials with large differences in properties are firmly combined. In this way, the material has a certain development effect and the mechanical properties of the material are also improved.
[0025] 3. The material with developing function prepared in this application is subjected to mechanical property testing. The tensile strength of the material with developing function obtained can reach 57.3MPa, the elongation at break can reach 73.4%, the flexural modulus can reach 1836MPa, and the notched impact strength can reach 15.2kJ / m 2 The obtained material with developing function has good mechanical properties. DETAILED DESCRIPTION
[0026] The present application is further described in detail below in conjunction with embodiments.
[0027] raw material The raw materials used in this application are all common commercially available materials.
[0028] Preparation Example Preparation Example 1 A modified developer, the preparation method of which is as follows: 1 kg of barium sulfate was added to 20 kg of the modified liquid, stirred at 65° C. for 0.5 h, then washed repeatedly with ethanol and deionized water for 3 times, and dried at a constant temperature of 70° C. for 2 h to obtain a modified developer.
[0029] The average particle size of barium sulfate is 80 nm, and the modified liquid is a mixture of aminosilane, acryloxysilane, isopropyl dioleyl acyloxy titanate and the like in a certain mass ratio.
[0030] Preparation Example 2 A modified developer is different from Preparation Example 1 in that 2 kg of barium sulfate is added to 20 kg of the modified liquid, and the remaining steps are the same as Preparation Example 2.
[0031] Preparation Example 3 A modified developer is different from Preparation Example 1 in that 4 kg of barium sulfate is added to 20 kg of the modified liquid, and the remaining steps are the same as Preparation Example 2. Example
[0032] Examples 1-4 A material with a developing function according to Example 1-4, whose raw materials and the amounts of each raw material are shown in Table 1, and whose preparation method is as follows: 1) melt-blending polyglycolic acid, 4-hydroxybutyl acrylate, polydioxanone and hyperbranched polyphosphate to obtain a first mixture; 2) Adding a modified developer, a dispersant and other raw materials to the first mixture, melt blending for 15 minutes, and then extruding to obtain a material with a developing function.
[0033] The modified developer is from Preparation Example 1.
[0034] Table 1 Raw materials and amounts of each raw material in Examples 1-4 (kg) Example 1 Example 2 Example 3 Example 4 Polyglycolic acid 75 80 85 90 Modified developer 5 5 5 5 Dispersants 8 6 4 2 4-Hydroxybutyl acrylate 1 2 3 4 Polydioxanone 6 5 4 2 Polyethylene carbonate 1 2 3 4 Hyperbranched polyphosphate 2 1.5 1 0.5 Example 5 A material with a developing function, which is different from Example 3 in that the modified developer comes from Preparation Example 2, and the remaining steps are the same as Example 3.
[0035] Example 6 A material with a developing function, which is different from Example 3 in that the modified developer comes from Preparation Example 3, and the remaining steps are the same as Example 3.
[0036] Example 7 A material with a developing function, which is different from Example 5 in that the average particle size of barium sulfate is 100 nm, and the remaining steps are the same as Example 5.
[0037] Example 8 A material with a developing function, which is different from Example 5 in that the average particle size of barium sulfate is 200 nm, and the remaining steps are the same as Example 5.
[0038] Example 9 A material with a developing function, which is different from Example 5 in that the added amount of the modified developer is 8 kg, and the remaining steps are the same as Example 5.
[0039] Example 10 A material with a developing function, which is different from Example 5 in that the added amount of the modified developer is 12 kg, and the remaining steps are the same as Example 5.
[0040] Embodiment 11 A material with a developing function, which is different from Example 5 in that the added amount of the modified developer is 15 kg, and the remaining steps are the same as Example 5.
[0041] Example 12 A material with a developing function, which is different from Example 3 in that 4 kg of tricalcium phosphate is also added to the raw material, and the remaining steps are the same as Example 3.
[0042] Embodiment 13 A material with a developing function, which is different from Example 3 in that 8 kg of tricalcium phosphate is also added to the raw material, and the remaining steps are the same as Example 3.
[0043] Embodiment 14 A material with a developing function, which is different from Example 3 in that 10 kg of tricalcium phosphate is also added to the raw material, and the remaining steps are the same as Example 3.
[0044] Comparative Example Comparative Example 1 A material with a developing function, which is different from Example 1 in that an equal amount of unmodified barium sulfate is used instead of the modified developer, and the remaining steps are the same as those of Example 1.
[0045] Comparative Example 2 A material with a developing function, which is different from Example 1 in that 0.5 kg of barium sulfate is added to 20 kg of the modified liquid, and the remaining steps are the same as those of Example 1.
[0046] Comparative Example 3 A material with a developing function, which is different from Example 1 in that 5 kg of barium sulfate is added to 20 kg of the modified liquid, and the remaining steps are the same as those of Example 1.
[0047] Comparative Example 4 A material with a developing function, which is different from Example 1 in that the amount of polyethylene carbonate added in the raw material is 0, and the remaining steps are the same as Example 1.
[0048] Comparative Example 5 A material with a developing function, which is different from Example 1 in that the amount of hyperbranched polyphosphate added in the raw material is 0, and the remaining steps are the same as Example 1.
[0049] Performance testing Detection method / test method The following performance tests were performed on the materials with developing function prepared in Examples 1-14 and Comparative Examples 1-5. The test results are shown in Table 2.
[0050] Tensile strength test: The tensile strength of the material is measured according to the test method described in GB / T1040.1-2018 "Determination of tensile properties of plastics".
[0051] Elongation at break test: The elongation at break of the material is measured according to the test method described in GB / T1040.1-2018 "Determination of tensile properties of plastics".
[0052] Flexural modulus test: The flexural modulus of the material is measured according to the test method described in ISO178-2010 "Determination of flexural properties of plastics".
[0053] Notched impact strength test: The impact strength of the material is measured according to the test method described in ISO179-2000 "Plastics - Determination of simply supported beam impact strength of rigid materials".
[0054] Table 2 Test results of Examples 1-14 and Comparative Examples 1-5 It can be seen from the test data of Examples 1-4 that the ratio of the raw materials in Example 3 is better, and the material with developing function prepared by the ratio of Example 3 has high tensile strength, elongation at break, bending modulus and impact strength, indicating that the comprehensive mechanical properties of the material are improved.
[0055] Combining the test data of Example 3 and Examples 5-6, it can be seen that when the modified developer of Preparation Example 2 is used in the preparation process of a material with a developing function, the obtained material with a developing function has good mechanical properties, among which the tensile strength, elongation at break, flexural modulus and impact strength are all improved.
[0056] Combining the test data of Example 5 and Examples 7-8, it can be seen that the smaller the average particle size of barium sulfate is, the better the comprehensive mechanical properties of the material finally prepared by the modified developer used for the preparation of the material with the developing function is, which means that the smaller the average particle size of barium sulfate is, the stronger the bonding force between the barium sulfate and other raw materials will be after modification, thereby improving the strength and toughness of the material with the developing function and making it have excellent mechanical properties.
[0057] Combining the test data of Example 5 and Examples 9-11, it can be seen that as the amount of modified developer added increases, the tensile strength, elongation at break, flexural modulus and impact strength of the obtained material with a developing function gradually increase. When the amount of modified developer added is 12 kg, the tensile strength of the obtained material with a developing function is 56.8 MPa, the elongation at break is 72.8%, the flexural modulus is 1836 MPa, and the notched impact strength is 14.9 kJ / m 2 .
[0058] Combining the test data of Example 10 and Examples 12-14, it can be seen that the addition of tricalcium phosphate to the raw material gradually enhances the tensile strength, elongation at break, flexural modulus and impact strength of the obtained material with a developing function. When the addition amount of tricalcium phosphate is 8 kg, the tensile strength of the obtained material with a developing function is 57.3 MPa, the elongation at break is 73.4%, the flexural modulus is 1836 MPa, and the notched impact strength is 15.2 kJ / m 2 .
[0059] Combining the test data of Example 1 and Comparative Example 1, it can be seen that the tensile strength, elongation at break, bending modulus and impact strength of the material with a developing function obtained by using an equal amount of unmodified barium sulfate instead of the modified developer are reduced. This indicates that the intermolecular force between the barium sulfate modified by the modifying liquid and other raw materials is enhanced, which can effectively improve the comprehensive mechanical properties of the material with a developing function.
[0060] Combining the test data of Example 1 and Comparative Examples 2-3, it can be seen that too little addition of barium sulfate in the modifying liquid will lead to poor development effect of the developing material. At the same time, too much addition of barium sulfate in the modifying liquid will result in incomplete modification of the surface of the barium sulfate. When added to the preparation process of the material with developing function, its dispersion is poor, resulting in reduced tensile strength, elongation at break, flexural modulus and impact strength of the prepared material.
[0061] Combined with the test data of Comparative Examples 4-5, it can be seen that when the addition amount of polyethylene carbonate or hyperbranched polyphosphate in the raw material is 0, the tensile strength, elongation at break, flexural modulus and impact strength of the obtained material with developing function are all reduced, indicating that polyethylene carbonate and hyperbranched polyphosphate have a synergistic effect in improving the toughness of the material.
[0062] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A material having a developing function, characterized in that: The invention comprises the following raw materials in parts by weight: 75-90 parts of polyglycolic acid, 5-15 parts of modified developer, 2-8 parts of dispersant, 1-4 parts of 4-hydroxybutyl acrylate, 2-6 parts of polydioxanone, 1-4 parts of polyethylene carbonate and 0.5-2 parts of hyperbranched polyphosphate; the modified developer is prepared from barium sulfate and modified liquid.
2. The material with developing function according to claim 1, characterized in that: The material with developing function comprises the following raw materials in parts by weight: 80-85 parts of polyglycolic acid, 8-12 parts of modified developer, 4-6 parts of dispersant, 2-3 parts of 4-hydroxybutyl acrylate, 4-5 parts of polydioxanone, 2-3 parts of polyethylene carbonate and 1-1.5 parts of hyperbranched polyphosphate.
3. The material with developing function according to claim 1, characterized in that: The mass ratio of barium sulfate to the modified liquid in the modified developer is (1-4):
20.
4. The material with developing function according to claim 3, characterized in that: The preparation method of the modified developer is as follows: adding barium sulfate to the modified solution, stirring at a temperature of 65-85° C. for 0.5-1 h, then washing repeatedly with ethanol and deionized water for 3-5 times, and drying at a constant temperature of 65-85° C. for 1-2 h to obtain the modified developer.
5. The material with developing function according to claim 4, characterized in that: The average particle size of the barium sulfate is 80-200 nm.
6. The material with developing function according to claim 4, characterized in that: The modified liquid is one or more of aminosilane, acryloxysilane, isopropyl dioleyl acyloxy titanate or isopropyl trititanate.
7. The material with developing function according to claim 1, characterized in that: The raw materials also include 4-10 parts by weight of tricalcium phosphate.
8. The material with developing function according to claim 1, characterized in that: The dispersant is a high molecular surfactant; the dispersant is one or more of polyethylene glycol, polyethylene oxide, and sodium polyacrylate.
9. A method for preparing a material with a developing function according to any one of claims 1 to 8, characterized in that: It includes the following steps: 1) melt-blending polyglycolic acid, 4-hydroxybutyl acrylate, polydioxanone and hyperbranched polyphosphate to obtain a first mixture; 2) Adding a modified developer, a dispersant and other raw materials to the first mixture, melt blending for 10-15 minutes, and then extruding to obtain a material with a developing function.