Surface modified silica powder as well as preparation method and application thereof
Through sodium hydroxide hydroxylation and silane coupling agent modification of silica powder, combined with the hydrolysis treatment of ethanol and isopropyl alcohol solutions, surface-modified silica powder with high mechanical properties and super-hydrophobicity was prepared, which solved the problem of the filler role of silica powder. It solves the problems of insufficient functionality and insufficient application in the field of oil-water separation when increasing, and achieves high-efficiency effects of oil-water separation and reduction of production costs.
Patent Information
- Application Number
- CN202410867709.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-29
AI Technical Summary
Existing silica powder cannot significantly improve product functionality when the role of filler is increased, and it is insufficiently used in the field of oil-water separation, and the problems of industrial organic wastewater discharge and oil leakage have not been effectively solved.
Use sodium hydroxide hydroxylated silica powder, combine it with ethanol and isopropyl alcohol solutions for hydrolysis, add silane coupling agent and triethoxymethylsilane, and prepare surface-modified silica powder through different rotation speed and temperature conditions to improve its mechanical properties. and superhydrophobicity for oil-water separation.
Surface-modified silica powder with high mechanical properties, chemical stability and super-hydrophobicity was prepared, which significantly improved its application effect in the field of oil-water separation, reduced production costs, and solved the problem of poor mechanical properties.
Smart Images

Figure CN118846591A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of silicon micropowder, in particular to surface-modified silicon micropowder and its preparation method and application. Background Art
[0002] The main component of silicon micropowder is SiO2, which is made from natural quartz or fused quartz through multiple processes such as crushing, ball milling (or vibration, air flow milling), flotation, acid washing and purification, and high-purity water treatment.
[0003] As a non-toxic, low-cost inorganic non-metallic material, silicon micropowder can not only act as a filler in polymer applications to reduce the production cost of the material, but also give the material some special properties. Silicon micropowder itself has many excellent properties, such as electrical insulation, corrosion resistance, heat resistance, light transmittance, etc. If combined with high molecular polymers, it can reduce the exothermic peak temperature, linear expansion coefficient and shrinkage rate of the polymer, while improving the strength and wear resistance of the polymer. It has been widely used in the field of semiconductor integrated circuits and electronic devices. It is the main material of glass fiber and is used to produce ordinary alkali-free glass fiber, glass fiber for the electronics industry, silicone rubber and plastic fillers.
[0004] Chen Duxu et al. (Research on the influence of spherical silicon micropowder modification on the performance of epoxy molding compound [D]. University of Jinan, 2023. DOI: 10.27166 / d.cnki.gsdcc.2023.000578.) designed three processes of silane coupling agent modification, surface etching-silane coupling agent modification, and surface coating-silane coupling agent modification to modify spherical silicon micropowder, and studied the influence of the three modification processes on the performance of spherical silicon micropowder and epoxy molding compound.
[0005] Chinese patent document CN117659743A discloses a method for modifying ultrafine silicon micropowder with solvent recovery function. The modified resin is dissolved in a solvent of hexafluoropropylene trimer; a specified amount of the modified resin solvent is weighed, mixed with a specified amount of the solvent and stirred; the ultrafine silicon micropowder is put into the mixed solvent for silicon micropowder dispersion reaction; the solvent is vacuum distilled and recovered; the modified silicon micropowder mixture after solvent distillation and recovery is dried to obtain modified silicon micropowder. This invention uses an organic phase as a solvent to better dissolve the modified resin and improve the hydrophobicity of the silicon micropowder surface.
[0006] Chinese patent CN117567880A discloses surface-modified silicon micropowder and a preparation method thereof, comprising the following steps: preparing an alcohol-water solution with anhydrous ethanol, water and a silane coupling agent in a mass ratio of 65-75:20-30:5-10, and fully hydrolyzing the silane coupling agent to obtain a solution A; the silane coupling agent is KH-570, KH-550, KH-560 or KBM-573; adding silicon micropowder to the solution A in a mass ratio of silicon micropowder to the silane coupling agent of 100:2-5 for modification; after the modification is completed, standing and cooling to room temperature, washing with ethanol to remove physically adsorbed silane coupling agent and reaction by-products, centrifuging, and drying the product obtained by centrifugation to obtain the surface-modified silicon micropowder.
[0007] In practical applications, silicon micropowder generally acts as a filler. However, when the amount of filler is increased too much, it will not significantly improve the functionality of the product, but will reduce the mechanical properties of the material and increase production costs. Therefore, there is an urgent need to solve the development of silicon micropowder towards functionalization.
[0008] In addition, many industrial organic wastewater discharges and oil spills are still issues that need to be urgently addressed today, and there are currently no reports on the use of modified silica powder for oil-water separation. Summary of the invention
[0009] The present invention aims to solve the existing problems and provides a surface-modified silicon micropowder and a preparation method and application thereof.
[0010] The object of the present invention is to provide a method for preparing surface-modified silicon micropowder, wherein the method for preparing surface-modified silicon micropowder comprises:
[0011] Step 1: Put the original silicon micropowder and sodium hydroxide into a three-necked flask for hydroxylation, then add deionized water into the three-necked flask, stir and reflux, and continue stirring at room temperature after the stirring is completed to obtain a silicon micropowder solution;
[0012] Step 2: centrifuging, dispersing, drying and grinding the silicon micropowder solution to obtain silicon micropowder particles;
[0013] Step 3: adding ethanol solution and isopropanol solution to silicon micropowder particles, mixing to obtain a reaction solvent, and finally dispersing the reaction solvent, stirring and refluxing to obtain a mixture I;
[0014] Step 4: Preparation of modified solution;
[0015] Step 5: adding the modified liquid droplets to the mixture I for hydrolysis, adding ammonia water to promote hydrolysis, stirring evenly, and obtaining the mixture II;
[0016] Step 6: Centrifuge the mixture II, add ethanol, and then disperse, centrifuge and dry to obtain surface-modified silicon micropowder.
[0017] Further, in the step 1, 4-6 parts of silicon micropowder raw powder and 1-3 parts of sodium hydroxide are taken by mass ratio, the silicon micropowder raw powder and sodium hydroxide are placed in a three-necked flask for hydroxylation, and then 80-120 ml of deionized water is added to the three-necked flask, and then stirred and refluxed at a temperature of 90°C-110°C for 2-3 hours. After the stirring is completed, stirring is continued at room temperature for 9-12 hours to obtain a silicon micropowder solution.
[0018] Further, the specific steps of step 2 are:
[0019] (1) placing the silicon powder solution in a centrifuge, centrifuging at a speed of 3500-5000 r / min for 3-5 min, discarding the supernatant, and obtaining precipitate I;
[0020] (2) Add 50-70 ml of deionized water to the precipitate I, shake well to obtain a suspension I, disperse the suspension I, place the suspension I in a centrifuge, centrifuge at a speed of 4000-5000 r / min for 5-8 min, discard the supernatant, and obtain a precipitate II;
[0021] (3) Add 80-100 ml of deionized water to the precipitate II, shake well to obtain suspension II, disperse the suspension II, place the suspension II in a centrifuge, centrifuge at a speed of 4500-5500 r / min for 8-10 min, discard the supernatant, and obtain precipitate III;
[0022] (4) Add 70-90 ml of deionized water to the precipitate III, shake well, and obtain a suspension III. Disperse the suspension III, place the suspension III in a centrifuge, and centrifuge for 5-7 minutes at a speed of 3000-3500 r / min. Discard the supernatant to obtain a precipitate IV.
[0023] (5) Drying the precipitate IV at a temperature of 40-60° C. for 4-6 hours, and finally grinding the precipitate IV to obtain silicon micropowder particles.
[0024] Furthermore, the particle size of the silicon micropowder particles is 800-1500 mesh.
[0025] Further, the specific steps of step three are:
[0026] (1) adding 0.8-1.2 parts of ethanol solution and 1.8-2.2 parts of isopropanol solution to silicon micropowder particles by volume, and mixing them uniformly to obtain a reaction solvent;
[0027] (2) The reaction solvent is stirred and refluxed at a temperature of 80-100° C. for 10-15 minutes to obtain a mixture I.
[0028] Further, the modified liquid includes deionized water, a silane coupling agent and triethoxymethylsilane;
[0029] The preparation method of the modified liquid comprises adding 1-3 parts of deionized water, 3-5 parts of a silane coupling agent and 3-5 parts of triethoxymethylsilane in a three-necked flask according to the volume ratio, and mixing them evenly to obtain the modified liquid;
[0030] The silane coupling agent is any one of dimethyldimethoxysilane or diethoxydimethylsilane.
[0031] Further, in the step 5, the modified liquid droplets are added to the mixture I for hydrolysis, and then 10-12m of ammonia water is added, and stirred for 1.5-3 hours at a temperature of 75-90°C and a rotation speed of 2000-3000r / min, and finally cooled to room temperature, and stirred for 11-13 hours at a rotation speed of 1500-2000r / min to obtain a mixture II. The addition of ammonia water in the present invention can provide an alkaline environment for the hydrolysis reaction of the mixture I and the modified liquid, which is convenient for effectively improving the mechanical properties of the product, increasing the specific surface area of the product, and making the product have high surface superhydrophobicity.
[0032] Further, the specific steps of step six are:
[0033] (1) placing the mixture II in a centrifuge, centrifuging for 3-5 min at a speed of 3500-5000 r / min, and pouring out the supernatant to obtain a precipitate V;
[0034] (2) adding 50-70 ml of ethanol to the precipitate V, shaking to obtain a suspension V, dispersing the suspension V, placing the suspension V in a centrifuge, centrifuging at a speed of 4000-5000 r / min for 5-8 min, discarding the supernatant, and obtaining a precipitate VI;
[0035] (3) adding 80-100 ml of ethanol to the precipitate VI, shaking to obtain a suspension VI, dispersing the suspension VI, placing the suspension VI in a centrifuge, centrifuging at a speed of 4500-5500 r / min for 8-10 min, discarding the supernatant, and obtaining a precipitate VII;
[0036] (4) adding 70-90 ml of ethanol to the precipitate VII, shaking to obtain a suspension VII, dispersing the suspension VII, placing the suspension VII in a centrifuge, centrifuging at a speed of 3000-3500 r / min for 5-7 min, discarding the supernatant, and obtaining a precipitate VIII;
[0037] (5) Drying the precipitate VIII at a temperature of 40-60° C. for 4-6 hours to obtain surface-modified silica powder.
[0038] The second object of the present invention is to prepare surface-modified silicon micropowder using a method for preparing surface-modified silicon micropowder.
[0039] The third object of the present invention is to apply the surface modified silicon micropowder mainly in the field of oil-water separation.
[0040] The beneficial effects of the present invention are:
[0041] The present application provides a method for preparing surface-modified silicon micropowder, which is simple and easy to operate, has high preparation efficiency, and can produce surface-modified silicon micropowder with high mechanical properties, high specific surface area, good chemical stability, and good surface super-hydrophobicity. The present application provides a method for preparing surface-modified silicon micropowder, which can overcome the shortcomings of current technology, solve the problem of poor mechanical properties in existing preparation methods, and increase its functional application.
[0042] The present application provides a method for preparing surface-modified silicon micropowder. The types and ratios of different silane coupling agents in the modification liquid will seriously affect the hydrolysis effect and the number of surface active groups of the silicon micropowder, which can effectively solve the problem of poor mechanics of the surface-modified silicon micropowder, thereby affecting the oil-water separation performance of the surface-modified silicon micropowder.
[0043] The present application provides a method for preparing surface-modified silicon micropowder, which uses different rotation speeds, different temperatures, and different times to prepare surface-modified silicon micropowder, which can affect the modification effect of the modification liquid and effectively solve the problem of poor mechanics of the surface-modified silicon micropowder.
[0044] The present application provides a method for preparing surface-modified silicon micropowder, which has low production cost, universal applicability, and is easy for large-scale production.
[0045] The present application provides a surface-modified silicon micropowder, which uses silicon micropowder particles of 800-1500 meshes, and can effectively improve the surface super-hydrophobicity of the surface-modified silicon micropowder.
[0046] The modification liquid used in the surface-modified silicon micropowder provided in the present application adopts deionized water, dimethyldimethoxysilane and triethoxymethylsilane, which can effectively improve the performance of the surface-modified silicon micropowder and solve the problem of poor mechanics.
[0047] The surface-modified silicon micropowder prepared by a preparation method of surface-modified silicon micropowder in the present invention has a high effect mainly in the field of oil-water separation, can effectively promote oil-water separation, and solve the problem of difficult treatment of oil and water.
[0048] In the present invention, the surface modified silicon micropowder is added to the oil-water emulsion, the emulsion quickly fades, and after standing the emulsion becomes clear and transparent, and the oil is absorbed by the modified surface modified silicon micropowder, indicating that the surface modified silicon micropowder has the ability to decompose oil pollution.
[0049] The addition of ammonia water in the present invention can provide an alkaline environment for the hydrolysis reaction of the mixture I and the modified liquid, thereby effectively improving the mechanical properties of the product, increasing the specific surface area of the product, and making the product have high surface super-hydrophobicity. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 Scanning images of the surface-modified silicon micropowder prepared in Example 1 under an electron microscope; (A) surface-modified silicon micropowder at a magnification of 10,000; (B) surface-modified silicon micropowder at a magnification of 40,000;
[0051] Figure 2 The surface modified silicon powder prepared in Example 1 is used for oil-water separation;
[0052] Figure 3 The scanning images of the silicon micropowder prepared in Comparative Example 1 under an electron microscope; (A) silicon micropowder at a magnification of 10,000; (B) silicon micropowder at a magnification of 40,000;
[0053] Figure 4 Figure 1 shows the surface modified silicon micropowder prepared in Comparative Example 1 for oil-water separation. DETAILED DESCRIPTION
[0054] In order to better understand the present invention, the technical solution of the present invention is described in detail with specific examples below, but the present invention is not limited thereto.
[0055] The raw materials used in the present invention are all commercially available products.
[0056] Example 1 A method for preparing surface-modified silicon micropowder
[0057] Step 1: Take 5 parts of silicon micropowder and 2 parts of sodium hydroxide according to the mass ratio, put the silicon micropowder and sodium hydroxide in a three-necked flask for hydroxylation, then add 100 ml of deionized water to the three-necked flask, and then stir and reflux at a temperature of 110°C for 2 hours. After the stirring is completed, continue stirring at room temperature for 12 hours to obtain a silicon micropowder solution.
[0058] Step 2: placing the silicon powder solution in a centrifuge, centrifuging at a speed of 3500 r / min for 3 min, discarding the supernatant, and obtaining precipitate I;
[0059] Add 60 ml of deionized water to the precipitate I, shake well to obtain suspension I, disperse the suspension I, place the suspension I in a centrifuge, centrifuge at a speed of 4000 r / min for 5 minutes, discard the supernatant, and obtain precipitate II;
[0060] Add 90 ml of deionized water to the precipitate II, shake well to obtain suspension II, disperse the suspension II, place the suspension II in a centrifuge, centrifuge at a speed of 4500 r / min for 10 min, discard the supernatant, and obtain precipitate III;
[0061] Add 70 ml of deionized water to the precipitate III, shake well, and obtain suspension III. Disperse the suspension III, place the suspension III in a centrifuge, centrifuge for 5 minutes at a speed of 3000 r / min, discard the supernatant, and obtain precipitate IV.
[0062] The precipitate IV was dried at 50°C for 5 hours, and finally the precipitate IV was ground to obtain silicon micropowder particles with a particle size of 1500 meshes.
[0063] Step 3: Add 1 part of ethanol solution and 2 parts of isopropanol solution to the silicon micropowder particles by volume ratio, and mix them evenly to obtain a reaction solvent;
[0064] (2) The reaction solvent was stirred and refluxed at 100° C. for 15 min to obtain a mixture I.
[0065] Step 4: Preparation of modified solution;
[0066] In a three-necked flask, 1 part of deionized water, 3 parts of dimethyldimethoxysilane and 3 parts of triethoxymethylsilane were added according to volume ratio, and mixed evenly to obtain a modified solution.
[0067] Step 5: Add the modified liquid droplets to the mixture I for hydrolysis, and add 10m of ammonia water at the same time, stir for 2 hours at a temperature of 90°C and a rotation speed of 3000r / min, and finally cool to room temperature, and continue stirring for 12 hours at a rotation speed of 2000r / min to obtain a mixture II;
[0068] Step 6: Place the mixture II in a centrifuge, centrifuge at a speed of 4000 r / min for 5 min, pour out the supernatant, and obtain a precipitate V;
[0069] Add 70 ml of ethanol to the precipitate V, shake well to obtain a suspension V, disperse the suspension V, place the suspension V in a centrifuge, centrifuge for 5-8 minutes at a speed of 4000-5000 r / min, discard the supernatant, and obtain a precipitate VI;
[0070] Add 100 ml of ethanol to the precipitate VI, shake well to obtain a suspension VI, disperse the suspension VI, place the suspension VI in a centrifuge, centrifuge at a speed of 5000 r / min for 10 min, discard the supernatant, and obtain a precipitate VII;
[0071] Add 90 ml of ethanol to the precipitate VII, shake well to obtain suspension VII, disperse the suspension VII, place the suspension VII in a centrifuge, centrifuge at a speed of 3000 r / min for 5-7 minutes, discard the supernatant, and obtain precipitate VIII;
[0072] The precipitate VIII was dried at 50°C for 5 hours to obtain surface-modified silica powder.
[0073] Step 7: Conduct oil-water separation experiment;
[0074] 0.5 g of Sudan III was added to 1 mL of chloroform, and after mixing, 60 mL of deionized water and 0.17 g of Tween 80 were added, and then stirred at room temperature for two hours to obtain an oil-water emulsion. Then, the original silicon micropowder and the surface-modified silicon micropowder obtained in Example 1 were added to the oil-water emulsion, and the oil-water separation was observed. It can be seen that the surface-modified silicon micropowder prepared by the present invention has oil-water separation performance.
[0075] Example 2 A method for preparing surface-modified silicon micropowder
[0076] Step 1: Take 4 parts of silicon micropowder and 1 part of sodium hydroxide according to the mass ratio, put the silicon micropowder and sodium hydroxide in a three-necked flask for hydroxylation, then add 80 ml of deionized water into the three-necked flask, and then stir and reflux at 90°C for 2.5 hours. After the stirring is completed, continue stirring at room temperature for hours to obtain a silicon micropowder solution.
[0077] Step 2: placing the silicon powder solution in a centrifuge, centrifuging at a speed of 3500 r / min for 4 min, discarding the supernatant, and obtaining precipitate I;
[0078] Add 50 ml of deionized water to the precipitate I, shake well to obtain suspension I, disperse the suspension I, place the suspension I in a centrifuge, centrifuge at a speed of 4000 r / min for 6 minutes, discard the supernatant, and obtain precipitate II;
[0079] Add 80 ml of deionized water to the precipitate II, shake well to obtain suspension II, disperse the suspension II, place the suspension II in a centrifuge, centrifuge at a speed of 4500 r / min for 8 minutes, discard the supernatant, and obtain precipitate III;
[0080] Add 80 ml of deionized water to the precipitate III, shake well, and obtain suspension III. Disperse the suspension III, place the suspension III in a centrifuge, centrifuge for 6 minutes at a speed of 3300 r / min, discard the supernatant, and obtain precipitate IV.
[0081] The precipitate IV was dried at 40°C for 4 hours, and finally the precipitate IV was ground to obtain silicon micropowder particles with a particle size of 800 meshes.
[0082] Step 3: Add 0.8 parts of ethanol solution and 1.8 parts of isopropanol solution to the silicon micropowder particles by volume, and mix well to obtain a reaction solvent;
[0083] The reaction solvent was stirred and refluxed at 80°C for 10 min to obtain a mixture I.
[0084] Step 4: Preparation of modified solution;
[0085] In a three-necked flask, 3 parts of deionized water, 5 parts of dimethyldimethoxysilane and 5 parts of triethoxymethylsilane were added according to volume ratio, and mixed evenly to obtain a modified solution.
[0086] Step 5: Add the modified liquid to the mixture I for hydrolysis, and add 11 ml of ammonia water at the same time, stir for 1.5 hours at a temperature of 75° C. and a speed of 2000 r / min, and finally cool to room temperature, and continue stirring for 11 hours at a speed of 1500 r / min to obtain a mixture II;
[0087] Step 6: Place the mixture II in a centrifuge, centrifuge at a speed of 3500 r / min for 4 min, pour out the supernatant, and obtain a precipitate V;
[0088] Add 50 ml of ethanol to the precipitate V, shake well to obtain a suspension V, disperse the suspension V, place the suspension V in a centrifuge, centrifuge at a speed of 4500 r / min for 5-8 minutes, discard the supernatant, and obtain a precipitate VI;
[0089] Add 80 ml of ethanol to the precipitate VI, shake well to obtain a suspension VI, disperse the suspension VI, place the suspension VI in a centrifuge, centrifuge at a speed of 4500 r / min for 8 minutes, discard the supernatant, and obtain a precipitate VII;
[0090] Add 70 ml of ethanol to the precipitate VII, shake well to obtain suspension VII, disperse the suspension VII, place the suspension VII in a centrifuge, centrifuge at a speed of 3000 r / min for 5 minutes, discard the supernatant, and obtain precipitate VIII;
[0091] The precipitate VIII was dried at 40°C for 4 hours to obtain surface-modified silica powder.
[0092] Step 7: Conduct oil-water separation experiment;
[0093] 0.5 g of Sudan III was added to 1 mL of chloroform, and after mixing, 60 mL of deionized water and 0.17 g of Tween 80 were added, and then stirred at room temperature for two hours to obtain an oil-water emulsion. Then, the original silicon micropowder and the surface-modified silicon micropowder obtained in Example 2 were added to the oil-water emulsion, and the oil-water separation was observed. It can be seen that the surface-modified silicon micropowder prepared by the present invention has oil-water separation performance.
[0094] Example 3 A method for preparing surface-modified silicon micropowder
[0095] Step 1: Take 6 parts of silicon micropowder and 3 parts of sodium hydroxide according to the mass ratio, put the silicon micropowder and sodium hydroxide in a three-necked flask for hydroxylation, then add 120 ml of deionized water to the three-necked flask, and then stir and reflux at 100°C for 3 hours. After the stirring is completed, continue stirring at room temperature for 9 hours to obtain a silicon micropowder solution.
[0096] Step 2: placing the silicon powder solution in a centrifuge, centrifuging at a speed of 3500 r / min for 3 min, discarding the supernatant, and obtaining precipitate I;
[0097] Add 70 ml of deionized water to the precipitate I, shake well to obtain suspension I, disperse the suspension I, place the suspension I in a centrifuge, centrifuge at a speed of 5000 r / min for 5-8 minutes, discard the supernatant, and obtain precipitate II;
[0098] Add 100 ml of deionized water to the precipitate II, shake well to obtain suspension II, disperse the suspension II, place the suspension II in a centrifuge, centrifuge at a speed of 4500 r / min for 8 minutes, discard the supernatant, and obtain precipitate III;
[0099] Add 90 ml of deionized water to the precipitate III, shake well, and obtain suspension III. Disperse the suspension III, place the suspension III in a centrifuge, centrifuge for 7 minutes at a speed of 3500 r / min, discard the supernatant, and obtain precipitate IV.
[0100] The precipitate IV was dried at 60°C for 6 hours, and finally the precipitate IV was ground to obtain silicon micropowder particles with a particle size of 800-1500 meshes.
[0101] Step 3: Add 1.2 parts of ethanol solution and 2.2 parts of isopropanol solution to the silicon micropowder particles by volume, mix well and obtain a reaction solvent;
[0102] The reaction solvent was stirred and refluxed at 100°C for 15 minutes to obtain a mixture I.
[0103] Step 4: Preparation of modified solution;
[0104] In a three-necked flask, 2 parts of deionized water, 4.5 parts of dimethyldimethoxysilane and 4.5 parts of triethoxymethylsilane were added according to volume ratio, and mixed evenly to obtain a modified solution.
[0105] Step 5: adding the modified liquid droplets to the mixture I for hydrolysis, adding 12m of aqueous ammonia, stirring at 80°C and 2000r / min for 3 hours, finally cooling to room temperature, and continuing stirring at 1800r / min for 13 hours to obtain a mixture II;
[0106] Step 6: Place the mixture II in a centrifuge, centrifuge for 5 min at a speed of 5000 r / min, pour out the supernatant, and obtain a precipitate V;
[0107] Add 70 ml of ethanol to the precipitate V, shake well to obtain a suspension V, disperse the suspension V, place the suspension V in a centrifuge, centrifuge for 5-8 minutes at a speed of 4000-5000 r / min, discard the supernatant, and obtain a precipitate VI;
[0108] Add 80-100 ml of ethanol to the precipitate VI, shake well to obtain a suspension VI, disperse the suspension VI, place the suspension VI in a centrifuge, centrifuge at a speed of 5500 r / min for 8 minutes, discard the supernatant, and obtain a precipitate VII;
[0109] Add 70 ml of ethanol to the precipitate VII, shake well to obtain suspension VII, disperse the suspension VII, place the suspension VII in a centrifuge, centrifuge at a speed of 3500 r / min for 7 minutes, discard the supernatant, and obtain precipitate VIII;
[0110] The precipitate VIII was dried at 60°C for 6 hours to obtain surface-modified silica powder.
[0111] Step 7: Conduct oil-water separation experiment;
[0112] 0.5 g of Sudan III was added to 1 mL of chloroform, and after being mixed evenly, 60 mL of deionized water and 0.17 g of Tween 80 were added, and then stirred at room temperature for two hours to obtain an oil-water emulsion. Then, the original silicon micropowder and the surface-modified silicon micropowder obtained in Example 3 were added to the oil-water emulsion, and the oil-water separation was observed. It can be seen that the surface-modified silicon micropowder prepared by the present invention has oil-water separation performance.
[0113] Comparative Example 1
[0114] The difference between Comparative Example 1 and Example 1 is that dimethyldimethoxysilane is replaced by diethoxydimethylsilane, and the other parts are exactly the same.
[0115] Comparative Example 2
[0116] The difference between Comparative Example 2 and Example 1 is that in the preparation of the modified liquid, deionized water is 1 part, dimethyldimethoxysilane is 1 part, and triethoxymethylsilane is 1 part, and the other contents are exactly the same.
[0117] Comparative Example 3
[0118] The difference between Comparative Example 3 and Example 1 is that in the preparation of the modified liquid, deionized water is 7 parts, dimethyldimethoxysilane is 8 parts, and triethoxymethylsilane is 8 parts, and the other parts are exactly the same.
[0119] The silicon micropowder prepared in Comparative Example 1 was subjected to an oil-water separation experiment.
[0120] Table 1 Properties of surface modified silicon micropowder and silicon micropowder prepared in Comparative Example 1
[0121]
[0122] When the contact angle θ>90° on the material surface, the liquid exhibits non-wetting properties on the solid surface. When the stable contact angle θ>150° and the rolling contact angle α<10° on the material surface, this type of material is a superhydrophobic material.
[0123] It can be seen from the above table that the addition of dimethyldimethoxysilane and diethoxydimethylsilane to the modified solution can cause a hydrolysis reaction, modify the surface of the silicon micropowder, and promote the oil-water separation effect. However, the modification effect of diethoxydimethylsilane is lower than that of dimethyldimethoxysilane. The super-hydrophobicity, specific surface area, and mechanical properties of the surface-modified silicon micropowder prepared by diethoxydimethylsilane are lower than those of the surface-modified silicon micropowder prepared by dimethyldimethoxysilane. Therefore, the surface-modified silicon micropowder prepared by adding diethoxydimethylsilane has a lower oil-water separation performance than the surface-modified silicon micropowder prepared by dimethyldimethoxysilane. The oil-water separation performance of the surface-modified silicon micropowder is lower than that of the surface-modified silicon micropowder prepared by dimethyldimethoxysilane. The experimental comparison of Example 1 and Comparative Example 1 and the figure and Figure 4It can be seen that the modification effect of comparative example 1 is inferior to that of example 1, and the time for oil-water separation is longer. It can be seen that preferentially using dimethyldimethoxysilane as a silane coupling agent to prepare surface-modified silicon micropowder can effectively promote oil-water separation.
[0124] It can be seen from the above table that excessive or insufficient addition of dimethyldimethoxysilane and diethoxydimethylsilane in the modifying liquid can affect the modification effect of the modifying liquid and the hydrolysis effect, resulting in poor super-hydrophobicity, poor specific surface area and poor mechanical properties of the prepared surface-modified silicon micropowder.
[0125] In the present invention, the surface modified silicon micropowder is added to the oil-water emulsion, the emulsion quickly fades, and after standing the emulsion becomes clear and transparent, and the oil is absorbed by the modified surface modified silicon micropowder, indicating that the surface modified silicon micropowder has the ability to decompose oil pollution.
[0126] pass Figure 2 It can be seen that when the surface-modified silica powder prepared in Example 1 is added to oil and water, before the oil and water are decomposed and the emulsion is broken, there are many small oil droplets in the emulsion; after the emulsion is broken, no oil droplets are observed in the emulsion, indicating that the oil droplets are adsorbed by the surface-modified silica powder, further proving that the silica powder modified by the silane coupling agent has demulsification performance, that is, oil-water separation performance.
[0127] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiment, it is still possible for a person skilled in the art to modify the technical solutions described in the aforementioned embodiment, or to perform equivalent replacements on parts thereof. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention. Although the specific implementation modes of the present invention have been described above in conjunction with the accompanying drawings, this is not a limitation on the protection scope of the present invention. A person skilled in the art should understand that, based on the technical solution of the present invention, various modifications or deformations that can be made by those skilled in the art without creative labor are still within the protection scope of the present invention.
Claims
1. A method for preparing surface-modified silicon micropowder, It is characterized in that The preparation method of the surface modified silicon micropowder: Step 1: Put the original silicon micropowder and sodium hydroxide into a three-necked flask for hydroxylation, then add deionized water into the three-necked flask, stir and reflux, and continue stirring at room temperature after the stirring is completed to obtain a silicon micropowder solution; Step 2: centrifuging, dispersing, drying and grinding the silicon micropowder solution to obtain silicon micropowder particles; Step 3: adding ethanol solution and isopropanol solution to silicon micropowder particles, mixing to obtain a reaction solvent, and finally dispersing the reaction solvent, stirring and refluxing to obtain a mixture I; Step 4: Preparation of modified solution; Step 5: adding the modified liquid droplets to the mixture I for hydrolysis, adding ammonia water to promote hydrolysis, stirring evenly, and obtaining the mixture II; Step 6: Centrifuge the mixture II, add ethanol, and then disperse, centrifuge and dry to obtain surface-modified silicon micropowder.
2. A method for preparing surface-modified silicon micropowder according to claim 1, Features: In the step 1, 4-6 parts of silicon micropowder and 1-3 parts of sodium hydroxide are taken according to the mass ratio, the silicon micropowder and the sodium hydroxide are placed in a three-necked flask for hydroxylation, and then 80-120 ml of deionized water is added to the three-necked flask, and then stirred and refluxed at a temperature of 90° C. to 110° C. for 2-3 hours. After the stirring is completed, stirring is continued at room temperature for 9-12 hours to obtain a silicon micropowder solution.
3. A method for preparing surface-modified silicon micropowder according to claim 1, Features: The specific steps of step 2 are: (1) placing the silicon powder solution in a centrifuge, centrifuging at a speed of 3500-5000 r / min for 3-5 min, discarding the supernatant, and obtaining precipitate I; (2) Add 50-70 ml of deionized water to the precipitate I, shake well to obtain a suspension I, disperse the suspension I, place the suspension I in a centrifuge, centrifuge at a speed of 4000-5000 r / min for 5-8 min, discard the supernatant, and obtain a precipitate II; (3) Add 80-100 ml of deionized water to the precipitate II, shake well to obtain suspension II, disperse the suspension II, place the suspension II in a centrifuge, centrifuge at a speed of 4500-5500 r / min for 8-10 min, discard the supernatant, and obtain precipitate III; (4) Add 70-90 ml of deionized water to the precipitate III, shake well, and obtain a suspension III. Disperse the suspension III, place the suspension III in a centrifuge, and centrifuge for 5-7 minutes at a speed of 3000-3500 r / min. Discard the supernatant to obtain a precipitate IV. (5) Drying the precipitate IV at a temperature of 40-60° C. for 4-6 hours, and finally grinding the precipitate IV to obtain silicon micropowder particles.
4. A method for preparing surface-modified silicon micropowder according to claim 1 or 3, Features: The particle size of the silicon micropowder particles is 800-1500 meshes.
5. The method for preparing surface-modified silicon micropowder according to claim 1, Features: The specific steps of step three are: (1) adding 0.8-1.2 parts of ethanol solution and 1.8-2.2 parts of isopropanol solution to silicon micropowder particles by volume, and mixing them uniformly to obtain a reaction solvent; (2) The reaction solvent is stirred and refluxed at a temperature of 80-100° C. for 10-15 minutes to obtain a mixture I.
6. The method for preparing surface-modified silicon micropowder according to claim 1, Features: The modified liquid includes deionized water, a silane coupling agent and triethoxymethylsilane; The preparation method of the modified liquid comprises adding 1-3 parts of deionized water, 3-5 parts of a silane coupling agent and 3-5 parts of triethoxymethylsilane in a three-necked flask according to the volume ratio, and mixing them evenly to obtain the modified liquid; The silane coupling agent is any one of dimethyldimethoxysilane or diethoxydimethylsilane.
7. The method for preparing surface-modified silicon micropowder according to claim 1, Features: In the step 5, the modified liquid droplets are added to the mixture I for hydrolysis, and then 10-12m of ammonia water is added, and stirred for 1.5-3 hours at a temperature of 75-90°C and a rotation speed of 2000-3000r / min, and finally cooled to room temperature, and stirred for 11-13 hours at a rotation speed of 1500-2000r / min to obtain a mixture II.
8. The method for preparing surface-modified silicon micropowder according to claim 1, Features: The specific steps of step six are: (1) placing the mixture II in a centrifuge, centrifuging for 3-5 min at a speed of 3500-5000 r / min, and pouring out the supernatant to obtain a precipitate V; (2) adding 50-70 ml of ethanol to the precipitate V, shaking to obtain a suspension V, dispersing the suspension V, placing the suspension V in a centrifuge, centrifuging at a speed of 4000-5000 r / min for 5-8 min, discarding the supernatant, and obtaining a precipitate VI; (3) adding 80-100 ml of ethanol to the precipitate VI, shaking to obtain a suspension VI, dispersing the suspension VI, placing the suspension VI in a centrifuge, centrifuging at a speed of 4500-5500 r / min for 8-10 min, discarding the supernatant, and obtaining a precipitate VII; (4) adding 70-90 ml of ethanol to the precipitate VII, shaking to obtain a suspension VII, dispersing the suspension VII, placing the suspension VII in a centrifuge, centrifuging at a speed of 3000-3500 r / min for 5-7 min, discarding the supernatant, and obtaining a precipitate VIII; (5) Drying the precipitate VIII at a temperature of 40-60° C. for 4-6 hours to obtain surface-modified silica powder.
9. A surface-modified silicon micropowder prepared according to the preparation method according to any one of claims 1 to 8.
10. Use of the surface-modified silicon micropowder according to claim 9, It is characterized in that Application of the surface modified silicon micropowder in the field of oil-water separation.