Photocatalyst and preparation method thereof
By distributing silicon crystals on the sponge and attaching titanium dioxide crystals, a porous structure photocatalyst is formed, which solves the complex problem of photocatalyst separation and recovery in suspension reactors, improves industrial feasibility and photocatalytic efficiency, and reduces operating costs and photocatalyst drain.
Patent Information
- Application Number
- CN202410779768.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-29
AI Technical Summary
The separation and recovery process of photocatalysts in suspension photocatalytic reactors is complicated, resulting in low feasibility of industrial application.
A porous structure photocatalyst composed of sponge, silicon crystal and titanium dioxide crystal is used. By distributing silicon dioxide and silicon carbide crystals on the sponge, and attaching titanium dioxide crystal under LED ultraviolet light, a transparent porous structure is formed to avoid the flow of photocatalyst and simplify Separation and recycling process.
It improves the industrial feasibility and photocatalytic efficiency of the photocatalyst, reduces the operating cost, avoids the loss of the photocatalyst, enhances the transparency and scattering of light, and improves the photocatalytic reaction efficiency.
Smart Images

Figure CN118847211A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the field of photocatalysis technology, and in particular to a photocatalyst and a method for preparing the photocatalyst. Background Art
[0002] Since the discovery of the photocatalytic process of semiconductor materials in the early 20th century, with the development of materials science and theoretical chemistry, the advantages of photocatalytic technology have been continuously revealed, and it is regarded as a reasonable alternative to deal with energy shortages and environmental pollution. Due to the advantages of mild conditions, stable and efficient performance, photocatalytic technology has been applied by many scientific researchers in recent years to air purification, sewage treatment, energy storage and conversion, and has attracted widespread attention.
[0003] The application of photocatalytic technology depends on photocatalytic reactors. Currently, common photocatalytic reactors include suspension reactors, fluidized bed reactors and fixed reactors. Among them, the suspension reactor completely mixes the powdered photocatalyst with the reaction system and then enters the light source coverage area of the photocatalytic reactor. In the photocatalytic reactor, it is necessary to keep the disturbance of the reaction system at all times to keep the reaction system in a uniformly mixed state. Although this type of photocatalytic reactor has a higher photocatalytic reaction rate. Among them, the fluidized bed reactor suspends solid photocatalyst powder or particles in a moving fluid through certain disturbance means. Such an operation enables the solid photocatalyst to have certain fluid characteristics and forms a solid fluidized state. Among them, the fixed reactor fixes the powdered or granular photocatalyst, and the fixed photocatalyst participates in the photocatalytic reaction on its exposed surface.
[0004] However, the inventors of the present invention found in the process of implementing the embodiments of the present invention that, for a slurry reactor, the separation and recovery process of the photocatalyst after the reaction is completed is relatively complicated, resulting in relatively low feasibility of industrialization. Summary of the invention
[0005] In view of the above problems, embodiments of the present invention provide a photocatalyst and a method for preparing the photocatalyst, which overcome the above problems or at least partially solve the above problems.
[0006] According to one aspect of an embodiment of the present invention, a photocatalyst is provided, comprising a sponge, silicon crystals, and titanium dioxide crystals; the silicon crystals are distributed in the sponge to form a porous skeleton, wherein the silicon crystals comprise silicon dioxide crystals and / or silicon carbide crystals; the titanium dioxide crystals are attached to the silicon crystals; the photocatalyst has a porous structure, and the transmittance of the photocatalyst under irradiation with a 25-watt LED ultraviolet lamp is 45-60%.
[0007] In an optional manner, the pore density of the sponge is 40-60 pp i.
[0008] In an optional manner, the sponge is a polyurethane sponge.
[0009] According to another aspect of an embodiment of the present invention, a method for preparing a photocatalyst is provided, comprising: dispersing nano-scale silicon dioxide powder in water to form a suspension, adjusting the pH value of the suspension to 10 and stirring to form a first solution; soaking a sponge in the first solution for 1-2 hours; vacuum drying the sponge soaked in the first solution to obtain a dry skeleton; sintering the dry skeleton to form a porous skeleton, wherein silicon crystals are distributed on the sponge in the porous skeleton, and the silicon crystals include silicon dioxide crystals and / or silicon carbide crystals; dissolving polyvinyl alcohol in a mass ratio of 5-10% in water, and then adding polyvinyl alcohol in a volume ratio of 15- 30% ethanol, stirring to obtain a second solution; immersing the porous skeleton in the second solution and aerating and disturbing it; adding a third solution to the second solution in which the porous skeleton is immersed, aerating and disturbing it, and then standing to allow titanium dioxide crystals to adhere to the porous skeleton, wherein the third solution is a solution obtained by mixing butyl titanate and anhydrous ethanol solution in a volume ratio of 1:1; drying the porous skeleton immersed in the second solution and added with the third solution to obtain the photocatalyst, wherein the photocatalyst has a porous structure and a light transmittance of 45-60% under irradiation of a 25-watt LED ultraviolet lamp.
[0010] In an optional manner, before the step of sintering the dried skeleton, the method also includes placing the dried skeleton in a muffle furnace for 1-2 hours, the air flow rate in the muffle furnace is 160-220 liters / hour, the heating rate of the muffle furnace is 1-2°C / minute, and the temperature in the muffle furnace is 400-800°C.
[0011] In an optional manner, the step of sintering the dried skeleton further comprises: heating the muffle furnace to 1200-1400° C. at a heating rate of 8-12° C. / min, and maintaining the temperature for 10-15 minutes.
[0012] In an optional manner, the volume percentage of the nano-scale silicon dioxide powder is 30-40%.
[0013] In an optional manner, the step of immersing the sponge in the first solution for 1-2 hours further comprises: immersing the sponge in the first solution for 1-2 hours, and during the immersion process, squeezing and releasing the sponge.
[0014] In an optional embodiment, the temperature of the water in which the polyvinyl alcohol is dissolved is 95°C.
[0015] The beneficial effects of the embodiments of the present invention include providing a photocatalyst, including: sponge, silicon crystals, titanium dioxide crystals; the silicon crystals are distributed in the sponge to form a porous skeleton, wherein the silicon crystals include silicon dioxide crystals and / or silicon carbide crystals; the titanium dioxide crystals are attached to the silicon crystals; wherein the photocatalyst is a porous structure, and the light transmittance of the photocatalyst under 25-watt LED ultraviolet lamp is 45-60%. The effective active component of the photocatalyst is titanium dioxide crystals, and the titanium dioxide crystals are attached to the porous skeleton formed by the silicon crystals and the sponge to form a whole, so that when the photocatalyst is photocatalyzed with the reaction system, the photocatalyst does not flow with the reaction system, and there is no need to separate and recover the photocatalyst, and the industrial feasibility is high.
[0016] In addition, the photocatalyst provided by the embodiment of the present invention does not flow with the reaction system when in use. Compared with the photocatalyst used in the fluidized bed reactor in the prior art, the photocatalyst provided by the present invention is not easy to lose, and its operating cost is low. In addition, the photocatalyst provided by the present invention is titanium dioxide attached to a porous skeleton formed by silicon crystals and sponges, so its light scattering degree is low and its photocatalytic efficiency is high. More importantly, the photocatalyst provided by the present invention is transparent, that is, the light transmittance under the irradiation of a 25-watt LED ultraviolet lamp is 45-60%, and its light scattering degree is low, which can effectively improve the photocatalytic efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] One or more embodiments are exemplarily described by pictures in the corresponding drawings, and these exemplified descriptions do not constitute limitations on the embodiments. Elements with the same reference numerals in the drawings represent similar elements, and unless otherwise stated, the figures in the drawings do not constitute proportional limitations.
[0018] Figure 1 It is a schematic diagram of a process for preparing a photocatalyst provided by an embodiment of the present invention;
[0019] Figure 2 It is a schematic flow chart of another method for preparing a photocatalyst provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0020] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0021] The embodiment of the present invention provides a photocatalyst, which includes a sponge, a silicon crystal, and a titanium dioxide crystal; the silicon crystal is distributed in the sponge to form a porous skeleton, wherein the silicon crystal includes a silicon dioxide crystal and / or a silicon carbide crystal; the titanium dioxide crystal is attached to the silicon crystal; the photocatalyst is a porous structure, and the light transmittance of the photocatalyst under the irradiation of a 25-watt LED ultraviolet lamp is 45-60%. The effective active component of the photocatalyst is the titanium dioxide crystal, which is attached to the porous skeleton formed by the silicon crystal and the sponge to form a whole, so that when the photocatalyst is photocatalyzed with the reaction system, the photocatalyst does not flow with the reaction system, and there is no problem of separating and recycling the photocatalyst, and the industrial feasibility is high.
[0022] In addition, the photocatalyst provided by the embodiment of the present invention does not flow with the reaction system when in use. Compared with the photocatalyst used in the fluidized bed reactor in the prior art, the photocatalyst provided by the present invention is not easy to lose, and its operating cost is low. In addition, the photocatalyst provided by the embodiment of the present invention is titanium dioxide attached to a porous skeleton formed by silicon crystals and sponges, which not only allows the reaction system to flow through, but also has a low degree of light scattering and a high photocatalytic efficiency. More importantly, the photocatalyst provided by the embodiment of the present invention is transparent, that is, the light transmittance under the irradiation of a 25-watt LED ultraviolet lamp is 45-60%, and its light scattering degree is low, which can effectively improve the photocatalytic efficiency.
[0023] In particular, compared with the suspension reactor in the prior art, the separation and recovery process of the photocatalyst after the reaction is completed is relatively complicated. When the photocatalyst provided in the embodiment of the present invention is used, since the photocatalyst does not flow, there is no problem of separation and recovery of the photocatalyst. Compared with the fluidized bed reactor in the prior art, which uses solid photocatalyst powder or particles, the solid photocatalyst powder or particles are suspended in the moving reaction system, and the solid photocatalyst powder or particles are easy to lose, and its operating cost is high. The photocatalyst provided in the embodiment of the present invention is a whole with a porous structure, which does not flow with the reaction system during the reaction, so the photocatalyst is not easy to lose. Compared with the fixed reactor in the prior art, it fixes the powdered or granular photocatalyst, and the fixed photocatalyst participates in the photocatalytic reaction on its exposed surface. Since the fixed photocatalyst has a limited surface area on its exposed surface, its scattering degree of light is high, which reduces the photocatalytic efficiency of the reaction system. The photocatalyst provided in the embodiment of the present invention is a porous structure and transparent. The light transmittance of the photocatalyst under the irradiation of a 25-watt LED ultraviolet lamp is 45-60%, and its scattering degree of light is low, which can effectively improve the photocatalytic efficiency.
[0024] In some embodiments, the pore density of the sponge is 40-60 pp i (Pores Per Line, the average number of pores per inch of length), so the pore size of the photocatalyst formed is appropriate and does not affect the permeation of water and gas. When the photocatalyst is applied to a specific photocatalytic reactor, there is no additional requirement for the water or air inlet pressure.
[0025] In some embodiments, the sponge is a polyurethane sponge.
[0026] In some embodiments, the polyurethane sponge is white, which is not likely to affect the light transmittance of the photocatalyst.
[0027] In some embodiments, the light transmittance of the polyurethane sponge under irradiation with a 25-watt LED ultraviolet lamp is less than 20%, which is not likely to affect the light transmittance of the photocatalyst finally formed.
[0028] In some embodiments, the porous framework has a pore density of 40-60 pp i.
[0029] In some embodiments, the photocatalyst has a pore density of 40-60 pp i.
[0030] It is worth noting that the shape of the photocatalyst can be a regular shape or any irregular shape, which can be set according to the specific needs of its specific application scenario.
[0031] The present invention provides a method for preparing a photocatalyst. Figure 1 , the preparation method of the photocatalyst comprises:
[0032] Step S10, dispersing nano-scale silicon dioxide powder in water to form a suspension, adjusting the pH value of the suspension to 10 and stirring to form a first solution.
[0033] In some embodiments, the volume percentage of the nano-scale silicon dioxide powder is 30-40%.
[0034] Step S20, soaking the sponge in the first solution for 1-2 hours.
[0035] In some embodiments, the step of soaking the sponge in the first solution for 1-2 hours further comprises soaking the sponge in the first solution for 1-2 hours, and squeezing and releasing the sponge during the soaking process. This configuration allows the sponge to be soaked in more of the first solution, i.e., more nano-silicon dioxide is attached to the sponge.
[0036] In some embodiments, the pore density of the sponge is 40-60 pp i, so the pore size of the formed photocatalyst is appropriate and does not affect the permeation of water and gas. When the photocatalyst is applied to a specific photocatalytic reactor, there is no additional requirement for the water or air inlet pressure.
[0037] In some embodiments, the sponge is a polyurethane sponge.
[0038] In some embodiments, the polyurethane sponge is white, which is not likely to affect the light transmittance of the photocatalyst.
[0039] In some embodiments, the light transmittance of the polyurethane sponge under irradiation with a 25-watt LED ultraviolet lamp is less than 20%, which is not likely to affect the light transmittance of the photocatalyst finally formed.
[0040] Step S30, vacuum drying the sponge impregnated with the first solution to obtain a dry skeleton.
[0041] In some embodiments, the set temperature of the vacuum drying may be 30-50° C., and correspondingly, the set time of the vacuum drying may be 16-36 hours.
[0042] Step S40, sintering the dried skeleton to form a porous skeleton, in which silicon crystals are distributed on the sponge, and the silicon crystals include silicon dioxide crystals and / or silicon carbide crystals.
[0043] In some embodiments, the step of sintering the dried skeleton further comprises: heating the muffle furnace to 1200-1400° C. at a heating rate of 8-12° C. / min and maintaining the temperature for 10-15 minutes.
[0044] In some embodiments, the porous framework has a pore density of 40-60 pp i.
[0045] In some embodiments, the pores of the porous skeleton correspond to pores of the sponge.
[0046] In some embodiments, see Figure 2 Before the step of sintering the dried skeleton, the method further comprises placing the dried skeleton in a muffle furnace for 1-2 hours, the air flow rate in the muffle furnace is 160-220 liters / hour, the heating rate of the muffle furnace is 1-2°C / minute, and the temperature in the muffle furnace is 400-800°C. Through this setting, the first solution impregnated on the sponge can be evenly heated, so that the catalytic effect of the photocatalyst finally formed is good.
[0047] Step S50, dissolving 5-10% polyvinyl alcohol by mass in water, then adding 15-30% ethanol by volume, and stirring to obtain a second solution.
[0048] In some embodiments, the temperature of the water for dissolving the polyvinyl alcohol can be 95° C., so as to facilitate the dissolution of the polyvinyl alcohol.
[0049] Step S60, immersing the porous framework in the second solution and aerating and disturbing the solution.
[0050] Step S70, adding a third solution to the second solution in which the porous skeleton is impregnated, and letting the solution stand after aeration disturbance to allow titanium dioxide crystals to adhere to the porous skeleton, wherein the third solution is a solution obtained by mixing butyl titanate and anhydrous ethanol solution in a volume ratio of 1:1.
[0051] It is worth noting that, in some embodiments, the step of adding the third solution to the second solution impregnated with the porous skeleton can be repeated 2-3 times, thereby increasing the content of the attached titanium dioxide and improving the catalytic function of the photocatalyst.
[0052] It is worth noting that the titanium dioxide crystals are synthesized by hydrolyzing the third solution after adding the second solution.
[0053] Step S80, drying the porous skeleton impregnated with the second solution and added with the third solution to obtain the photocatalyst, wherein the photocatalyst is a porous structure, and the light transmittance of the photocatalyst under irradiation of a 25-watt LED ultraviolet lamp is 45-60%.
[0054] In some embodiments, the pore density of the photocatalyst is 40-60 pp i, which means that the pore density of the photocatalyst is appropriate and does not affect the permeation of water and gas. When the photocatalyst is applied to a specific photocatalytic reactor, there is no additional requirement for the pressure of the water or gas inlet.
[0055] In some embodiments, a pore of the photocatalyst corresponds to a pore of the sponge.
[0056] In some embodiments, the temperature for drying the porous framework impregnated with the second solution and added with the third solution may be 40° C., and the corresponding drying time may be 12 hours.
[0057] According to the preparation method of the photocatalyst provided by the embodiment of the present application, the embodiment of the present invention forms a porous skeleton by impregnating a suspension of silicon dioxide on a sponge, and then drying and sintering the porous skeleton. The porous skeleton is transparent, and then titanium dioxide is attached to the porous skeleton. The photocatalyst thus formed has the function of a photocatalyst on the one hand, and on the other hand, the photocatalyst is a porous structure that allows an external reaction system (such as sewage to be treated) to flow through, that is, the formed photocatalyst may not flow with the external reaction system. In specific applications, there is no problem of separating and recovering the photocatalyst, and its industrial feasibility is high. In addition, relative to the photocatalyst used in the fluidized bed reactor in the prior art, the photocatalyst provided by the embodiment of the present invention does not flow with the reaction system when used, so the photocatalyst provided by the present invention is not easy to lose, and its operating cost is low. In addition, the photocatalyst provided by the embodiment of the present invention is titanium dioxide attached to a porous skeleton formed by silicon crystals and sponges, so it is not only available for the reaction system to flow through, but also has a low degree of light scattering, and its photocatalytic efficiency is high. More importantly, the photocatalyst provided by the embodiment of the present invention is transparent, that is, the light transmittance under the irradiation of a 25-watt LED ultraviolet lamp is 45-60%, and the light scattering degree thereof is low, which can effectively improve the photocatalytic efficiency.
[0058] In order to help readers understand the inventive concept of the embodiments of the present invention, the technical effects of using the embodiments of the present invention are demonstrated as follows.
[0059] Example
[0060] A nano-scale silica powder with a volume percentage of 35% is dispersed in water to form a suspension, and the pH value of the suspension is adjusted to 10 by adding 1 mol / L of tetramethylammonium hydroxide and stirred to form the first solution. A polyurethane sponge with a porosity of 50 pp i is selected as a template, and it is immersed in the first solution for 2 hours, and the sponge is continuously squeezed and released during the impregnation process so that more silica nanoparticles can be immersed in it. Then, the sponge after impregnation is taken out, and it is placed in an oven and vacuum dried at 30-50°C for 24 hours. The dried sponge is placed in a muffle furnace with an air flow rate of 200 liters / hour and a heating rate of 1°C / minute. After the furnace temperature reaches 600°C, it is maintained for 1-2 hours to ensure uniform heating. Subsequently, the furnace temperature is raised to 1300°C at a heating rate of 10°C / minute for sintering and maintained for 12 minutes. When the obtained material is cooled to room temperature, it is taken out for use as a porous skeleton.
[0061] The third solution is prepared by mixing butyl titanate with anhydrous ethanol solution in a ratio of 1:1 for standby use; polyvinyl alcohol with a mass ratio of 10% is dissolved in water at 95°C, and then ethanol with a volume ratio of 30% is added, and the second solution is obtained after stirring, and the porous skeleton is immersed in the second solution, and aeration disturbance is performed for 2 hours during the immersion process. The third solution is then added dropwise, and aeration disturbance is maintained. The operation is repeated 2-3 times, and then the solution is allowed to stand for 2 hours until the titanium dioxide crystals synthesized by hydrolysis are fully attached to the porous skeleton, and then taken out and dried in an oven at 40°C for 12 hours.
[0062] Comparative Example
[0063] A polyurethane sponge with a porosity of 50 pp i was selected as a template, and a photocatalyst was formed by coating using a sol-gel method, wherein the coating material was a silicon dioxide-titanium dioxide composite material.
[0064] Photocatalytic experiment
[0065] The photocatalysts obtained in the embodiment and the comparative example were added to a photocatalytic reactor with an aeration device at the bottom, the volume of which was 30 L, and then a 10 mg / L bisphenol A solution was continuously introduced into the reactor at a flow rate of 100 mL / min to conduct a continuous flow experiment. During the reaction, the bottom was continuously aerated to provide oxygen for the photocatalytic oxidation process and provide disturbance for the system.
[0066] The experimental results show that 3 hours after the start of the photocatalytic experiment, when the photocatalyst in the embodiment is used, the concentration of bisphenol A in the solution is reduced by 78.8%, and thereafter the effluent water maintains a small fluctuation, with the fluctuation amount being less than 10%. When the photocatalyst in the comparative example is used, the concentration of bisphenol A in the solution is reduced by 48.5%, which is 30.3% lower than that in the embodiment. That is, the photocatalytic efficiency of the photocatalyst provided in the embodiment of the present application can be increased by 30.3%.
[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may also be combined, the steps may be implemented in any order, and there are many other changes in different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they may still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A photocatalyst, characterized in that: include: Sponge, silicon crystals, titanium dioxide crystals; The silicon crystals are distributed in the sponge to form a porous skeleton, wherein the silicon crystals include silicon dioxide crystals and / or silicon carbide crystals; The titanium dioxide crystal is attached to the silicon crystal; The photocatalyst has a porous structure, and the light transmittance of the photocatalyst under the irradiation of a 25-watt LED ultraviolet lamp is 45-60%.
2. The photocatalyst according to claim 1, characterized in that The pore density of the sponge is 40-60ppi.
3. The photocatalyst according to claim 1, characterized in that The sponge is a polyurethane sponge.
4. A method for preparing a photocatalyst, characterized in that: include: Dispersing nano-scale silicon dioxide powder in water to form a suspension, adjusting the pH value of the suspension to 10 and stirring to form a first solution; Soak the sponge in the first solution for 1-2 hours; vacuum drying the sponge impregnated with the first solution to obtain a dry skeleton; Sintering the dried skeleton to form a porous skeleton, wherein silicon crystals are distributed on the sponge, and the silicon crystals include silicon dioxide crystals and / or silicon carbide crystals; Dissolving 5-10% polyvinyl alcohol by mass in water, then adding 15-30% ethanol by volume, and stirring to obtain a second solution; Immersing the porous framework in the second solution and aerating and disturbing it; Adding a third solution to the second solution in which the porous skeleton is impregnated, and letting the solution stand after aeration disturbance to allow titanium dioxide crystals to adhere to the porous skeleton, wherein the third solution is a solution obtained by mixing butyl titanate and anhydrous ethanol solution in a volume ratio of 1:1; The porous skeleton impregnated with the second solution and added with the third solution is dried to obtain the photocatalyst, wherein the photocatalyst is a porous structure and the light transmittance of the photocatalyst under irradiation of a 25-watt LED ultraviolet lamp is 45-60%.
5. The method for preparing a photocatalyst according to claim 4, characterized in that: Before the step of sintering the dried skeleton, the method further includes: placing the dried skeleton in a muffle furnace for 1-2 hours, the air flow in the muffle furnace is 160-220 liters / hour, the heating rate of the muffle furnace is 1-2°C / minute, and the temperature in the muffle furnace is 400-800°C.
6. The method for preparing a photocatalyst according to claim 5, characterized in that: The step of sintering the dried skeleton further comprises: The muffle furnace was heated to 1200-1400° C. at a heating rate of 8-12° C. / min and maintained for 10-15 minutes.
7. The method for preparing a photocatalyst according to claim 4, characterized in that: The volume percentage of the nano-scale silicon dioxide powder is 30-40%.
8. The method for preparing a photocatalyst according to claim 4, characterized in that: The step of soaking the sponge in the first solution for 1-2 hours further comprises soaking the sponge in the first solution for 1-2 hours, and squeezing and releasing the sponge during the soaking process.
9. The method for preparing a photocatalyst according to claim 4, characterized in that: The temperature of the water in which the polyvinyl alcohol is dissolved is 95°C.
Citation Information
Patent Citations
Integrated photocatalyst and preparation method thereof
CN102233267A
Polyurethane foam supported liver / graphene / titanium dioxide nano particle composite material, preparation method thereof and application thereof
CN105170132A
Recoverable elastic integral photocatalyst and preparation method thereof
CN108057457A
Porous adsorption supported light-catalyzed reaction film and preparation method and application thereof
CN108579821A
Titanium dioxide / silicon dioxide photocatalyst and preparation method thereof
CN109499562A