High-strength and high-toughness seamless steel tube and preparation method thereof

Through the use of composite heat treatment and modified quenching fluid, the problems of brittleness and cumbersome processes of seamless steel pipes after quenching are solved, the preparation of seamless steel pipes with high strength and toughness is achieved, the process steps are simplified and the performance is improved.

CN118847748APending Publication Date: 2024-10-29ZHEJIANG YONGSHANG SPECIAL MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410938930.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing seamless steel pipes require high-temperature tempering after quenching. The process steps are cumbersome and affect the construction period. At the same time, the brittleness of martensite after quenching leads to a decrease in toughness, making it difficult to achieve both high strength and high toughness.

Method used

Using a composite heat treatment method, the outer wall of the light tube is sprayed with an external water-based quenching liquid, and the inner wall is sprayed with an internal oil-based quenching liquid, so that the cooling speed of the outer wall is greater than that of the inner wall, forming a "hard on the outside and tough on the inside" structure, avoiding high-temperature tempering and reducing process steps and construction period. Combination of modified polyethylene glycol and polyvinyl alcohol in external aqueous quenching fluid to increase cooling rate and strength.

Benefits of technology

The high strength and toughness of seamless steel pipes are achieved, the yield strength and tensile strength are significantly improved, and the elongation reaches more than 17.9%. There is no need for high-temperature tempering and the process is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847748A_ABST
    Figure CN118847748A_ABST
Patent Text Reader

Abstract

The invention provides a high-strength and high-toughness seamless steel tube and a preparation method thereof, and belongs to the technical field of seamless steel tubes, the preparation method of the high-strength and high-toughness seamless steel tube comprises the following steps: S1, round billet continuous casting; s2, round billet rolling; heating, perforating and rolling the round billet to obtain a polished pipe; s3, composite heat treatment; after the light pipe is heated to 880-920 DEG C, external water-based quenching liquid is sprayed to the outer wall of the light pipe, meanwhile, internal oil-based quenching liquid is sprayed to the inner wall of the light pipe, the cooling speed of the outer wall of the light pipe is larger than that of the inner wall of the light pipe, and after the temperature of the outer wall of the light pipe and the temperature of the inner wall of the light pipe are both reduced to be lower than 240 DEG C, the light pipe is cooled to be in a closed state. And meanwhile, spraying of the external water-based quenching liquid and the internal oil-based quenching liquid is stopped, natural cooling is conducted, and the high-strength and high-toughness seamless steel pipe is obtained. High-temperature tempering is not needed, the process steps are reduced, the construction period is shortened, and meanwhile it is guaranteed that the manufactured seamless steel pipe has high strength and high toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of seamless steel pipes, and specifically relates to a high-strength and high-toughness seamless steel pipe and a preparation method thereof. Background Art

[0002] Quenching is an important heat treatment process to improve the strength and hardness of steel pipes. By heating to above the critical temperature and then cooling rapidly, the austenite in the steel is transformed into martensite, thereby significantly improving the strength and hardness of the steel pipe. During the quenching process, the austenite in the steel is transformed into martensite. Although this process can enhance the hardness, martensite is more brittle than austenite, which makes the material more likely to break when subjected to impact or deformation, resulting in a decrease in toughness.

[0003] In the prior art, high temperature tempering is used, that is, after quenching, the steel pipe is placed at a higher temperature for a period of time and then cooled, which can eliminate the internal stress caused by quenching and decompose the martensite to form a softer structure, such as troostite, so as to improve the toughness and ductility of the material while ensuring a certain strength / hardness. However, this quenching and tempering process has many steps and is relatively cumbersome, which affects the construction period. Summary of the invention

[0004] In order to solve the problems existing in the background technology, the present invention provides a high-strength and high-toughness seamless steel pipe and a preparation method thereof, which does not require high-temperature tempering, reduces process steps, shortens construction period, and ensures that the seamless steel pipe has both high strength and high toughness.

[0005] In order to achieve the above-mentioned object, in a first aspect, the present invention provides a method for preparing a high-strength and high-toughness seamless steel pipe, comprising the following steps:

[0006] S1. Continuous casting of round billets; the chemical composition of the round billets is as follows by mass percentage: C: 0.10-0.16%, Si: 0.15-0.25%, Cr: 0.8-1.2%, Mn: 0.4-0.65%, Al: 0.02-0.04%, Mo: 0.4-0.5%, Ni: 0.2-0.6%, V: 0.18-0.22%, Nb: 0.04-0.08%, P≤0.025%, S≤0.015%, N≤0.006% and rare earth elements: 0.06-0.08%, and the balance is iron and unavoidable impurities; the rare earth elements are composed of praseodymium and yttrium, and the mass ratio of praseodymium to yttrium is 1:0.8-1.2;

[0007] S2, round billet rolling: heating, punching and rolling the round billet to obtain a smooth tube;

[0008] S3, composite heat treatment; after heating the light tube to 880-920℃, spray external water-based quenching liquid on the outer wall of the light tube, and at the same time, spray internal oil-based quenching liquid on the inner wall of the light tube. The cooling rate of the outer wall of the light tube is greater than the cooling rate of the inner wall of the light tube. After the temperature of the outer wall of the light tube and the temperature of the inner wall of the light tube are both reduced to below 240℃, stop spraying the external water-based quenching liquid and the internal oil-based quenching liquid at the same time, and cool naturally to obtain a high-strength and high-toughness seamless steel tube.

[0009] Furthermore, the external aqueous quenching liquid includes modified polyethylene glycol, polyvinyl alcohol and water, and the mass ratio of the three is (15-20): (8-10): 70.

[0010] Furthermore, the preparation method of the modified polyethylene glycol is as follows:

[0011] a1. Add 3 g of cellulose to 50-60 g of dimethyl sulfoxide, stir and heat to 110°C, swell for 120 min, add 20-25 g of paraformaldehyde, keep the temperature constant for 90 min to completely dissolve the cellulose, and filter to obtain a cellulose solution;

[0012] a2. Dissolve 20 g of polyethylene glycol in 80 g of dimethyl sulfoxide, stir and heat to 70°C, add 5 g of 2,4-toluene diisocyanate and 0.05 g of dibutyltin dilaurate, react for 60 min, add the cellulose solution obtained in a1, react for 120 min, wait for the reaction product to cool to room temperature, add 450-600 mL of anhydrous ethanol, precipitate and regenerate at 70°C, then reduce the pressure and filter the precipitate, and vacuum dry to obtain modified polyethylene glycol.

[0013] Furthermore, the preparation method of the external aqueous quenching liquid is as follows:

[0014] A1. Slowly add polyvinyl alcohol into water, heat to 85-95°C, and continue stirring until it is completely dissolved to obtain a solution;

[0015] A2. After the solution obtained in A1 is cooled naturally to room temperature, modified polyethylene glycol is added and stirred continuously until it is completely dissolved to obtain an external aqueous quenching solution.

[0016] Furthermore, the internal oily quenching liquid includes poly-α-olefin, surfactant, antioxidant and mineral oil, and the mass ratio of the four is (5-10): (1-3): (0.1-1): 85.

[0017] Furthermore, the surfactant includes sodium stearate and / or potassium stearate.

[0018] Furthermore, the antioxidant includes antioxidant 1010 and / or antioxidant 1076.

[0019] Furthermore, the preparation method of the internal oily quenching liquid is as follows:

[0020] B1. Add antioxidant to half amount of mineral oil, heat to 40-70°C, stir at 80-150rpm for 20-30min to obtain antioxidant dispersed oil;

[0021] B2. Add the surfactant to the other half of the mineral oil, heat to 40-70°C, and stir at 80-150 rpm for 20-30 min to obtain an active dispersed oil;

[0022] B3. Mix the antioxidant dispersed oil obtained in B1 with the active dispersed oil obtained in B2, add poly-α-olefin, keep warm at 40-70°C, and stir at a speed of 150-200 rpm for 30-40 minutes to obtain an internal oily quenching liquid.

[0023] Furthermore, the specific operation of S2 is: when the round billet is heated to 1200-1280°C in an annular furnace, the inner hole is axially penetrated to obtain a hollow tube body; when the temperature is reduced to 1060°C-1100°C, rolling is performed to obtain a rough tube; when the temperature is reduced to 780°C-880°C, tension reduction is performed to obtain a smooth tube.

[0024] In a second aspect, the present invention provides a high-strength and high-toughness seamless steel pipe, which is produced by the above-mentioned preparation method.

[0025] This application has the following beneficial effects:

[0026] 1. The present invention adopts composite heat treatment. When an external aqueous quenching liquid is sprayed on the outer wall of the light tube, an internal oily quenching liquid is sprayed on the inner wall of the light tube. The cooling rate of the outer wall of the light tube is greater than the cooling rate of the inner wall of the light tube. The external rapid hardening is combined with the internal slow quenching to form a "hard outside and tough inside" structure. No high-temperature tempering is required. While reducing the process steps and shortening the construction period, it is ensured that the seamless steel pipe has both high strength and high toughness.

[0027] 2. In the preparation of the external aqueous quenching liquid, polyethylene glycol is modified with cellulose, and cellulose groups are introduced to enhance the interaction with water, thereby increasing the cooling rate and, to a certain extent, improving the strength (yield strength and tensile strength) of the seamless steel pipe; the addition of polyvinyl alcohol can form a double network structure with polyethylene glycol, which helps the aqueous quenching liquid to disperse heat more evenly during the cooling process, thereby improving the strength (yield strength and tensile strength) of the seamless steel pipe; and the above two work synergistically, and the double network hydrogel composed of the modified polyethylene glycol and polyvinyl alcohol shows higher water absorption capacity and better swelling performance, which helps to absorb and disperse heat more quickly, thereby synergistically improving the strength (yield strength and tensile strength) of the seamless steel pipe. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 , a comparative trend diagram of the strength (yield strength and tensile strength) of the seamless steel pipes obtained in Examples 1-9 of the present invention and Comparative Examples 1-9;

[0029] Figure 2 , a comparison trend chart of the toughness (elongation) of seamless steel pipes obtained from Examples 1-9 of the present invention and Comparative Examples 1-9. DETAILED DESCRIPTION

[0030] The present application is further described in detail below with reference to the embodiments.

[0031] Unless otherwise specified, the raw materials used in the examples and comparative examples of the present application are all commercially available.

[0032] Embodiment 1: A method for preparing a high-strength and high-toughness seamless steel pipe comprises the following steps:

[0033] S1. Continuous casting of round billets; the chemical compositions of the round billets are as follows by mass percentage: C: 0.14%, Si: 0.2%, Cr: 1%, Mn: 0.5%, Al: 0.03%, Mo: 0.45%, Ni: 0.4%, V: 0.2%, Nb: 0.06%, P: 0.02%, S: 0.01%, N: 0.005% and rare earth elements: 0.07%, and the balance is iron and unavoidable impurities; wherein the rare earth elements consist of praseodymium and yttrium, and the mass ratio of praseodymium to yttrium is 1:1.

[0034] S2, rolling of round billets; heating the round billet to 1240°C in a ring furnace, axially piercing the inner hole to obtain a hollow tube body; cooling to 1080°C, rolling to obtain a rough tube; cooling to 840°C, tension reducing to obtain a smooth tube.

[0035] S3, composite heat treatment; after heating the light tube to 900 ℃, place the light tube on a rotating device and drive the light tube to rotate, then spray external water-based quenching liquid on the outer wall of the light tube, and at the same time, spray internal oil-based quenching liquid on the inner wall of the light tube. The cooling rate of the outer wall of the light tube is greater than the cooling rate of the inner wall of the light tube. After the temperature of the outer wall of the light tube and the temperature of the inner wall of the light tube are both reduced to below 240 ℃, stop spraying the external water-based quenching liquid and the internal oil-based quenching liquid at the same time, and cool naturally to obtain a high-strength and high-toughness seamless steel tube.

[0036] The external aqueous quenching liquid includes modified polyethylene glycol, polyvinyl alcohol and water, and the mass ratio of the three is 17:9:70. The preparation method of the external aqueous quenching liquid is as follows: A1, slowly add polyvinyl alcohol into water, heat to 90°C, and continue to stir until it is completely dissolved to obtain a solution; A2, after the solution obtained in A1 is naturally cooled to room temperature, add modified polyethylene glycol, continue to stir until it is completely dissolved, and obtain the external aqueous quenching liquid.

[0037] Among them, polyvinyl alcohol (088-20G) was purchased from Shanghai Hongshi Industrial Co., Ltd.

[0038] The preparation method of modified polyethylene glycol is as follows: a1, 3g of cellulose (dried under reduced pressure and vacuum at 100°C for 48h to fully remove adsorbed moisture) is added to 55g of dimethyl sulfoxide (distilled under reduced pressure and the fraction at 160-163°C is collected), stirred and heated to 110°C, swollen for 120min, 22g of paraformaldehyde is added, and the temperature is kept constant for 90min to completely dissolve the cellulose, and a cellulose solution is obtained by suction filtration; a2, 20g of polyethylene glycol is dissolved in 80g of dimethyl sulfoxide, stirred and heated to 70°C, 5g of 2,4-toluene diisocyanate and 0.05g of dibutyltin dilaurate are added, and after reacting for 60min, the cellulose solution obtained in a1 is added, and the reaction is continued for 120min. After the reaction product is cooled to room temperature, 500mL of anhydrous ethanol is added, and precipitation regeneration is carried out at 70°C, and the precipitate is then filtered under reduced pressure and vacuum dried to obtain modified polyethylene glycol.

[0039] Cellulose (cellophane regenerated cellulose) was purchased from Shandong Henglian New Materials Co., Ltd. Dimethyl sulfoxide was purchased from Shanghai Longti Chemical Co., Ltd. Paraformaldehyde (content ≥ 99%) was purchased from Langfang Pengcai Fine Chemical Co., Ltd. Polyethylene glycol (PEG4000) was purchased from Shanghai Beko Chemical Co., Ltd. 2,4-Toluene diisocyanate was purchased from Shanghai Ruidong Chemical Group Co., Ltd. Dibutyltin dilaurate was purchased from Hubei Longxin Chemical Industry Co., Ltd.

[0040] The internal oily quenching liquid includes polyalphaolefin, surfactant, antioxidant and mineral oil, and the mass ratio of the four is 8:2:0.5:85. Among them, polyalphaolefin (Exxon PAO-6) was purchased from Shenzhen Jinze Wanchang Petrochemical Co., Ltd. The surfactant is sodium stearate. The antioxidant includes antioxidant 1010 and antioxidant 1076, and the mass ratio of the two is 1:1. Antioxidant 1010 and antioxidant 1076 are purchased from Henan Wanshan New Materials Technology Co., Ltd. The mineral oil is 60N base oil, purchased from Guangzhou Mingen Petroleum Products Co., Ltd.

[0041] The preparation method of the internal oily quenching liquid is as follows: B1. Add an antioxidant to half of the mineral oil, heat to 55°C, and stir at 115 rpm for 25 minutes to obtain an antioxidant dispersed oil; B2. Add a surfactant to the other half of the mineral oil, heat to 55°C, and stir at 115 rpm for 25 minutes to obtain an active dispersed oil; B3. Mix the antioxidant dispersed oil obtained in B1 and the active dispersed oil obtained in B2, add polyα-olefin, keep warm at 60°C, and stir at 170 rpm for 35 minutes to obtain an internal oily quenching liquid.

[0042] Example 2: The difference between this example and Example 1 is: S1, round billet continuous casting; the chemical composition of the round billet is as follows by mass percentage: C: 0.10%, Si: 0.15%, Cr: 0.8%, Mn: 0.4%, Al: 0.02%, Mo: 0.4%, Ni: 0.2%, V: 0.18%, Nb: 0.04%, P: 0.02%, S: 0.01%, N: 0.006% and rare earth elements: 0.06%, and the balance is iron and unavoidable impurities; the rare earth elements are composed of praseodymium and yttrium, and the mass ratio of praseodymium to yttrium is 1:0.8.

[0043] Example 3: The difference between this example and Example 1 is: S1, round billet continuous casting; the chemical composition of the round billet is as follows by mass percentage: C: 0.16%, Si: 0.25%, Cr: 1.2%, Mn: 0.65%, Al: 0.04%, Mo: 0.5%, Ni: 0.6%, V: 0.22%, Nb: 0.08%, P: 0.025%, S: 0.015%, N: 0.006% and rare earth elements: 0.08%, and the balance is iron and unavoidable impurities; the rare earth elements are composed of praseodymium and yttrium, and the mass ratio of praseodymium to yttrium is 1:1.2.

[0044] Example 4: The difference between this example and Example 1 is that the external aqueous quenching liquid includes modified polyethylene glycol, polyvinyl alcohol and water, and the mass ratio of the three is 15:8:70.

[0045] The preparation method of the external aqueous quenching liquid is as follows: A1. Slowly add polyvinyl alcohol into water, heat it to 90°C, and continue to stir until it is completely dissolved to obtain a solution; A2. After the solution obtained in A1 is naturally cooled to room temperature, add modified polyethylene glycol, and continue to stir until it is completely dissolved to obtain an external aqueous quenching liquid.

[0046] Example 5: The difference between this example and Example 1 is that the external aqueous quenching liquid includes modified polyethylene glycol, polyvinyl alcohol and water, and the mass ratio of the three is 20:10:70.

[0047] The preparation method of the external aqueous quenching liquid is as follows: A1. Slowly add polyvinyl alcohol into water, heat it to 90°C, and continue to stir until it is completely dissolved to obtain a solution; A2. After the solution obtained in A1 is naturally cooled to room temperature, add modified polyethylene glycol, and continue to stir until it is completely dissolved to obtain an external aqueous quenching liquid.

[0048] Example 6: The difference between this example and Example 1 is that the preparation method of modified polyethylene glycol is as follows: a1. 3 g of cellulose (dried under reduced pressure and vacuum at 100°C for 48 h to fully remove adsorbed water) is added to 50 g of dimethyl sulfoxide (distilled under reduced pressure and the fraction at 160-163°C is collected), heated to 110°C with stirring, swollen for 120 min, 20 g of paraformaldehyde is added, and the temperature is kept constant for 90 min to completely dissolve the cellulose, and filtered to obtain cellulose. a2. Dissolve 20 g of polyethylene glycol in 80 g of dimethyl sulfoxide, stir and heat to 70°C, add 5 g of 2,4-toluene diisocyanate and 0.05 g of dibutyltin dilaurate, react for 60 min, add the cellulose solution obtained in a1, react for 120 min, wait for the reaction product to cool to room temperature, add 450 mL of anhydrous ethanol, precipitate and regenerate at 70°C, then reduce the pressure and filter the precipitate, and vacuum dry to obtain modified polyethylene glycol.

[0049] Example 7: The difference between this example and Example 1 is that the preparation method of modified polyethylene glycol is as follows: a1. 3 g of cellulose (dried under reduced pressure and vacuum at 100°C for 48 h to fully remove adsorbed water) is added to 60 g of dimethyl sulfoxide (distilled under reduced pressure and the fraction at 160-163°C is collected), heated to 110°C with stirring, swollen for 120 min, 25 g of paraformaldehyde is added, and the temperature is kept constant for 90 min to completely dissolve the cellulose, and filtered to obtain cellulose. a2. Dissolve 20 g of polyethylene glycol in 80 g of dimethyl sulfoxide, stir and heat to 70°C, add 5 g of 2,4-toluene diisocyanate and 0.05 g of dibutyltin dilaurate, react for 60 min, add the cellulose solution obtained in a1, react for 120 min, wait for the reaction product to cool to room temperature, add 600 mL of anhydrous ethanol, precipitate and regenerate at 70°C, then reduce the pressure and filter the precipitate, and vacuum dry to obtain modified polyethylene glycol.

[0050] Example 8: The difference between this example and Example 1 is that the internal oily quenching liquid includes poly-α-olefin, surfactant, antioxidant and mineral oil, and the mass ratio of the four is 5:1:0.1:85.

[0051] The preparation method of the internal oily quenching liquid is as follows: B1. Add an antioxidant to half of the mineral oil, heat to 40°C, and stir at 80 rpm for 20 minutes to obtain an antioxidant dispersed oil; B2. Add a surfactant to the other half of the mineral oil, heat to 40°C, and stir at 80 rpm for 20 minutes to obtain an active dispersed oil; B3. Mix the antioxidant dispersed oil obtained in B1 and the active dispersed oil obtained in B2, add polyα-olefin, keep warm at 40°C, and stir at 150 rpm for 30 minutes to obtain an internal oily quenching liquid.

[0052] Example 9: The difference between this example and Example 1 is that the internal oily quenching liquid includes poly-α-olefin, surfactant, antioxidant and mineral oil, and the mass ratio of the four is 10:3:1:85.

[0053] The preparation method of the internal oily quenching liquid is as follows: B1. Add an antioxidant to half of the mineral oil, heat to 70°C, and stir at 150 rpm for 30 minutes to obtain an antioxidant dispersed oil; B2. Add a surfactant to the other half of the mineral oil, heat to 70°C, and stir at 150 rpm for 30 minutes to obtain an active dispersed oil; B3. Mix the antioxidant dispersed oil obtained in B1 and the active dispersed oil obtained in B2, add polyα-olefin, keep warm at 70°C, and stir at 200 rpm for 40 minutes to obtain an internal oily quenching liquid.

[0054] Comparative Example 1: The difference between this comparative example and Example 1 is that the external aqueous quenching liquid is sprayed on both the outer wall and the inner wall of the light tube.

[0055] Specifically, S3, composite heat treatment; after heating the light tube to 900°C, place the light tube on a rotating device and drive the light tube to rotate, then spray external aqueous quenching liquid on the outer wall and inner wall of the light tube, after the temperature of the outer wall of the light tube and the temperature of the inner wall of the light tube are both reduced to below 240°C, stop spraying the external aqueous quenching liquid at the same time, and cool naturally to obtain a high-strength and high-toughness seamless steel pipe.

[0056] Comparative Example 2: The difference between this comparative example and Example 1 is that the internal oily quenching liquid is sprayed on both the outer wall and the inner wall of the light tube.

[0057] Specifically, S3, composite heat treatment; after heating the light tube to 900°C, place the light tube on a rotating device and drive the light tube to rotate, then spray the internal oily quenching liquid on the outer wall and the inner wall of the light tube, and after the temperature of the outer wall of the light tube and the temperature of the inner wall of the light tube are both reduced to below 240°C, stop spraying the internal oily quenching liquid at the same time, and cool naturally to obtain a high-strength and high-toughness seamless steel pipe.

[0058] Comparative Example 3: The difference between this comparative example and Example 1 is that the internal oily quenching liquid is sprayed on the outer wall of the light tube, and the external water-based quenching liquid is sprayed on the inner wall of the light tube.

[0059] Specifically, S3, composite heat treatment; after heating the light tube to 900°C, place the light tube on a rotating device and drive the light tube to rotate, then spray the inner oily quenching liquid on the outer wall of the light tube, and at the same time, spray the outer water-based quenching liquid on the inner wall of the light tube. The cooling rate of the outer wall of the light tube is lower than the cooling rate of the inner wall of the light tube. After the temperature of the outer wall of the light tube and the temperature of the inner wall of the light tube are both reduced to below 240°C, stop spraying the external water-based quenching liquid and the internal oily quenching liquid at the same time, and cool naturally to obtain a high-strength and high-toughness seamless steel tube.

[0060] Comparative Example 4: This comparative example differs from Example 1 in that in the preparation of the external aqueous quenching liquid, the modified polyethylene glycol is replaced by polyethylene glycol.

[0061] Specifically, the external aqueous quenching liquid includes polyethylene glycol, polyvinyl alcohol and water, and the mass ratio of the three is 17:9:70.

[0062] Comparative Example 5: The difference between this comparative example and comparative example 4 is that external aqueous quenching liquid is sprayed on both the outer wall and the inner wall of the light tube.

[0063] Comparative Example 6: The difference between this comparative example and comparative example 4 is that in the preparation of the external aqueous quenching liquid, polyvinyl alcohol is replaced by polyethylene glycol.

[0064] Specifically, the external aqueous quenching liquid includes polyethylene glycol and water, and the mass ratio of the two is 26:70.

[0065] Comparative Example 7: The difference between this comparative example and comparative example 6 is that external aqueous quenching liquid is sprayed on both the outer wall and the inner wall of the light tube.

[0066] Comparative Example 8: The difference between this comparative example and Example 1 is that in the preparation of the external aqueous quenching liquid, polyvinyl alcohol is replaced by modified polyethylene glycol.

[0067] Comparative Example 9: The difference between this comparative example and comparative example 8 is that external aqueous quenching liquid is sprayed on both the outer wall and the inner wall of the light tube.

[0068] Test example: Test object: products of Examples 1-9 and Comparative Examples 1-9.

[0069] Test items and basis: GB / T 228.1-2021 "Tensile test of metallic materials - Part 1: Test method at room temperature" is used to test the tensile strength, yield strength and elongation.

[0070] Test results: See Table 1.

[0071] Table 1. Test data of products of Examples 1-9 and Comparative Examples 1-9

[0072] Yield strength / MPa Tensile strength / MPa Elongation / % Example 1 806 1004 18.5 Example 2 790 989 18.7 Example 3 814 1011 18.9 Example 4 810 1017 19.3 Example 5 797 982 17.9 Example 6 794 995 18.8 Example 7 822 1026 19.1 Example 8 801 1008 18.3 Example 9 806 998 18.2 Comparative Example 1 889 1119 11.6 Comparative Example 2 741 915 22.5 Comparative Example 3 780 969 16.7 Comparative Example 4 781 973 17.6 Comparative Example 5 823 1043 12.3 Comparative Example 6 757 944 17.3 Comparative Example 7 787 984 13.3 Comparative Example 8 773 965 17.8 Comparative Example 9 813 1039 12.8

[0073] Result analysis: Analyze Examples 1-9 and combine the data in Table 1 and Figure 1-2 It can be seen that the present invention does not require high-temperature tempering, reduces process steps, shortens construction period, and ensures that the seamless steel pipe has both high strength (yield strength of up to 790MPa or more, tensile strength of up to 982MPa or more) and high toughness (elongation of up to 17.9% or more).

[0074] Analyze Example 1 and Comparative Examples 1-3 and combine the data in Table 1 and Figure 1-2It can be seen that compared with Example 1 (the outer wall of the light tube uses the external aqueous quenching liquid of the present invention and the inner wall uses the internal oily quenching liquid of the present invention), when both the inner and outer walls of the light tube are quenched with the external aqueous quenching liquid of the present invention, the strength (yield strength and tensile strength) of the obtained seamless steel pipe is improved, but the toughness (elongation) is greatly reduced; when both the inner and outer walls of the light tube are quenched with the internal oily quenching liquid of the present invention, the toughness (elongation) of the obtained seamless steel pipe is improved, but the strength (yield strength and tensile strength) is greatly reduced; when the outer wall of the light tube uses the internal oily quenching liquid of the present invention and the inner wall uses the external aqueous quenching liquid of the present invention, the strength (yield strength and tensile strength) and toughness (elongation) of the obtained seamless steel pipe are slightly reduced.

[0075] Analyze Example 1 and Comparative Examples 4-9 and combine the data in Table 1 and Figure 1-2 It can be seen that when the external aqueous quenching liquid prepared by the present invention is used to quench the outer wall of the light tube, in the preparation of the external aqueous quenching liquid, the addition of polyvinyl alcohol can cooperate with polyethylene glycol to improve the strength (yield strength and tensile strength) of the seamless steel pipe; the modification treatment of polyethylene glycol can also improve the strength (yield strength and tensile strength) of the seamless steel pipe; and there is a synergistic effect between the two, which can synergistically improve the strength (yield strength and tensile strength) of the seamless steel pipe; while improving the strength, the toughness (elongation) of the seamless steel pipe is not greatly affected.

[0076] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0077] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing a high-strength and high-toughness seamless steel pipe, characterized in that: The steps include: S1. Continuous casting of round billets; the chemical composition of the round billets is as follows by mass percentage: C: 0.10-0.16%, Si: 0.15-0.25%, Cr: 0.8-1.2%, Mn: 0.4-0.65%, Al: 0.02-0.04%, Mo: 0.4-0.5%, Ni: 0.2-0.6%, V: 0.18-0.22%, Nb: 0.04-0.08%, P≤0.025%, S≤0.015%, N≤0.006% and rare earth elements: 0.06-0.08%, and the balance is iron and unavoidable impurities; the rare earth elements are composed of praseodymium and yttrium, and the mass ratio of praseodymium to yttrium is 1:0.8-1.2; S2, round billet rolling: heating, punching and rolling the round billet to obtain a smooth tube; S3, composite heat treatment; after heating the light tube to 880-920℃, spray external water-based quenching liquid on the outer wall of the light tube, and at the same time, spray internal oil-based quenching liquid on the inner wall of the light tube. The cooling rate of the outer wall of the light tube is greater than the cooling rate of the inner wall of the light tube. After the temperature of the outer wall of the light tube and the temperature of the inner wall of the light tube are both reduced to below 240℃, stop spraying the external water-based quenching liquid and the internal oil-based quenching liquid at the same time, and cool naturally to obtain a high-strength and high-toughness seamless steel tube.

2. The method for preparing a high-strength and high-toughness seamless steel pipe according to claim 1, characterized in that: The external aqueous quenching liquid comprises modified polyethylene glycol, polyvinyl alcohol and water, and the mass ratio of the three is (15-20):(8-10):

70.

3. The method for preparing a high-strength and high-toughness seamless steel pipe according to claim 2, characterized in that: The preparation method of the modified polyethylene glycol is as follows: a1. Add 3 g of cellulose to 50-60 g of dimethyl sulfoxide, stir and heat to 110°C, swell for 120 min, add 20-25 g of paraformaldehyde, keep the temperature constant for 90 min to completely dissolve the cellulose, and filter to obtain a cellulose solution; a2. Dissolve 20 g of polyethylene glycol in 80 g of dimethyl sulfoxide, stir and heat to 70°C, add 5 g of 2,4-toluene diisocyanate and 0.05 g of dibutyltin dilaurate, react for 60 min, add the cellulose solution obtained in a1, react for 120 min, wait for the reaction product to cool to room temperature, add 450-600 mL of anhydrous ethanol, precipitate and regenerate at 70°C, then reduce the pressure and filter the precipitate, and vacuum dry to obtain modified polyethylene glycol.

4. The method for preparing a high-strength and high-toughness seamless steel pipe according to claim 2 or 3, characterized in that: The preparation method of the external aqueous quenching liquid is as follows: A1. Slowly add polyvinyl alcohol into water, heat to 85-95°C, and continue stirring until it is completely dissolved to obtain a solution; A2. After the solution obtained in A1 is cooled naturally to room temperature, modified polyethylene glycol is added and stirred continuously until it is completely dissolved to obtain an external aqueous quenching solution.

5. The method for preparing a high-strength and high-toughness seamless steel pipe according to claim 1, characterized in that: The internal oily quenching liquid comprises poly-alpha-olefin, surfactant, antioxidant and mineral oil, and the mass ratio of the four is (5-10):(1-3):(0.1-1):

85.

6. The method for preparing a high-strength and high-toughness seamless steel pipe according to claim 5, characterized in that: The surfactant includes sodium stearate and / or potassium stearate.

7. The method for preparing a high-strength and high-toughness seamless steel pipe according to claim 5, characterized in that: The antioxidant includes antioxidant 1010 and / or antioxidant 1076.

8. The method for preparing a high-strength and high-toughness seamless steel pipe according to claim 5, 6 or 7, characterized in that: The preparation method of the internal oily quenching liquid is as follows: B1. Add antioxidant to half amount of mineral oil, heat to 40-70°C, stir at 80-150rpm for 20-30min to obtain antioxidant dispersed oil; B2. Add the surfactant to the other half of the mineral oil, heat to 40-70°C, and stir at 80-150 rpm for 20-30 min to obtain an active dispersed oil; B3. Mix the antioxidant dispersed oil obtained in B1 with the active dispersed oil obtained in B2, add poly-α-olefin, keep warm at 40-70°C, and stir at a speed of 150-200 rpm for 30-40 minutes to obtain an internal oily quenching liquid.

9. The method for preparing a high-strength and high-toughness seamless steel pipe according to claim 1, characterized in that: The specific operation of S2 is: when the round billet is heated to 1200-1280℃ in an annular furnace, the inner hole is axially penetrated to obtain a hollow tube body; when the temperature is lowered to 1060℃-1100℃, rolling is performed to obtain a rough tube; when the temperature is lowered to 780℃-880℃, tension reduction is performed to obtain a smooth tube.

10. A high-strength and high-toughness seamless steel pipe, characterized in that: The method is prepared according to any one of claims 1 to 9.