Forming method of small-size thin-wall wrinkled filter screen for hydraulic system

By combining electron beam cutting and stamping/spinning/rolling processes, the problem of forming micro-pleated filters with complex curved surfaces in hydraulic systems is solved, tearing defects are avoided, processing accuracy and quality are improved, and it is suitable for small-sized, highly complex applications. parts.

CN118848435AActive Publication Date: 2024-10-29XIAN UNIV OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410949899.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-29
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

In hydraulic systems, it is difficult to form complex curved micro-pleated filters, especially in maintaining the shape of regular circular micropores, and existing methods are prone to cracking defects.

Method used

Combining electron beam cutting technology with stamping/spinning/rolling processes, a large depth-to-diameter ratio micro-through hole array is first processed on the plate, and then the curved screen structure is formed by stamping/spinning machine tools, and then completed using stamping/rolling machine tools. The processing of wrinkles ensures that only the appearance of the curved surface will be deformed without structural deformation.

Benefits of technology

It effectively avoids the cracking defects at the micro-through holes of the filter, improves the processing accuracy and quality, and is suitable for the forming of small-sized and high-complexity parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118848435A_ABST
    Figure CN118848435A_ABST
Patent Text Reader

Abstract

The invention discloses a forming method of a small-size thin-wall wrinkled filter screen for a hydraulic system, which comprises the following steps: processing a micro-through hole surface structure with a large depth-diameter ratio on an original plate through an electron beam cutting method to form a surface micro-through hole flat plate; fitting the size of each part of the unfolded curved surface of the folded filter screen model by unfolding the folded surface of the folded filter screen model, then carrying out stamping / spinning shaping on the micro-through-hole flat plate through a stamping / spinning machine tool, processing the micro-through-hole flat plate into a curved-surface screen, and cutting the end part of the curved-surface screen at the same time; and stamping / rolling shaping is conducted on the curved-surface screen through a stamping / rolling machine tool, the curved-surface screen with wrinkles is machined, and meanwhile end cutting is conducted on the curved-surface screen with the wrinkles. The forming method is efficient, convenient and fast, the machining precision is high, multiple forming methods can be combined, the micro-through-hole position of the folded filter screen machined through the method does not have the tension crack defect, and the forming method is particularly suitable for machining of small-size and high-complexity parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydraulic system component processing methods, and in particular relates to a forming method for a small-size thin-wall pleated filter screen for a hydraulic system. Background Art

[0002] In the hydraulic system of the machine, such as throttles, safety valves and other sensitive components are resistant to small particles of contaminants, however, large particles of contaminants can cause these components to fail, leading to catastrophic consequences. When the hydraulic system of the machine is running, the role of the filter is to maintain the cleanliness of the main channel, and the large particles of contaminants introduced after a period of operation need to be protected by a pleated filter. This pleated filter is usually located upstream of important components such as check valves, throttle valves and safety valves, or integrated with these components. If the filter malfunctions, it will quickly cause failures and may even cause more serious risks.

[0003] The hydraulic system of the machine is extremely complex, involving many different types of parts. Since the parts using pleated screens have different shapes, the pleated screens required for each part will also be adjusted according to the shape of the part. The structure of some parts is relatively regular, but there are still a large number of parts that need to be equipped with pleated screens with complex curved surfaces. In addition, due to the small size of these parts, many of them are at the millimeter level, and the overall structure is less than one centimeter, it is extremely difficult to form such tiny parts with microchannels and complex curved surfaces. For example, for a curved pleated screen with a length of several millimeters, the pleated surface is short and the shape is complex, which makes it difficult to form the pleated surface. At the same time, it is also difficult to form micropores on the pleated surface, especially at the root of the pleats. It is particularly difficult to maintain the shape of the micropores with regular circular through holes. Based on this, a Chinese patent with publication number CN113843586B and publication date December 28, 2021 discloses a combined processing method for complex curved pleated filter screens for aircraft hydraulic systems. This method is particularly suitable for the processing of small-sized, highly complex parts, but the processing method is too single and does not take into account the problem of cracking defects that are prone to occur when drawing perforated mesh plates into spherical parts.

[0004] Electron beam cutting technology uses the energy of electron beam to melt the material to be cut, and forms the incision through evaporation of the melt or gravity flow. This technology can usually achieve the processing of micro holes with large depth-to-diameter ratio. Its advantages include high power density, small workpiece deformation, high precision, and almost no material selectivity. At present, electron beam cutting technology is mainly used in semiconductor manufacturing, micro-electromechanical systems, nano-electromechanical systems, and microscopes, but there are no reports showing its application in the processing of complex curved micro-components. Summary of the invention

[0005] The object of the present invention is to provide a forming method for a small-sized thin-walled pleated filter screen for a hydraulic system, wherein the micro-through holes of the pleated filter screen processed by the method will not have tearing defects.

[0006] The technical solution adopted by the present invention is a method for forming a small-sized thin-walled pleated filter screen for a hydraulic system, which is specifically implemented according to the following steps:

[0007] S1. Processing a surface structure of micro-through holes with a large aspect ratio on the original plate by electron beam cutting to form a surface micro-through hole plate;

[0008] S2, by unfolding the pleated surface of the pleated filter model, fitting the size of each part of the unfolded curved surface, and then punching / spinning the micro-through-hole flat plate obtained in step S1 through a punching / spinning machine to form a curved screen, and at the same time cutting the end of the curved screen;

[0009] S3, punching / rolling the curved screen obtained in step S2 by a punching / rolling machine to form a curved screen with pleats, and simultaneously cutting the ends of the curved screen with pleats.

[0010] The present invention is also characterized in that:

[0011] Step S1 is specifically as follows:

[0012] S11, clamping and fixing the original plate on the electron beam processing platform;

[0013] S12, importing the microporous pattern to be processed into the equipment and setting the electron beam processing parameters;

[0014] S13, starting the electron beam processing platform, and processing a surface structure of micro-through holes with a large aspect ratio according to a set processing trajectory to form a surface micro-through hole flat plate;

[0015] S14, after the processing is completed, the surface micro-through-hole plate is removed.

[0016] Step S2 is specifically as follows:

[0017] S21, determining the size of each part of the curved surface after the pleated filter model is unfolded, and manufacturing a deep drawing deformation die LS01 for stamping / spinning according to the size;

[0018] S22, cutting and blanking: placing the flat plate with micro-through holes obtained in step S1 on a punching / spinning machine processing position, and cutting and blanking the plate using a cutting die according to the size obtained in step S21 to obtain a circular flat plate blank;

[0019] S23, primary deformation: keep the processing position of the circular flat blank unchanged, set the stamping / spinning process parameters, use the drawing deformation die LS01 to stamp / spin the circular flat blank, the stamping / spinning depth is greater than the total height of the pleated filter after unfolding, and obtain the curved screen after stamping / spinning is completed.

[0020] Step S21 is specifically as follows:

[0021] Unfold the pleated surface of the pleated filter model, set the center of the opening side of the filter model as the zero point, which is Hmm away from the center point of the head. Then, starting from the zero point plane, measure the unfolded length of the corresponding filter pleats every hmm. This length is the circumference of the plane circle corresponding to the curved screen required to be processed in step S2. From this, the radius of the plane circle corresponding to the curved screen can be obtained. The group radius data is fitted with the corresponding distance from the top of the ball to obtain a quadratic curve. The curve can be rotated along the y-axis to obtain a schematic diagram of the curved screen. The deep drawing deformation die LS01 is made based on the curve and the schematic diagram.

[0022] Step S3 is specifically as follows:

[0023] S31, secondary deformation: placing the curved screen obtained in step S2 at the processing position of the stamping / rolling machine, setting the stamping / rolling process parameters, using the drawing deformation die LS02 to perform stamping / rolling deformation on the curved screen, controlling the wrinkle formation in the middle and bottom areas of the screen, and obtaining a secondary deformed part after the stamping / rolling is completed;

[0024] S32, initial shaping: keeping the processing position of the secondary deformation part unchanged, using a wrinkle shaping mold to correct the overall shape of the curved surface of the secondary deformation part, including initial wrinkle shaping, to obtain a quasi-finished product with wrinkles;

[0025] S33, secondary shaping and blanking: keep the processing position of the quasi-finished part unchanged, use the wrinkle shaping-cutting composite mold to align the curved surface and wrinkles of the finished part for secondary shaping, and at the same time cut the bottom of the finished part to form a round flat end shell surface to obtain the finished part;

[0026] S34. Sample inspection: inspect the shape and size of the curved surface, wrinkled curved surface, and micro-holes on the curved surface of the finished product.

[0027] During the deformation process of step S23 or step S31, the appearance of the curved surface is deformed, but no structural deformation is generated.

[0028] The beneficial effects of the present invention are:

[0029] The method of the present invention combines electron beam cutting technology with stamping / spinning / rolling processes. First, a micro-through hole array with a large aspect ratio is processed on a plate using electron beam cutting technology, and then the processing of the pleated filter is completed in two steps: first, a stamping / spinning machine is used to process only the curved screen structure in the filter without processing the pleats, and then a stamping / rolling machine is used to complete the processing of the pleats. In the two forming processes, only the curved surface appearance is deformed, and no structural deformation is generated, so that the shape of the circular hole is not deformed. This processing method can avoid the occurrence of tearing defects at the micro-through holes of the filter, and further ensure the quality of the processed filter.

[0030] The forming method of the present invention is efficient and convenient, has high processing accuracy, and has a variety of forming methods that can be combined. It is particularly suitable for the processing of small-sized and highly complex parts. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 A schematic diagram of the structure of a pleated filter screen processed according to an embodiment of the present invention;

[0032] Figure 2 A schematic diagram of the structure of a micropore array in a pleated filter screen processed according to an embodiment of the present invention;

[0033] Figure 3 Schematic diagram of the unfolding of the pleated filter screen in the embodiment of the present invention;

[0034] Figure 4 Schematic diagram of the structure of the drawing deformation die LS01 used in Example 1 of the present invention;

[0035] Figure 5 Schematic diagram of the structure of the drawing deformation die LS02 used in Example 1 of the present invention;

[0036] Figure 6 Schematic diagram of the structure of the spinning deformation die used in Example 2 of the present invention;

[0037] Figure 7 Schematic diagram of the structure of the forming deformation die used in Example 2 of the present invention.

[0038] Among them, 1. screen body, 2. pleats, 3. micropores. DETAILED DESCRIPTION

[0039] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0040] The forming method of the small-sized thin-walled pleated filter for hydraulic system of the present invention firstly processes a micro-through hole array on the original plate by electron beam cutting technology; then uses a stamping / spinning machine to stamp / spin the plate with the micro-through hole array to form a curved screen structure; then uses a stamping / rolling machine to stamp / roll the end of the curved screen to form pleats; finally, cuts the end of the curved screen to form a pleated filter. The method is specifically implemented according to the following steps:

[0041] S1: Taking stainless steel plate as an example, the original plate is processed with large depth-to-diameter ratio micropores on the stainless steel plate by electron beam cutting method, so as to obtain a micropore array on the surface of the stainless steel plate. Specifically:

[0042] S11: clamping and fixing the stainless steel plate on the electron beam processing platform;

[0043] S12: importing the microporous pattern to be processed into the equipment and setting the electron beam processing parameters;

[0044] S13: starting the electron beam processing platform, and processing a surface structure of micro-through holes with a large aspect ratio according to a set processing trajectory to form a surface micro-through hole flat plate;

[0045] S14: After the processing is completed, the surface micro-through-hole plate is removed.

[0046] S2: The dimensions of each part of the curved surface of the pleated filter after unfolding are fitted by unfolding the pleated surface, and then the micro-through-hole flat plate obtained in step S1 is punched / spun to shape by a punching / spinning machine to form a curved screen, i.e., a primary deformation part, and the ends of the screen are cut at the same time. Specifically:

[0047] S21: Determine the unfolded size of the pleated filter and make the deep drawing and deformation die LS01 for stamping / spinning:

[0048] Unfold the pleated surface of the pleated filter model, set the center of the opening side of the filter model as the zero point, which is Hmm away from the center point of the head. Then, starting from the zero point plane, measure the unfolded length of the corresponding filter pleats every hmm. This length is the circumference of the plane circle corresponding to the primary deformation part processed in step S2. From this, the radius of the plane circle corresponding to the primary deformation part can be obtained. The group radius data is fitted with the corresponding distance from the ball top to obtain a quadratic curve. The curve is rotated along the y-axis to obtain a schematic diagram of the primary deformation part. The deep drawing deformation die LS01 is manufactured based on the curve and the schematic diagram.

[0049] S22: Cutting and blanking: placing the flat plate with micro-through holes obtained in step S1 on a punching / spinning machine processing position, and cutting and blanking the plate using a cutting die according to the size obtained in step S21 to obtain a circular flat plate blank;

[0050] S23: primary deformation: after cutting and blanking, the processing position of the circular flat blank is kept unchanged, the stamping / spinning process parameters are set, and the circular flat blank is stamped / spinned by the drawing deformation die LS01. The stamping / spinning depth is greater than Hmm to ensure that the subsequent forming is comprehensive. In addition, during the screen forming process, the curved surface appearance is deformed but the structural deformation is not generated. After the stamping / spinning is completed, a primary deformed part, i.e., a curved screen, is obtained.

[0051] S3: Use a stamping / rolling machine to perform micro-stamping / rolling on the curved screen obtained in step S2 to form a curved screen with folds, and cut the ends of the screen at the same time.

[0052] S31: secondary deformation: placing the curved screen obtained in step S2 at the processing position of the stamping / rolling machine, setting the stamping / rolling process parameters, and using the drawing deformation die LS02 to perform stamping / rolling deformation on the curved screen, and controlling the wrinkle formation in the middle and bottom areas of the screen. During the wrinkle formation process in the middle and bottom areas of the screen, the curved surface appearance is deformed, but no structural deformation is generated. After the stamping / rolling is completed, a secondary deformed part is obtained;

[0053] S32: Initial shaping: After the two-stage deformation, the processing position of the secondary deformation part is kept unchanged, and the secondary deformation part is shaped by a fold shaping mold, and the overall shape of the screen surface is corrected, including the initial shaping of the folds, to obtain a quasi-finished product with folds;

[0054] S33: Secondary shaping and blanking: After the initial shaping, the processing position of the quasi-finished part is kept fixed, and the fold shaping-cutting composite mold is used to perform secondary shaping on the quasi-finished part, and the screen surface and folds are finally shaped. At the same time, the bottom of the finished part is cut to form a round flat end shell surface to obtain the finished part;

[0055] S34: Sample inspection: Check the shape and size of the curved surface, wrinkled curved surface, and micropores on the curved surface of the finished product to see if they meet the size and accuracy requirements of the curved screen with wrinkles on the surface.

[0056] Embodiment 1:

[0057] The flat plate used in this embodiment was processed as follows before being installed on the electron beam processing platform:

[0058] 1) Place the plate into an ultrasonic cleaner and clean for 1 to 3 minutes;

[0059] 2) Take out the board, wipe off the moisture on the surface, put it into the dryer, and dry it at 150-250℃ for 2-4 minutes;

[0060] 3) After drying, take out the board and use a laminating machine to laminator the surface. Laminating is to prevent scratches on the board surface, and the protective film will be removed when it is used.

[0061] Figure 1 and Figure 2 It is a schematic structural diagram of the pleated filter screen processed in this embodiment, wherein a circle of pleats 2 is provided on the circular curved screen body 1, and micropores 3 are opened on the screen body 1, including on the pleats 2.

[0062] The specific processing steps of the filter screen in this embodiment are:

[0063] S1: Through the electron beam cutting method, the processing of large aspect ratio micro-holes is realized on the processed flat plate, so as to obtain a micro-hole array on the surface of the plate. Specifically:

[0064] S11: clamping and fixing the flat plate on the electron beam processing platform;

[0065] S12: importing the microporous pattern to be processed into the equipment and setting the electron beam processing parameters;

[0066] S13: starting the electron beam processing platform, and processing a surface structure of micro-through holes with a large aspect ratio according to a set processing trajectory to form a surface micro-through hole flat plate;

[0067] S14: After the processing is completed, the surface micro-through-hole plate is removed.

[0068] S2: The dimensions of each part of the curved surface after the pleated filter is unfolded are fitted by unfolding the pleated surface, and then the micro-perforated flat plate obtained in step S1 is punched and shaped by a punching machine to form a curved screen, i.e., a one-time punching deformation part, and the end of the screen is cut at the same time. Specifically:

[0069] S21: Determine the unfolded size of the pleated filter and make the deep drawing deformation die LS01 for stamping:

[0070] like Figure 3 As shown, unfold the pleated surface of the pleated filter model, set the center of the opening side of the filter model as the zero point, which is Hmm away from the center point of the head, and then start from the zero point plane, measure the unfolded length of the corresponding filter pleats every hmm, which is the circumference of the plane circle corresponding to the primary stamping deformation part to be processed in step S2, from which the radius of the plane circle corresponding to the primary stamping deformation part can be obtained, and the measured The group radius data is fitted with the corresponding distance from the ball top to obtain a quadratic curve. The curve is rotated along the y-axis to obtain a schematic diagram of a stamping deformation part. The deep drawing deformation die LS01 is manufactured based on the curve and the schematic diagram.

[0071] S22: Cutting and blanking: placing the plate obtained in step S1 on a punching machine processing position, and cutting and blanking the plate using a cutting die according to the size obtained in step S21 to obtain a circular flat blank;

[0072] S23: One-time stamping deformation: After cutting and blanking, keep the processing position of the circular flat blank unchanged, use the deep drawing deformation die LS01 to stamp and deform the circular flat blank once, and the stamping depth is greater than Hmm to ensure the subsequent forming is comprehensive. Control the screen forming, and during the screen forming process, the curved surface appearance is deformed, but the structural deformation is not generated, and a one-time stamping deformation part, that is, the curved screen, is obtained. Figure 4 As shown, the structure of the drawing deformation die LS01 used in this step;

[0073] S3: Perform secondary micro-stamping and shaping of the curved screen obtained in step S2 by a stamping machine to produce a curved screen with folds, and at the same time perform end cutting of the screen. Specifically:

[0074] S31: Secondary stamping deformation: Place the curved screen obtained in step S2 at the processing position of the stamping machine, and use the deep drawing deformation die LS02 to perform secondary stamping deformation on the curved screen, and control the wrinkle formation in the middle and bottom areas of the screen. During the wrinkle formation process in the middle and bottom areas of the screen, the curved surface appearance is deformed, but no structural deformation is generated, and a secondary stamping deformed part is obtained. Figure 5 As shown, the structure of the drawing deformation die LS02 used in this step;

[0075] S32: Initial shaping: After the two-stage stamping deformation, the processing position of the secondary stamping deformed part is kept unchanged, and the secondary stamping deformed part is shaped by a wrinkle shaping die, and the overall shape of the screen surface is corrected, including the initial shaping of the wrinkles, to obtain a semi-finished stamping part with wrinkles;

[0076] S33: Secondary shaping and blanking: After the initial shaping, the processing position of the semi-finished stamping part is kept fixed, and the fold shaping-cutting composite die is used to perform secondary shaping on the finished stamping part, and the screen surface and folds are finally shaped. At the same time, the bottom of the finished stamping part is cut to form a round flat end shell surface to obtain the finished stamping part;

[0077] S34: Stamping sample inspection: Check the shape and size of the curved surface, wrinkled curved surface, and micropores on the curved surface of the finished stamping parts to see if they meet the size and accuracy requirements of the curved screen with wrinkles on the surface.

[0078] Embodiment 2:

[0079] This embodiment is basically the same as the embodiment 1, except that the curved screen is formed by spinning in step S2, and the curved screen with pleats is formed by rolling in step S3. In the actual manufacturing process, different forming methods can be selected and combined for manufacturing according to existing conditions or needs. Steps S23 and S31 of this embodiment are specifically as follows:

[0080] S23: Spinning deformation: After cutting and blanking, keep the processing position of the circular flat blank unchanged, and use a spinning deformation die to spin the circular flat blank. The spinning depth is greater than Hmm to ensure comprehensive subsequent forming. During spinning, the mold is fed up and down as a whole, and the spinning balls connected to springs on both sides of the mold are fed along the generatrix direction. An iron rod is connected to the inside of the spring to ensure that the spring is not bent during the feeding process. Control the forming of the screen. During the forming process of the screen, the curved surface appearance is deformed, but the structure is not deformed, so that a spinning deformation part, i.e. a curved screen, is obtained. Figure 6 As shown, the structure of the spinning deformation die used in this step;

[0081] S31: Rolling deformation: Place the spun deformed part obtained in step S2 in the processing position of the rolling machine, replace the rolling mold, and use the forming deformation mold to roll the spun deformed part. During rolling, the curved screen is rolled and shaped by the roller molds on both sides of the curved screen and the forming mold on the inside. The angles of the rollers on both sides of the curved screen can be changed over time to improve the forming efficiency. Control the wrinkle forming in the middle and bottom areas of the screen. During the wrinkle forming process in the middle and bottom areas of the screen, the curved surface appearance is deformed but the structure is not deformed, so a rolled deformed part is obtained. Figure 7 As shown, the structure of the forming deformation die used in this step;

[0082] The remaining steps are the same as in Example 1.

[0083] Embodiment 3:

[0084] The forming method of the small-sized thin-walled pleated filter screen for hydraulic system is specifically implemented according to the following steps:

[0085] S1. Processing a surface structure of micro-through holes with a large aspect ratio on the original plate by electron beam cutting to form a surface micro-through hole plate;

[0086] S2, by unfolding the pleated surface of the pleated filter model, fitting the size of each part of the unfolded curved surface, and then punching / spinning the micro-through-hole flat plate obtained in step S1 through a punching / spinning machine to form a curved screen, and at the same time cutting the end of the curved screen;

[0087] S3, punching / rolling the curved screen obtained in step S2 by a punching / rolling machine to form a curved screen with pleats, and simultaneously cutting the ends of the curved screen with pleats.

Claims

1. Forming method of small-size thin-wall pleated filter screen for hydraulic system, It is characterized in that Follow the steps below to implement it: S1. Processing a surface structure of micro-through holes with a large depth-to-diameter ratio on the original plate by electron beam cutting to form a surface micro-through-hole plate; S2, by unfolding the pleated surface of the pleated filter model, fitting the size of each part of the unfolded curved surface, and then punching / spinning the micro-through-hole flat plate obtained in step S1 through a punching / spinning machine to form a curved screen, and at the same time cutting the end of the curved screen; S3, punching / rolling the curved screen obtained in step S2 by a punching / rolling machine to form a curved screen with pleats, and simultaneously cutting the ends of the curved screen with pleats.

2. The forming method of the small-sized thin-wall pleated filter screen for hydraulic system according to claim 1, It is characterized in that Step S1 is specifically as follows: S11, clamping and fixing the original plate on the electron beam processing platform; S12, importing the microporous pattern to be processed into the equipment and setting the electron beam processing parameters; S13, starting the electron beam processing platform, and processing a surface structure of micro-through holes with a large aspect ratio according to a set processing trajectory to form a surface micro-through hole flat plate; S14, after the processing is completed, the surface micro-through-hole plate is removed.

3. The forming method of the small-sized thin-wall pleated filter screen for hydraulic system according to claim 1, It is characterized in that Step S2 is specifically as follows: S21, determining the size of each part of the curved surface after the pleated filter model is unfolded, and manufacturing a deep drawing deformation die LS01 for stamping / spinning according to the size; S22, cutting and blanking: placing the flat plate with micro-through holes obtained in step S1 on a punching / spinning machine processing position, and cutting and blanking the plate using a cutting die according to the size obtained in step S21 to obtain a circular flat plate blank; S23, primary deformation: keep the processing position of the circular flat blank unchanged, set the stamping / spinning process parameters, use the drawing deformation die LS01 to stamp / spin the circular flat blank, the stamping / spinning depth is greater than the total height of the pleated filter after unfolding, and obtain the curved screen after stamping / spinning is completed.

4. The method for forming a small-sized thin-wall pleated filter screen for a hydraulic system according to claim 3, It is characterized in that Step S21 is specifically as follows: Unfold the pleated surface of the pleated filter model, set the center of the opening side of the filter model as the zero point, which is Hmm away from the center point of the head. Then, starting from the zero point plane, measure the unfolded length of the corresponding filter pleats every hmm. This length is the circumference of the plane circle corresponding to the curved screen required to be processed in step S2. From this, the radius of the plane circle corresponding to the curved screen can be obtained. The group radius data is fitted with the corresponding distance from the top of the ball to obtain a quadratic curve. The curve can be rotated along the y-axis to obtain a schematic diagram of the curved screen. The deep drawing deformation die LS01 is made based on the curve and the schematic diagram.

5. The method for forming a small-sized thin-wall pleated filter screen for a hydraulic system according to claim 1, It is characterized in that Step S3 is specifically as follows: S31, secondary deformation: placing the curved screen obtained in step S2 at the processing position of the stamping / rolling machine, setting the stamping / rolling process parameters, using the drawing deformation die LS02 to perform stamping / rolling deformation on the curved screen, controlling the wrinkle formation in the middle and bottom areas of the screen, and obtaining a secondary deformed part after the stamping / rolling is completed; S32, initial shaping: keeping the processing position of the secondary deformation part unchanged, using a wrinkle shaping mold to correct the overall shape of the curved surface of the secondary deformation part, including initial wrinkle shaping, to obtain a quasi-finished product with wrinkles; S33, secondary shaping and blanking: keep the processing position of the quasi-finished part unchanged, use the wrinkle shaping-cutting composite mold to align the curved surface and wrinkles of the finished part for secondary shaping, and at the same time cut the bottom of the finished part to form a round flat end shell surface to obtain the finished part; S34. Sample inspection: inspect the shape and size of the curved surface, wrinkled curved surface, and micro-holes on the curved surface of the finished product.

6. A method for forming a small-sized thin-walled pleated filter screen for a hydraulic system according to claim 3 or 5, It is characterized in that During the deformation process of step S23 or step S31, the appearance of the curved surface is deformed, but no structural deformation is generated.

Citation Information

Patent Citations

  • Additive manufacturing equipment combining electron beam selective melting and electron beam cutting

    CN106825567A

  • Die-free multipoint spinning three-dimensional curved surface forming method

    CN109175051A

  • Tool and method for forming high-precision miniature throttle valve filter screen

    CN113441623A

  • Combined machining method for complex curved surface safety filter screen of aircraft hydraulic system

    CN113843586A

  • Press forming method

    JP2007326112A