Preparation method of anion exchange membrane water electrolyser anode catalyst
By preparing nickel iron phosphide (NiFeP) catalyst, the problems of high energy consumption and overpotential of the anode of anion exchange membrane water electrolyzer are solved, and a low-cost and efficient water electrolysis reaction is achieved, which has the potential for commercial application.
Patent Information
- Application Number
- CN202410895750.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-05
AI Technical Summary
The anode of anion exchange membrane water electrolyzer has high energy consumption and over-potential problems during the water electrolysis process, resulting in excessively high cell pressure in the electrolyzer, which limits the commercial application of water electrolysis hydrogen production technology. Traditional precious metal catalysts are costly and have limited natural resources. .
Using nickel iron phosphide (NiFeP) as a catalyst, by dissolving Ni salt and Fe salt in oleylamine, adding a phosphorus source and a reducing agent, and preparing a nanoscale NiFeP catalyst through a temperature-raising procedure, it is used for the anode of anion exchange membrane water electrolyzer. Reduce reaction energy consumption and improve electrolysis efficiency.
The NiFeP catalyst exhibits low cell pressure, excellent electrochemical stability and high energy efficiency in AEMWE. The cost is lower than RuO2 and IrO2. It has significant commercial value and application prospects. It can effectively generate oxygen and generate oxygen during the electrolysis of water to produce hydrogen. Maintain high activity for a long time.
Smart Images

Figure CN118851112A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of new energy materials, and in particular relates to a method for preparing an anode catalyst of an anion exchange membrane water electrolyzer. Background Art
[0002] Anion exchange membrane water electrolyzer (AEMWE) is a new type of water electrolysis technology that uses anion exchange membrane (AEM) to separate the anode and cathode in the electrolyzer. The high ion selectivity of AEM can effectively transfer OH in the solution. - , to prevent gas crossover and electrolyte crossover, thereby improving electrolysis efficiency and hydrogen purity. The overpotential of the anode oxygen evolution reaction (OER) is high, much higher than the overpotential of the cathode hydrogen evolution reaction (HER), which means that during water electrolysis, most of the energy loss occurs in the anode OER, causing the electrolyzer pressure to be too high. Therefore, it is necessary to develop new anode catalysts to reduce reaction energy consumption and accelerate the rate of hydrogen production by electrolysis of water.
[0003] As a green and efficient energy carrier, hydrogen production by water electrolysis is widely regarded as one of the most promising green hydrogen production methods due to its environmentally friendly, pure product and carbon-free production process. In the process of water electrolysis, OER is a key half-reaction responsible for the decomposition of water or hydroxide into oxygen. However, the high energy consumption of the OER reaction, especially its large overpotential, has become the main obstacle to the large-scale application of this technology. Therefore, researchers are committed to finding solutions to achieve the commercial deployment of water electrolysis hydrogen production technology. Although traditional precious metal catalytic materials have excellent performance, the main problem they face is limited natural resources and high cost. Therefore, it is particularly important to develop non-precious metal catalysts that have both high catalytic performance and economic benefits. Commercial RuO2 and IrO2 are often used as standards for evaluating OER performance, but they are extremely cost-effective compared to NiFe-based catalysts. Therefore, the development of advanced NiFe-based catalysts to replace traditional precious metal catalysts not only has broad application prospects, but also has significant commercial value. Summary of the invention
[0004] The purpose of the present invention is to overcome the defects of the prior art and provide a method for preparing an anode catalyst of an anion exchange membrane water electrolyzer.
[0005] Nickel iron phosphide (NiFeP) is a transition metal phosphide, in which Ni and Fe belong to the 3d family of materials. Their d orbital holes may be related to catalytic activity, providing active sites during the reaction process and facilitating the OER. The present invention prepares a nanoscale NiFeP catalyst. In the AEMWE test, at 60°C, 1Acm -2Under the conditions of , it shows an extremely low cell voltage (1.71V), which is better than commercial IrO2. Secondly, NiFeP has excellent stability and excellent energy efficiency, and shows excellent performance in AEMWE test. Therefore, NiFeP prepared by the present invention may play an important role in future hydrogen energy conversion technology due to its high activity and low cost advantages.
[0006] In order to achieve the above object, one of the technical solutions of the present invention is: a method for preparing an anion exchange membrane water electrolyzer anode catalyst, comprising the following steps:
[0007] (1) preparing a precursor solution: dissolving Ni salt and Fe salt in oleylamine, and stirring to mix uniformly to obtain a precursor solution;
[0008] (2) adding a phosphorus source and a reducing agent: adding a phosphorus source and a reducing agent to the precursor solution prepared in step (1), stirring and mixing to obtain a mixed solution;
[0009] (3) Preparation of NiFeP: The mixed solution obtained in step (2) is passed through a protective gas for washing to remove impurities; the temperature is adjusted and a heating program is set, and the program is run. When the heating process is completed, the preparation of the NiFeP catalyst is completed.
[0010] In a preferred embodiment of the present invention, in step (1), the Ni salt is nickel acetylacetonate, the Fe salt is ferric acetylacetonate, the concentration of the Ni salt in the precursor solution is 0.01-0.04 mol / L, and the concentration of the Fe salt in the precursor solution is 0.01-0.05 mol / L.
[0011] In a preferred embodiment of the present invention, the concentration of the oleylamine solution in step (1) is 70-85 vol%.
[0012] In a preferred embodiment of the present invention, the phosphorus source and reducing agent in step (2) are n-octyl phosphine, which is both a reducing agent and a phosphating agent. Adding the "P" source and reducing agent means adding 180-250uL of n-octyl phosphine with a purity of 99% to the above 10mL mixed solution, where n-octyl phosphine is both a reducing agent and a phosphating agent, and finally stirring for 30min to fully mix the solution.
[0013] In a preferred embodiment of the present invention, the volume ratio of the phosphorus source and the reducing agent to the precursor solution in step (2) is 180-250:800-1200.
[0014] In a preferred embodiment of the present invention, the protective atmosphere in step (3) is a high-purity inert gas N2 or Ar.
[0015] In a preferred embodiment of the present invention, the heating program in step (3) is a three-stage programmed temperature heating and temperature control program. In the first stage, the temperature is increased from 20°C to 50°C at a heating rate of 8-10°C / min, and the temperature is kept for 20-40 minutes. In the second stage, the temperature is increased from 50°C to 100°C at a heating rate of 18-22°C / min, and the temperature is kept for 20-40 minutes. In the third stage, the temperature is increased from 100°C to 270°C at a heating rate of 14-16°C / min, and the temperature is kept for 50-70 minutes. After the insulation is completed, the temperature is naturally cooled to room temperature.
[0016] In order to achieve the above objectives, the second technical solution of the present invention is: an anode catalyst for an anion exchange membrane water electrolyzer prepared by the above preparation method.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The NiFeP catalyst prepared by the present invention can effectively promote the generation of oxygen in the water decomposition reaction in AEMWE, and has high activity and energy efficiency;
[0019] 2. The NiFeP catalyst prepared by the present invention exhibits excellent electrochemical stability in AEMWE, can withstand corrosion and oxidation during long-term electrolysis, and maintains high activity during long-term operation, thereby improving the overall economic benefits;
[0020] 3. The NiFeP catalyst prepared by the present invention has a very low cost compared with RuO2 or IrO2 and Pt / C, and shows great benefit potential in the large current AEMWE hydrogen production technology. The development of NiFeP catalyst to replace traditional precious metal oxides has great application prospects and commercial value;
[0021] 4. The synthesis process of the NiFeP catalyst of the present invention generally adopts an environmentally friendly chemical method, and the catalytic process does not produce harmful substances, which is in line with the principles of sustainable development and green chemistry. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 TEM images of NiFeP prepared in Example 1 at different resolutions and a particle size distribution diagram of NiFeP;
[0023] Figure 2 Dark field TEM of NiFeP prepared in Example 1, and EDX element mapping of each element;
[0024] Figure 3 EDX element contents of Ni, Fe and P in NiFeP prepared in Example 1;
[0025] Figure 4a and 4b are the lattice spacings of NiFeP prepared in Example 1, Figure 4 cd are the XPS spectra of Ni 2p and Fe 2p, respectively;
[0026] Figure 5 a is the LSV of NiFeP tested in RDE, the solution is 1.0M KOH, the scan rate is 5mV / s, Figure 5 b is a schematic diagram of NiFeP used in AEMWE device, Figure 5 c is the AEMWE test data cable, Figure 5 d is the stability of NiFeP tested in the AEMWE device with a current density of 1Acm -2 , Figure 5 e is NiFeP in AEMWE device with 1Acm -2 The voltage efficiency and potential decay rate of the test. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is described in more detail below with reference to the accompanying drawings and specific embodiments, but the protection scope of the present invention is not limited to these embodiments.
[0028] A method for preparing an anion exchange membrane water electrolyzer anode catalyst comprises the following steps:
[0029] (1) preparing a precursor solution: dissolving Ni salt and Fe salt in oleylamine, and stirring to mix uniformly to obtain a precursor solution;
[0030] (2) adding a phosphorus source and a reducing agent: adding a phosphorus source and a reducing agent to the precursor solution prepared in step (1), stirring and mixing to obtain a mixed solution;
[0031] (3) Preparation of NiFeP: The mixed solution obtained in step (2) is passed through a protective gas for washing to remove impurities; the temperature is adjusted and a heating program is set, and the program is run. When the heating process is completed, the preparation of the NiFeP catalyst is completed.
[0032] In the step (1), the Ni salt is nickel acetylacetonate, the Fe salt is iron acetylacetonate, the concentration of the Ni salt in the precursor solution is 0.01-0.04 mol / L, and the concentration of the Fe salt in the precursor solution is 0.01-0.05 mol / L.
[0033] The concentration of the oleylamine solution in step (1) is 70-85 vol%.
[0034] In the step (2), the phosphorus source and reducing agent are n-octylphosphine, which is both a reducing agent and a phosphating agent.
[0035] In the step (2), the volume ratio of the phosphorus source and the reducing agent to the precursor solution is 180-250:800-1200.
[0036] The protective atmosphere in step (3) is high-purity inert gas N2 or Ar.
[0037] The temperature rise program in step (3) is a three-stage programmed temperature rise control program. In the first stage, the temperature is raised from 20°C to 50°C at a heating rate of 8-10°C / min and kept warm for 20-40min. In the second stage, the temperature is raised from 50°C to 100°C at a heating rate of 18-22°C / min and kept warm for 20-40min. In the third stage, the temperature is raised from 100°C to 270°C at a heating rate of 14-16°C / min and kept warm for 50-70min. After the insulation is completed, the temperature is naturally cooled to room temperature.
[0038] An anode catalyst for an anion exchange membrane water electrolyzer prepared by the above preparation method.
[0039] The anode catalyst of the anion exchange membrane water electrolyzer needs to be carbon-loaded before testing. First, it is cleaned with a mixed solution of ethanol and n-hexane in a volume ratio of 5:1 as a cleaning agent to remove residues; the anode catalyst NiFeP catalyst is dispersed in n-hexane, a corresponding amount of carbon carrier is added, and then anhydrous ethanol is added for ultrasonic dispersion, and finally centrifugal separation is performed at a centrifugal speed of 10000-12000r / min to obtain NiFeP with a mass fraction of 20%-50% carbon.
[0040] Example 1
[0041] (1) Take 0.473mmol of nickel acetylacetonate and 0.159mmol of ferric acetylacetonate and mix with 15mL of 70vol% oleylamine and stir for 30min to make the above solution fully mixed. Then take 1mL of the above solution and dilute it to 10mL with 70% oleylamine. Transfer the solution to a three-necked flask and stir it well. Add 200uL of n-octylphosphine and sonicate for 30min to complete the preparation stage.
[0042] (2) The flask was transferred to a programmed temperature device, N2 gas was introduced for 20 min, and then the temperature was programmed. The first stage was to heat from 20°C to 50°C at a rate of 10°C / min and keep warm for 30 min. The second stage was to heat from 50°C to 100°C at a rate of 20°C / min and keep warm for 30 min. The third stage was to heat from 100°C to 270°C at a rate of 15°C / min and keep warm for 60 min. After the 270°C insulation program was completed, it was naturally cooled to room temperature in the heating mantle. The brown-black sample obtained was NiFeP. The sample was then cleaned and ultrasonicated with a mixed solution of ethanol and n-hexane in a volume ratio of 5:1, and finally centrifuged at a speed of 10000r / min to complete the cleaning of NiFeP.
[0043] (3) 1.45 mg NiFeP was dispersed in 10 mL n-hexane, and 5.77 mg XC-72 was added, and ultrasonicated for 20 min. Then 30 mL anhydrous ethanol was added and ultrasonicated for 10 min. The mixture was centrifuged to obtain carbon-loaded NiFeP.
[0044] Example 2
[0045] (1) Take 0.315mmol of nickel acetylacetonate and 0.318mmol of ferric acetylacetonate and mix with 15mL of 70% oleylamine and stir for 30min to make the above solution fully mixed. Then take 1mL of the above solution and dilute it to 10mL with 70% oleylamine. Transfer the solution to a three-necked flask and stir it well. Add 200uL of n-octylphosphine and sonicate for 30min to complete the preparation stage.
[0046] (2) The flask was transferred to a programmed temperature device, N2 gas was introduced for 20 min, and then the temperature was programmed. The first stage was to heat from 20°C to 50°C at a rate of 10°C / min and keep warm for 30 min. The second stage was to heat from 50°C to 100°C at a rate of 20°C / min and keep warm for 30 min. The third stage was to heat from 100°C to 270°C at a rate of 15°C / min and keep warm for 60 min. After the 270°C insulation program was completed, it was naturally cooled to room temperature in the heating mantle. The brown-black sample obtained was NiFeP. The sample was then cleaned and ultrasonicated with a mixed solution of ethanol and n-hexane in a volume ratio of 5:1, and finally centrifuged at a speed of 10000r / min to complete the cleaning of NiFeP.
[0047] (3) 1.45 mg NiFeP was dispersed in 10 mL n-hexane, and 5.77 mg XC-72 was added, and ultrasonicated for 20 min. Then 30 mL anhydrous ethanol was added and ultrasonicated for 10 min. The mixture was centrifuged to obtain carbon-loaded NiFeP.
[0048] Example 3
[0049] (1) Take 0.157mmol of nickel acetylacetonate and 0.477mmol of iron acetylacetonate and mix with 15mL of 70% oleylamine and stir for 30min to make the above solution fully mixed. Then take 1mL of the above solution and dilute it to 10mL with 70% oleylamine. Transfer the solution to a three-necked flask and stir it well. Add 200uL of n-octylphosphine and sonicate for 30min to complete the preparation stage.
[0050] (2) The flask was transferred to a programmed temperature device, N2 gas was introduced for 20 min, and then the temperature was programmed. The first stage was to heat from 20°C to 50°C at a rate of 10°C / min and keep warm for 30 min. The second stage was to heat from 50°C to 100°C at a rate of 20°C / min and keep warm for 30 min. The third stage was to heat from 100°C to 270°C at a rate of 15°C / min and keep warm for 60 min. After the 270°C insulation program was completed, it was naturally cooled to room temperature in the heating mantle. The brown-black sample obtained was NiFeP. The sample was then cleaned and ultrasonicated with a mixed solution of ethanol and n-hexane in a volume ratio of 5:1, and finally centrifuged at a speed of 10000r / min to complete the cleaning of NiFeP.
[0051] (3) 1.45 mg NiFeP was dispersed in 10 mL n-hexane, and 5.77 mg XC-72 was added, and ultrasonicated for 20 min. Then 30 mL anhydrous ethanol was added and ultrasonicated for 10 min. The mixture was centrifuged to obtain carbon-loaded NiFeP.
[0052] Figure 1 This is the TEM of NiFeP in implementation case 1. It can be seen from the figure that NiFeP is nano-spherical with uniform particle size. After statistics, it is known that the average particle size is about 6.5nm. The uniformly dispersed nanoparticles and nano-scale particle size ensure ultra-high specific surface area and active sites.
[0053] Figure 2 This is the dark field TEM of NiFeP in implementation case 1. The box is the high-energy X-ray irradiation scanning area. From the mapping results on the right, we can see that the outlines of the elements Ni, Fe, and P are obvious, which preliminarily confirms the successful preparation of the NiFeP catalyst.
[0054] Figure 3 The EDX content analysis of NiFeP in Case 1 was carried out, and the results showed that Ni:Fe:P=2.4:1:1.1, which was basically consistent with our feed ratio, indicating the full reduction of Ni and Fe, further confirming the successful preparation of the catalyst.
[0055] Figure 4 a and 4b are the lattice spacings of the catalyst in Example 1, which were determined to be 0.215nm and 0.227nm by measurement, respectively, which are the (231) crystal plane in Ni3P and the (111) crystal plane in Fe2P. Subsequently, combined with XPS testing, the peaks of Ni-P and Fe-P can be clearly seen from the figure, confirming the successful preparation of NiFeP.
[0056] Figure 5 To implement the performance test of NiFeP in Case 1. First Figure 5a is the RDE test. It can be seen from the figure that compared with commercial IrO2, NiFeP has a lower potential at 10mAcm -2 The OER activity of NiFeP is much better than that of commercial iridium oxide. AEMWE test was further conducted. It can be seen in Figure c that at 60 ° C, 1M KOH solution, 1Acm -2 The corresponding potential is only 1.71V, which is much smaller than the cell voltage of IrO2 (1.97V), indicating that the activity of NiFeP in AEMWE is better than that of IrO2. Subsequently, a large current stability test was conducted. It can be seen from Figure d that at 1Acm -2 After 22 hours of testing, the potential of NiFeP was always lower than that of IrO2, and the decay after 22 hours was about 8%. After 17 hours, the decay of IrO2 was 11.5%, which shows that the stability of NiFeP is better than that of IrO2. Finally, the voltage efficiency of NiFeP and IrO2 was calculated, NiFeP was 81.3%, and IrO2 was 67.3%, indicating that NiFeP has a higher hydrogen production efficiency in AEMWE. The voltage decay rate was further calculated, and NiFeP was only 0.0018mV s -1 The decay rate is much lower than that of IrO2. The experimental results show that NiFeP exhibits excellent activity and stability, and has great potential in the future development of green hydrogen.
[0057] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some or all of the technical features thereof may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing an anion exchange membrane water electrolyzer anode catalyst, characterized in that: The steps include: (1) preparing a precursor solution: dissolving Ni salt and Fe salt in an oleylamine solution, and stirring and mixing to obtain a precursor solution; (2) adding a phosphorus source and a reducing agent: adding a phosphorus source and a reducing agent to the precursor solution prepared in step (1), stirring and mixing to obtain a mixed solution; (3) Preparation of NiFeP: The mixed solution obtained in step (2) is passed through a protective gas for washing to remove impurities; the temperature is adjusted and a heating program is set, and the program is run. When the heating process is completed, the preparation of the NiFeP catalyst is completed.
2. The method for preparing an anion exchange membrane water electrolyzer anode catalyst according to claim 1, characterized in that: In the step (1), the Ni salt is nickel acetylacetonate, and the Fe salt is iron acetylacetonate.
3. The method for preparing an anion exchange membrane water electrolyzer anode catalyst according to claim 1, characterized in that: The concentration of Ni salt in the precursor solution in step (1) is 0.01-0.04 mol / L.
4. The method for preparing an anion exchange membrane water electrolyzer anode catalyst according to claim 1, characterized in that: The concentration of the Fe salt in the precursor solution in step (1) is 0.01-0.05 mol / L.
5. The method for preparing an anion exchange membrane water electrolyzer anode catalyst according to claim 1, characterized in that: The concentration of the oleylamine solution in step (1) is 70-85 vol%.
6. The method for preparing an anion exchange membrane water electrolyzer anode catalyst according to claim 1, characterized in that: In the step (2), the phosphorus source and the reducing agent are n-octylphosphine.
7. The method for preparing an anion exchange membrane water electrolyzer anode catalyst according to claim 1, characterized in that: In the step (2), the volume ratio of the phosphorus source and the reducing agent to the precursor solution is 180-250:800-1200.
8. The method for preparing an anion exchange membrane water electrolyzer anode catalyst according to claim 1, characterized in that: The protective atmosphere in step (3) is high-purity inert gas N2 or Ar.
9. The method for preparing an anion exchange membrane water electrolyzer anode catalyst according to claim 1, characterized in that: The temperature rise program in step (3) is a three-stage programmed temperature rise control program. In the first stage, the temperature is raised from 20°C to 50°C at a heating rate of 8-10°C / min and kept warm for 20-40min. In the second stage, the temperature is raised from 50°C to 100°C at a heating rate of 18-22°C / min and kept warm for 20-40min. In the third stage, the temperature is raised from 100°C to 270°C at a heating rate of 14-16°C / min and kept warm for 50-70min. After the insulation is completed, the temperature is naturally cooled to room temperature.
10. The anode catalyst obtained by the method for preparing an anode catalyst for an anion exchange membrane water electrolyzer according to any one of claims 1 to 9.
Citation Information
Patent Citations
Nickel-cobalt-phosphorus crystal, and preparation method and application thereof
CN105152149A
NiFeP bifunctional transition metal phosphide catalyst as well as preparation and use thereof
CN107376958A
Porous Amorphous Metallic Electrocatalytic Materials for Water Electrolysis
US20200291536A1
Fast Ambient-Temperature Synthesis of OER Catalysts for Water Electrolysis
US20230220570A1