High-dispersion cerium dioxide-loaded hydrogen-substituted graphdiyne composite material for NH3 detection sensor and preparation method thereof

By replacing the graphite monoacetylene composite material with highly dispersed ceria loaded with hydrogen, the problem of low sensor performance in ammonia and hydrogen gas detection is solved, and high sensitivity and fast response NH3 detection results are achieved.

CN118851242APending Publication Date: 2024-10-29XIAN TECH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410846553.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing technology cannot provide efficient quantitative detection and monitoring of ammonia hydrogen (NH3) gas, and the application of ceria in the sensor field is limited by agglomeration problems, resulting in low gas sensing performance.

Method used

Highly dispersed ceria is used to load hydrogen-substituted graphite monoyne composite materials. CeO2 is evenly distributed on hydrogen-substituted graphite monoyne (HsGY) through the preparation method to form a cubic-shaped composite material, which increases the specific surface area to improve gas sensing performance.

Benefits of technology

It achieves highly sensitive detection of NH3 gas, has good sensor stability and fast response-recovery speed, overcomes the problem of poor dispersion of CeO2, and provides more active sites to improve sensitivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851242A_ABST
    Figure CN118851242A_ABST
Patent Text Reader

Abstract

The invention relates to a high-dispersion cerium dioxide loaded hydrogen substituted graphdiyne composite material for an NH3 detection sensor and a preparation method of the composite material. The method comprises the following steps: step 1, preparing HsGY powder; step 2, synthesizing the HsGY CeO2 composite material: preparing a cerium nitrate solution and a sodium hydroxide solution, and respectively stirring at room temperature; adding polyvinylpyrrolidone, HsGY powder and the sodium hydroxide solution into a cerium nitrate solution; then carrying out hydrothermal treatment, washing and drying; and finally calcining. According to the invention, high dispersion of CeO2 is realized, interface contact between HsGY and CeO2 can be improved to the greatest extent, adsorption of more gas molecules and transmission of carriers in a gas-sensitive test process are facilitated, and more active sites are provided for target gas, so that the gas-sensitive performance is improved; the prepared sensor is good in stability, has high sensitivity to 10-80 ppmNH3, is applied to a gas sensitive sensor to detect NH3 gas, is high in response-recovery speed, and can realize high-sensitivity detection of NH3 at room temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of gas sensors, and in particular relates to a highly dispersed cerium dioxide loaded hydrogen-substituted graphite monoacetylene composite material for an NH3 detection sensor and a preparation method thereof. Background Art

[0002] NH3 is widely used in the synthesis of various chemicals, including fertilizers and explosives, and they are key ingredients in agricultural and industrial processes. However, NH3 is a colorless gas that is corrosive and can be harmful to human health and the environment. Prolonged exposure to high concentrations of NH3 can cause serious health effects on the skin, eyes, nose, and even breathing and brain. According to the U.S. Occupational Safety and Health Administration (OSHA), the safe exposure limit of NH3 has been used in various applications such as fertilizers, petroleum industry, cleaning products, and refrigerants. The NH3 safe exposure limit is 25ppm. Therefore, the quantitative detection and monitoring of NH3 has become a critical issue that needs to be addressed in various environments.

[0003] Recently, two-dimensional (2D) materials have been widely studied for gas sensors. Hydrogen-substituted graphene (HsGY) is an intrinsic bandgap semiconductor composed of sp and sp 2 A carbon material composed of hybridized carbon atoms, showing a two-dimensional planar lattice structure. First principle calculations (DFT) show that HsGY exhibits greater adsorption energy for small molecule gases, higher electron capture ability and detection ability for NH3 gas at room temperature compared to graphene. It has been experimentally demonstrated that HsGY has a high conductivity (0.045S / m) and was first applied to NH3 detection at room temperature, with a response value of 4.9 for 100ppm NH3, which is due to the high chemical reactivity of its alkyne bond.

[0004] Cerium dioxide (CeO2) is an n-type semiconductor. Due to its 4f shell properties, unique electronic structure and Ce element (Ce 3+ and Ce 4+ ) has been widely used as NH3 gas sensor due to its highly reversible redox reaction between multiple valence states. However, CeO2 obtained by various preparation methods is very easy to agglomerate, resulting in low gas-sensitive performance, which limits the application of CeO2 in the sensor field.

[0005] In summary, the existing technology cannot provide an effective solution for efficient quantitative detection and monitoring of NH3. Summary of the invention

[0006] The purpose of the present invention is to provide a highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for an NH3 detection sensor and a preparation method thereof, so as to solve the problem that the prior art cannot provide efficient quantitative detection and monitoring of NH3.

[0007] In order to achieve the purpose of the present invention, the present invention provides a highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for NH3 detection sensor and a preparation method thereof, comprising the following steps:

[0008] Step 1: Preparation of HsGY powder:

[0009] Step 2: Synthesis of HsGY@CeO2 composite material:

[0010] (1) preparing a cerium nitrate solution and a sodium hydroxide solution, respectively, and stirring them at room temperature; then adding polyvinyl pyrrolidone, HsGY powder and the above sodium hydroxide solution to the cerium nitrate solution, and ultrasonically stirring them at room temperature; then transferring the solution to a stainless steel high-pressure container, performing a hydrothermal treatment, and washing the precipitate with ethanol and pure water for several times after cooling, respectively, and vacuum drying; finally placing the solid in a muffle furnace and calcining it at 400-600° C. for 3-5 hours.

[0011] Furthermore, in the above step 2, 1-3 g of cerium nitrate hexahydrate (99.0%) is dissolved in 30-50 mL of pure water to form a cerium nitrate solution, which is stirred at room temperature for 20-30 minutes.

[0012] Furthermore, in the above step 2, 16-17 g of sodium hydroxide (96.0%) is dissolved in 20-40 mL of pure water to form a sodium hydroxide solution, which is stirred at room temperature for 20-30 minutes.

[0013] Furthermore, 0.5-1 g of the polyvinyl pyrrolidone and 10-30 mg of HsGY powder are added, and ultrasonic stirring is performed at room temperature for 20-30 minutes.

[0014] Furthermore, the temperature of the hydrothermal treatment is 150-200° C. and the time is 18-24 hours.

[0015] Furthermore, the vacuum drying is carried out at a temperature of 60-100° C. and for a time of 6-14 hours.

[0016] Furthermore, the calcination temperature is 400-600° C. and the calcination time is 3-5 hours.

[0017] Furthermore, the above step 1 is specifically to firstly uniformly dissolve 100-300 mg of 1,3,5-triethynylbenzene in 100-200 mL of chloroform solvent to form an organic phase at the interface of the two phases; then slowly add an aqueous phase formed by 200-400 mL of pure water along the wall of the glass container; then add an aqueous solution containing 50-150 mg of bis(triphenylphosphine)palladium(II) chloride, 20-40 mg of cuprous iodide and 400-420 mg of 1,3,5-tribromobenzene to the above aqueous phase, and perform a synthesis reaction at room temperature for 72-96 hours; finally, put HsGY into a mortar and grind it for 5-10 minutes to form HsGY powder.

[0018] Furthermore, the NH3 detection sensor prepared by the above preparation method uses a highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material.

[0019] The beneficial effects of the present invention are:

[0020] (1) The present invention prepares a composite material of cubic CeO2 and HsGY, in which the CeO2 cubes are distributed on the HsGY in a uniform and discrete state. Therefore, the HsGY@CeO2 composite material has a large specific surface area and can maximize the interface contact between HsGY and CeO2. This structure is conducive to the adsorption of more gas molecules and the transmission of carriers during gas sensing testing, providing more active sites for the target gas, thereby improving the gas sensing performance.

[0021] (2) The sensor prepared by the present invention has good stability, high sensitivity to 10-80ppm NH3, can be used in gas sensors to detect NH3 gas, and has a fast response-recovery speed. Therefore, high-sensitivity detection of NH3 can be achieved at room temperature.

[0022] (3) Since the load material used is HsGY, which contains abundant alkyne bonds, high dispersion of CeO2 is achieved. The present invention utilizes the advantage of anchoring and separating CeO2 by alkyne bonds in HsGY, and composites the two, thus overcoming the problem of poor dispersion of CeO2 as a sensor. At the same time, the larger specific surface area provides more active sites for NH3 gas sensing, which is conducive to improving sensitivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Raman analysis (Raman) of the HsGY@CeO2 composite material obtained in Example 2;

[0024] Figure 2 X-ray electron spectroscopy (XPS) analysis of the HsGY@CeO2 composite material obtained in Example 2;

[0025] Figure 3X-ray diffraction analysis (XRD) of the HsGY@CeO2 composite material obtained in Example 2;

[0026] Figure 4 Fourier transform infrared spectroscopy analysis (FT-IR) of the HsGY@CeO2 composite material obtained in Example 2;

[0027] Figure 5 The ultraviolet-visible diffuse reflectance absorption spectrum analysis (UV-vis) of the HsGY@CeO2 composite material obtained in Example 2;

[0028] Figure 6 The scanning electron microscope (SEM) and X-ray energy spectrum (EDS) of the HsGY@CeO2 composite material obtained in Example 2;

[0029] Figure 7 This is a transmission electron microscopy (TEM) image of the HsGY@CeO2 composite material obtained in Example 2;

[0030] Figure 8 The Brunauer-Emmett-Teller surface area and pore size distribution (BET) of the HsGY@CeO2 composite material obtained in Example 2;

[0031] Fig. 9 This is the NH3 gas-sensing property diagram of the HsGY@CeO2 composite material obtained in Example 2. DETAILED DESCRIPTION

[0032] The method of the present invention is described below by specific examples, but the present invention is not limited thereto. The experimental methods described in the following examples are conventional methods unless otherwise specified, and the reagents and materials can be obtained from commercial sources unless otherwise specified. These descriptions are only to further illustrate the features and advantages of the present invention, and are not intended to limit the claims of the present invention.

[0033] Embodiment 1: A method for preparing a highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for an NH3 detection sensor, comprising the following steps:

[0034] Step 1: Preparation of HsGY powder:

[0035] 100 mg of 1,3,5-triethynylbenzene was uniformly dissolved in 100 mL of chloroform solvent to form an organic phase at the interface of the two phases, and then an aqueous phase formed by 200 mL of pure water was slowly added along the wall of the glass container. After that, an aqueous solution containing 50 mg of bis(triphenylphosphine)palladium(II) chloride, 20 mg of cuprous iodide and 400 mg of 1,3,5-tribromobenzene was added to the above aqueous phase, and the synthesis reaction was carried out at room temperature for 72 hours. Finally, HsGY was placed in a mortar and ground for 5 minutes to form HsGY powder.

[0036] Step 2: Synthesis of HsGY@CeO2 composite material:

[0037] 3g of cerium nitrate hexahydrate (mass concentration 99.0%) was dissolved in 30mL of pure water to form a cerium nitrate solution, and 16g of sodium hydroxide (mass concentration 96.0%) was dissolved in 20mL of pure water to form a sodium hydroxide solution, which were stirred at room temperature for 20 minutes. Then 0.5g of polyvinyl pyrrolidone, 30mg of HsGY powder and the above sodium hydroxide solution were added to the cerium nitrate solution, and ultrasonically stirred for 30 minutes at room temperature. After that, the solution was transferred to a 100mL stainless steel high-pressure container, hydrothermally treated at 150°C for 18 hours, and the precipitate was washed 3 times with ethanol and pure water respectively after cooling, and vacuum dried at 60°C for 14 hours. Finally, the solid was placed in a muffle furnace and calcined at 400°C for 3 hours.

[0038] Embodiment 2: A method for preparing a highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for an NH3 detection sensor, comprising the following steps:

[0039] Step 1: Preparation of HsGY powder:

[0040] 200 mg of 1,3,5-triethynylbenzene was uniformly dissolved in 150 mL of chloroform solvent to form an organic phase at the interface of the two phases, and then an aqueous phase formed by 300 mL of pure water was slowly added along the wall of the glass container. Then, an aqueous solution containing 100 mg of bis(triphenylphosphine)palladium(II) chloride, 30 mg of cuprous iodide and 410 mg of 1,3,5-tribromobenzene was added to the above aqueous phase, and the synthesis reaction was carried out at room temperature for 84 hours. Finally, HsGY was placed in a mortar and ground for 8 minutes to form HsGY powder.

[0041] Step 2: Synthesis of HsGY@CeO2 composite material:

[0042] 2g of hexahydrated cerium nitrate (mass concentration 99.0%) was dissolved in 40mL of pure water to form a cerium nitrate solution, and 16.5g of sodium hydroxide (mass concentration 96.0%) was dissolved in 30mL of pure water to form a sodium hydroxide solution, and then stirred at room temperature for 30 minutes. Next, 0.7g of polyvinyl pyrrolidone, 30mg of HsGY powder and the above sodium hydroxide solution were added to the cerium nitrate solution, and ultrasonically stirred at room temperature for 30 minutes. The solution was then transferred to a 100mL stainless steel high-pressure container, hydrothermally treated at 180°C for 21 hours, and the precipitate was washed 4 times with ethanol and pure water respectively after cooling, and vacuum dried at 80°C for 16 hours. Finally, the solid was placed in a muffle furnace and calcined at 500°C for 4 hours.

[0043] Embodiment 3: A method for preparing a highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for an NH3 detection sensor, comprising the following steps:

[0044] Step 1: Preparation of HsGY powder:

[0045] 300 mg of 1,3,5-triethynylbenzene was uniformly dissolved in 200 mL of chloroform solvent to form an organic phase at the interface of the two phases. An aqueous phase formed by 400 mL of pure water was slowly added along the wall of the glass container. Then, an aqueous solution containing 150 mg of bis(triphenylphosphine)palladium(II) chloride, 40 mg of cuprous iodide and 420 mg of 1,3,5-tribromobenzene was added to the above aqueous phase, and the synthesis reaction was carried out at room temperature for 96 hours. Finally, HsGY was placed in a mortar and ground for 10 minutes to form HsGY powder.

[0046] Step 2: Synthesis of HsGY@CeO2 composite material:

[0047] 1g of cerium nitrate hexahydrate (mass concentration 99.0%) was dissolved in 50mL of pure water to form a cerium nitrate solution, and 17g of sodium hydroxide (mass concentration 96.0%) was dissolved in 40mL of pure water to form a sodium hydroxide solution, and then stirred at room temperature for 30 minutes. Next, 1g of polyvinyl pyrrolidone, 20mg of HsGY powder and the above sodium hydroxide solution were added to the cerium nitrate solution, and ultrasonically stirred at room temperature for 30 minutes. The solution was then transferred to a 100mL stainless steel high-pressure container, hydrothermally treated at 200°C for 18 hours, and after cooling, the precipitate was washed 5 times with ethanol and pure water, respectively, and vacuum dried at 100°C for 18 hours. Finally, the solid was placed in a muffle furnace and calcined at 600°C for 5 hours.

[0048] Example 2 is the best example. The HsGY@CeO2 composite material prepared in Example 2 is used as a gas-sensitive material, and the composite material is coated on the Ag-Pd interdigital electrode by drop coating. The electrode substrate with the gas-sensitive material is heated to 300°C at a rate of 15°C / min and kept at this temperature for 200 minutes by high-temperature annealing, and then cooled to room temperature in the furnace to obtain an NH3 gas sensor. Related experiments are carried out, and the results are as follows:

[0049] (a) Raman spectrum of HsGY@CeO2 composite material

[0050] The Raman spectrum of the HsGY@CeO2 composite material prepared by the present invention is as follows: Figure 1 As shown, the spectrum of CeO2 is at 460 cm -1 A sharp peak appears at , which is attributed to the F 2g vibration, while the D band (1378cm -1) and G band (1581cm -1 ) corresponds to E in the material 2g The first-order scattering of the mode and the existence of defects in HsGY. In addition, the vibration of the conjugated acetylenic bond (-C≡C-) of HsGY@CeO2 is about 2210cm -1 It shows that the HsGY@CeO2 composite material was successfully prepared.

[0051] (b) XPS spectrum of HsGY@CeO2 composite material

[0052] The XPS spectrum of the HsGY@CeO2 composite material prepared by the present invention is as follows: Figure 2 As shown, the entire range of the total energy spectrum has corresponding C (C 1s), O (O 1s) and Ce (Ce 3d 3 / 2 and Ce 3d 5 / 2 ) element's peak value ( Figure 2 a), confirming the chemical composition of the HsGY@CeO2 composite material. C1s spectrum of HsGY@CeO2 ( Figure 2 b) can be decomposed into binding energies of 284.6 eV (CC (sp 2 )), 285eV (CC(sp)), 286.2eV (CO) and 288.5eV (C=O). Figure 2 c Calculation of oxygen vacancies (O v ) component is 33.2%, indicating that the HsGY@CeO2 composite material has a strong oxygen absorption capacity. Figure 2 As shown in Figure d, the Ce 3d spectrum of HsGY@CeO2 can be divided into 8 peaks, among which the peaks marked as V0, V1, V2, V3 and U0, U1, U2, U3 can be attributed to Ce 3d 5 / 2 and Ce 3d 3 / 2 The peaks labeled V1 and U1 represent Ce 3+ The initial electronic state of 3d104f1, the remaining peaks correspond to Ce 4+ 3d104f0, this is due to the high reducibility of the CeO2 surface, which leads to the 3+ and Ce 4+ The electronic states coexist.

[0053] (c) XRD pattern of HsGY@CeO2 composite material

[0054] The XRD pattern of the HsGY@CeO2 composite material prepared by the present invention is as follows: Figure 3As shown, it can be seen that CeO2 crystals have been formed, and their diffraction peaks are located at 28.6°, 33.2°, 47.5°, 56.4°, 59.1°, 69.4°, 77.0°, 79.1° and 89.2°, corresponding to (111), (200), (220), (311), (222), (400), (331), (420) and (422) of CeO2, respectively. In addition, the peak at 24° corresponds to the 0.37nm diffraction spacing of HsGY, proving that the HsGY@CeO2 composite material was successfully prepared.

[0055] (d) FT-IR spectrum of HsGY@CeO2 composite material

[0056] The FT-IR spectrum of the HsGY@CeO2 composite material prepared by the present invention is as follows: Figure 4 As shown, it can be seen that at about 480cm -1 There is only one obvious peak at 3400 cm-1, which is attributed to the Ce-O-Ce vibration mode. -1 A peak was observed near 1406 cm -1 The main peak at 2196cm is attributed to the skeleton vibration of the aromatic ring, revealing the presence of the benzene ring. -1 The observed weak band is attributed to the acetylene band, proving that the HsGY@CeO2 composite material was successfully prepared.

[0057] (e) UV-vis spectrum of HsGY@CeO2 composite material

[0058] The electronic band structure of HsGY@CeO2 composite material was further analyzed by UV-vis. The band gap ( Figure 5 ). From (αhν) 1 / 2 The bandgap width (E g ) is 1.64eV.

[0059] (f) SEM image of HsGY@CeO2 composite material

[0060] SEM test results ( Figure 6 ) showed that CeO2 cubes were distributed on HsGY in a uniform and discrete state, which led to an increase in the specific surface area of ​​the HsGY@CeO2 composite material. This structure is beneficial to the adsorption of more gas molecules and the transport of carriers during gas sensing testing, providing more active sites for the target gas.

[0061] (g) TEM and EDS images of HsGY@CeO2 composite materials

[0062] From the TEM test results ( Figure 7 a) It can be seen that CeO2 cubes are uniformly and discretely fixed on HsGY. The crystallinity and lattice spacing of HsGY and CeO2 were recorded using high-resolution TEM ( Figure 7 b), confirming the amorphous nature of HsGY, the lattice edge of HsGY@CeO2 shows The lattice spacing of CeO2 (111) is very close to that of CeO2, and the close interface between CeO2 and HsGY can also be clearly seen. In addition, in the SAED pattern ( Figure 7 c) The observed clear diffraction rings also demonstrate the polycrystalline nature of the HsGY@CeO2 composite. Figure 7 The EDS of df shows that C, O and Ce elements are uniformly distributed on the surface, which also confirms the successful preparation of HsGY@CeO2 composites.

[0063] (h) BET surface area and pore size distribution of HsGY@CeO2 composites

[0064] The BET surface area and pore size distribution test results of HsGY@CeO2 composite materials are shown in Figure 8 As shown in Figure 2, it can be seen that the specific surface area of ​​the HsGY@CeO2 composite material is 176.27 m 2 / g, and its larger specific surface area provides more active sites for NH3 gas sensing, which is beneficial to improving the sensitivity.

[0065] (i) Analysis of NH3 gas-sensing properties of HsGY@CeO2 composite material

[0066] See also Fig. 9 It can be seen that the gas-sensitive response value of the HsGY@CeO2 composite material sensor prepared in Example 2 increases with the increase of NH3 concentration at room temperature. At the same time, the response-recovery time to 80ppm NH3 is 31s and 111s, respectively, and the linear relationship is good from 10 to 80ppm NH3 (R 2 =0.981).

[0067] The above embodiments are only preferred technical solutions of the present invention and are not to be regarded as limitations of the present invention. The protection scope of the present invention shall be the technical solutions recorded in the claims, including equivalent replacement solutions of the technical features in the technical solutions recorded in the claims, that is, equivalent replacement improvements within this scope are also within the protection scope of the present invention.

Claims

1. A method for preparing a highly dispersed cerium dioxide-loaded hydrogen-substituted graphite monoacetylene composite material for NH3 detection sensors, characterized in that: The steps include: Step 1: Preparation of HsGY powder: Step 2: Synthesis of HsGY@CeO2 composite material: A cerium nitrate solution and a sodium hydroxide solution are prepared and stirred at room temperature respectively; then polyvinyl pyrrolidone, HsGY powder and the sodium hydroxide solution are added to the cerium nitrate solution and ultrasonically stirred at room temperature; The solution is then transferred to a stainless steel high-pressure container for hydrothermal treatment. After cooling, the precipitate is washed several times with ethanol and pure water respectively, and vacuum dried. Finally, the solid is placed in a muffle furnace and calcined at 400-600°C for 3-5 hours.

2. The method for preparing the highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for NH3 detection sensor according to claim 1, characterized in that: In the step 2, 1-3 g of cerium nitrate hexahydrate with a mass concentration of 99.0% is dissolved in 30-50 mL of pure water to form a cerium nitrate solution, which is stirred at room temperature for 20-30 minutes.

3. The method for preparing the highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for NH3 detection sensor according to claim 2, characterized in that: In the step 2, 16-17 g of sodium hydroxide with a mass concentration of 96.0% is dissolved in 20-40 mL of pure water to form a sodium hydroxide solution, and the solution is stirred at room temperature for 20-30 minutes.

4. The method for preparing the highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for NH3 detection sensor according to claim 2 or 3, characterized in that: The polyvinyl pyrrolidone is added in an amount of 0.5-1 g and the HsGY powder is added in an amount of 10-30 mg, and the mixture is ultrasonically stirred at room temperature for 20-30 minutes.

5. The highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for NH3 detection sensor according to claim 4 and the preparation method thereof are characterized in that: The temperature of the hydrothermal treatment is 150-200° C. and the time is 18-24 hours.

6. The method for preparing the highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for NH3 detection sensor according to claim 5, characterized in that: The vacuum drying is carried out at a temperature of 60-100° C. and for a time of 6-14 hours.

7. The method for preparing the highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for NH3 detection sensor according to claim 6, characterized in that: The calcination temperature is 400-600° C. and the calcination time is 3-5 hours.

8. The method for preparing the highly dispersed ceria-loaded hydrogen-substituted graphite monoacetylene composite material for NH3 detection sensor according to claim 7, characterized in that: The step 1 specifically comprises firstly dissolving 100-300 mg of 1,3,5-triethynylbenzene uniformly in 100-200 mL of chloroform solvent to form an organic phase at the interface of the two phases, then slowly adding an aqueous phase formed by 200-400 mL of pure water along the wall of the glass container; then adding an aqueous solution containing 50-150 mg of bis(triphenylphosphine)palladium(II) chloride, 20-40 mg of cuprous iodide and 400-420 mg of 1,3,5-tribromobenzene to the aqueous phase, and performing a synthesis reaction at room temperature for 72-96 hours; finally, putting HsGY into a mortar and grinding it for 5-10 minutes to form HsGY powder.

9. The highly dispersed ceria-loaded hydrogen-substituted graphite monoyne composite material for NH3 detection sensor prepared by the preparation method according to claim 1.