Method for preventing glass plate from being blocked in high-temperature flushing or high-temperature wetting process of muffle furnace overflow brick

By adjusting the temperature and traction roller parameters during the glass production process, the problem of glass plate blocking during high-temperature washing or high-temperature wetting is solved, ensuring the continuity and efficiency of production, and avoiding blocking caused by winding the traction roller.

CN118851544AActive Publication Date: 2024-10-29SICHUAN SHUWANG CHENSHENG NEW MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411108296.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-10-29
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

During the glass production process, during high-temperature washing or high-temperature wetting, the glass plate is prone to unstable flow due to excessive temperature, resulting in overflow bricks and blockage, resulting in production interruption and economic losses.

Method used

By inserting cooling water pipes in the B2 area of ​​the setting furnace, the temperatures in different areas are adjusted, and the spacing and rotation speed of the traction rollers of the annealing furnace are adjusted to prevent the glass plate from wrapping around the traction rollers and causing blockage.

Benefits of technology

It effectively avoids the blockage caused by the winding of the traction roller during the high-temperature wetting or high-temperature washing process of the glass plate, ensuring normal production and improving production efficiency and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851544A_ABST
    Figure CN118851544A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preventing a glass plate from being blocked in the high-temperature flushing or high-temperature wetting process of a muffle furnace overflow brick, and relates to the technical field of glass production. According to the technical scheme, a cooling water pipe is inserted into a B2 area of a shaping furnace, so that the temperature of a B1 area of the shaping furnace is 1080 + / -20 DEG C, the temperature of the B2 area of the shaping furnace is 980 + / -20 DEG C, the temperature of a C1 area of an annealing furnace is 900 + / -20 DEG C, and the temperature of a C2 area of the annealing furnace is 800 + / -20 DEG C. In the forming high-temperature wetting or high-temperature washing process, the cooling water pipe is inserted into the B2 area of the shaping furnace, the temperatures of different areas of the shaping furnace and the annealing furnace are adjusted, and the parameters of the traction roller of the annealing furnace are adjusted, so that the phenomenon of material blockage at the traction roller of the annealing furnace due to winding of glass by the rotating traction roller can be well avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass production, and in particular to a method for preventing glass plates from being blocked during high-temperature washing or high-temperature wetting of muffle furnace overflow bricks. Background Art

[0002] In the production process of liquid crystal glass substrate forming equipment, in order to deal with some defects, such as: dealing with crystallization of the manifold, dealing with platinum needles, dealing with silicon zirconium stone and other defects, a high-temperature flushing method is often used to achieve the purpose of dealing with the above defects. High-temperature flushing means raising the temperature in the muffle furnace to above 1275°C, and flushing and washing the manifold and overflow bricks with a higher temperature flowing glass liquid to achieve the purpose of eliminating the above defects. However, when high-temperature flushing is adopted, it is easy to cause blocking, because after the temperature of the muffle furnace is increased, the temperature of the glass liquid in the muffle furnace is also very high, which can reach above 1275℃. The glass liquid flows down from the bottom of the overflow brick. Due to the high temperature and low viscosity of the glass plate, the traction roller in the annealing furnace cannot clamp the glass plate. When the glass plate flows down from the bottom of the overflow brick, the flow rate is very fast. When the glass plate flows through the setting furnace, annealing furnace and other locations, it flows freely by gravity. If no better method is adopted, the glass plate is easy to be folded and piled up in the furnace, thereby causing blocking in the setting furnace and annealing furnace. If it is not handled in time, more and more hot glass will accumulate in the furnace, which will soon cause blocking. The hot glass will fill the annealing furnace. If it is not handled in time, the hot glass will continue to accumulate in the setting furnace and even in the muffle furnace, causing great losses. Once blocked, the following problems will occur: 1) The kiln feeder will no longer feed; 2) The platinum channel must discharge from the mixing barrel and stop feeding to the molding equipment; 3) After the molding is cut off, when dealing with the broken glass at the blockage, the hot glass accumulates together to form a mass of glass balls, which is not easy to handle and takes a long time to shovel away bit by bit. After the treatment is completed, the molding equipment has to be re-wetted, which loses at least one week of time. Therefore, once blockage occurs, it will seriously affect normal production and cause significant economic losses. Therefore, it is urgent to provide a method to avoid glass plate blockage during high-temperature flushing or high-temperature wetting of muffle furnace overflow bricks to solve the above problems. Summary of the invention

[0003] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art and provide a method for preventing glass plates from being blocked during high-temperature flushing or high-temperature wetting of muffle furnace overflow bricks. During the high-temperature wetting and high-temperature flushing processes, it can not only ensure that the expected effects of high-temperature wetting and high-temperature flushing are achieved, but also avoid blockage caused by traction rollers wrapping around the glass.

[0004] When forming high-temperature wetting or high-temperature flushing overflow bricks, the glass temperature on the overflow bricks is above 1275℃, and the glass liquid flows down from the tip of the overflow brick, and the tip temperature is above 1235℃, and enters the shaping furnace to form a glass ribbon. Because the muffle furnace is not equipped with a side-pulling machine under high temperature, the glass ribbon is not clamped by the side-pulling machine, and flows vertically and freely downward by its own gravity, then flows to the traction roller of the annealing furnace, then to the outlet of the annealing furnace, and finally enters the broken glass tank. In this downward process, the glass ribbon passes through the B1 and B2 zones of the shaping furnace, and then flows through the C1 and C2 zones of the annealing furnace where the traction rollers are installed, and finally passes through the C3-C9 zones of the annealing furnace to the outlet of the annealing furnace and enters the broken glass tank. If the temperature of the glass ribbon is not well controlled, the glass ribbon is prone to folding, bending, breaking, winding and balling in the middle, thereby forming blockage.

[0005] Based on the above situation, the technical solution of the present invention is:

[0006] A method to avoid glass plate clogging during high-temperature flushing or high-temperature wetting of the muffle furnace overflow bricks is to insert a cooling water pipe into the B2 zone of the shaping furnace to make the temperature of the B1 zone of the shaping furnace 1080±20℃, the temperature of the B2 zone 980±20℃, the temperature of the C1 zone of the annealing furnace 900±20℃, and the temperature of the C2 zone 800±20℃.

[0007] If the temperature in the above-mentioned area is too high, the glass ribbon will easily wrap around the traction roller and adhere to other equipment when it flows to the annealing furnace and other equipment, forming a blockage; at the same time, due to the high temperature, after the glass ribbon reaches the annealing furnace outlet, under the action of water, the glass ribbon will not break, but will easily hinder the flow at the broken glass mouth, pushing the glass ribbon upward, and the upper glass ribbon will easily bend, causing blockage. When the temperature in the above-mentioned area is too low, the glass ribbon will easily break in the annealing furnace area, and the middle glass ribbon will easily break. Once the middle of the glass ribbon breaks, there will be no stable downward gravity, and the glass will not be smoothly pulled and flowed downward, and the glass ribbon will float in the shaping furnace and annealing furnace. When encountering interference, the glass ribbon will be folded, and the shaping furnace glass will adhere to the silicon-carbon plate, and the annealing furnace will form an accumulation of blockage.

[0008] Preferably, the cooling water pipe spans across the B2 zone of the shaping furnace.

[0009] Preferably, the diameter of the cooling water pipe is 20-25 mm.

[0010] Preferably, during high-temperature flushing or high-temperature wetting, the traction rollers on the left and right sides of the annealing furnace are supported so that the spacing between the two traction rollers is 10-15 mm and the support height of the rocker arm outside the traction roller is 15-25 mm.

[0011] The purpose of this operation is: 1) If the gap between the traction rollers is too small or there is no gap, a clamping force will be formed on the glass ribbon. The force will be transmitted to the glass ribbon. Since the temperature of the glass ribbon here is still very high, the glass ribbon will form a clamping and holding force. This force will form a force on the glass ribbon in the rotation direction of the traction roller, so that the glass ribbon will be wrapped around the traction roller along the rotation direction of the traction roller. Once wrapped, if it is not handled in time, it will cause blockage, resulting in serious consequences; 2) If the gap between the traction rollers is too large, the traction roller will not play a traction role. If the gap is too large, the airflow will turn up, causing the glass ribbon to be unstable when flowing downward and easily folded. The flow of the glass ribbon is disturbed, causing blockage.

[0012] Preferably, the rotation speed of the traction roller is 5000-8000 mm / min.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] 1. In the process of high-temperature wetting or high-temperature washing during molding, the present invention inserts a cooling water pipe into the B2 zone of the shaping furnace, adjusts the temperatures of different zones of the shaping furnace and the annealing furnace, and adjusts the parameters of the traction roller of the annealing furnace, thereby effectively avoiding the phenomenon of material blockage at the traction roller of the annealing furnace due to the rotating traction roller winding around the glass.

[0015] 2. The method of the present invention can solve the problem of blockage caused by traction rollers entangled in the glass, thereby avoiding the occurrence of blockage and allowing the high-temperature wetting or high-temperature flushing process to proceed normally and smoothly, achieving the purpose of countermeasures against defects through high-temperature flushing, allowing normal production, improving production efficiency, and creating economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a structural schematic diagram of a shaping furnace and an annealing furnace of the present invention.

[0017] In the figure, 1. Muffle furnace; 2. Shaping furnace; 201. B1 zone; 202. B2 zone; 3. Cooling water pipe; 4. Annealing furnace; 401. C1 zone; 402. C2 zone; 5. Pulling roller. DETAILED DESCRIPTION

[0018] In order to enable persons skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.

[0019] like Figure 1As shown, the present invention provides a method for avoiding glass plate blocking during high-temperature washing or high-temperature wetting of muffle furnace overflow bricks, a cooling water pipe 3 with a diameter of 20-25 cm is inserted into the B2 zone 202 of the shaping furnace 2, and the cooling water pipe 3 spans the B2 zone 202 of the shaping furnace 2, so that the temperature of the B1 zone 201 of the shaping furnace 2 is 1080±20℃, the temperature of the B2 zone 202 is 980±20℃, the temperature of the C1 zone 401 of the annealing furnace 4 is 900±20℃, and the temperature of the C2 zone 402 is 800±20℃.

[0020] At the same time, during high-temperature flushing or high-temperature wetting, the traction rollers 5 on the left and right sides of the annealing furnace 4 are supported so that the spacing between the two traction rollers 5 is 10-15mm, the rocker support height outside the traction roller 5 is 15-25mm, and the rotation speed of the traction roller 5 is 5000-8000mm / min.

[0021] Example 1

[0022] When producing the G6 generation liquid crystal glass substrate in this embodiment, due to the large amount of crystallization on the confluence plate at both ends of the overflow brick, the confluence state is not good, and the glass plate bait seriously affects the normal production, so it is decided to high-temperature flush the overflow brick of the muffle furnace 1. During high-temperature flushing, the conditions are set as follows: the temperature of the A zone of the muffle furnace 1 is about 1275°C, the temperature of the tip of the overflow brick is about 1235°C, the diameter of the cooling water pipe 3 inserted in the B2 zone 202 of the setting furnace 2 is 20mm, the temperature of the B1 zone 201 of the setting furnace 2 is set to 1060°C, the temperature of the B2 zone 202 is set to 960°C, the temperature of the C1 zone 401 of the annealing furnace 4 is set to 880°C, and the temperature of the C2 zone 402 is set to 780°C. At the same time, the traction rollers 5 on the left and right sides of the annealing furnace 4 are supported, so that the spacing between the two traction rollers 5 is 10mm, the rocker support height outside the traction roller 5 is 15mm, and the rotation speed of the traction roller 5 is 5000mm / min.

[0023] After this high-temperature flushing was completed, the formed lead plate was produced normally with very good results. The crystallization of the busbars at both ends of the overflow brick was basically flushed, the production was very stable, and the yield rate was significantly improved.

[0024] Comparative Example 1

[0025] Comparative Example 1 When producing G6 generation liquid crystal glass substrates, due to the large amount of crystallization on the confluence plates at both ends of the overflow bricks, the confluence condition is poor, and the bait has bubble belts, which often cause broken plates to occur, seriously affecting normal production. Therefore, it is decided to high-temperature flush the overflow bricks of the muffle furnace 1. During high-temperature flushing, the temperature of the A zone of the muffle furnace 1 is about 1270°C, the temperature of the tip of the overflow brick is about 1230°C, and the diameter of the cooling water pipe 3 inserted in the B2 zone 202 of the setting furnace 2 is 30mm, so that the temperature of the B1 zone 201 of the setting furnace 2 is 1055°C, the temperature of the B2 zone 202 is 955°C, and the temperature of the C1 zone 401 of the annealing furnace 4 is 855°C, and the temperature of the C2 zone 402 is 775°C.

[0026] During this high-temperature washing process, the glass plates were often broken in the annealing furnace 4, causing the glass plates to break. The broken glass had to be cleaned manually, and the high-temperature washing did not maintain continuity. After the washing was completed, after the forming lead plate was produced, the crystallization of the busbar was reduced to a certain extent, but it was not significantly improved. During the production process, it was not long before the state before the high-temperature washing appeared again, and the high-temperature washing had to be carried out again. Analysis of the reasons showed that the temperature of the high-temperature washing did not reach the predetermined temperature, and the frequent plate breaking treatment and window opening to clean the broken glass would cause the temperature in the furnace to drop, resulting in the inability to continuously wash at high temperature.

[0027] Example 2

[0028] When producing the G5 liquid crystal glass substrate in this embodiment, due to the platinum needle defect in the glass plate, which lasted for a long time without improvement, seriously affecting the quality and yield rate, the overflow brick of the muffle furnace 1 was washed at high temperature, and the washing setting parameters were: the cooling water pipe 3 inserted in the B2 zone 202 of the setting furnace 2 was 25mm in diameter, so that the temperature of the B1 zone 201 of the setting furnace 2 was 1100°C, the temperature of the B2 zone 202 was 1000°C, the temperature of the C1 zone 401 of the annealing furnace 4 was 920°C, and the temperature of the C2 zone 402 was 820°C. At the same time, the traction rollers 5 on the left and right sides of the annealing furnace 4 were supported, so that the spacing between the two traction rollers 5 was 15mm, the rocker support height outside the traction roller 5 was 25mm, and the rotation speed of the traction roller 5 was 8000mm / min.

[0029] After this high-temperature washing and normal production of the formed lead plate, the platinum needle defects on the glass plate basically disappeared and the yield rate was greatly improved.

[0030] Comparative Example 2

[0031] Comparative Example 2 When producing G5 liquid crystal glass substrate, due to the platinum needle defect in the glass plate, the overflow brick was washed at high temperature, and the parameters were set as follows: the diameter of the cooling water pipe 3 inserted in the B2 zone 202 of the shaping furnace 2 was 18 mm, the temperature of the B1 zone 201 of the shaping furnace 2 was 1105°C, the temperature of the B2 zone 202 was 1005°C, the temperature of the C1 zone 401 of the annealing furnace 4 was 930°C, and the temperature of the C2 zone 402 was 830°C. The traction roller 5 of the C2 zone 402 of the annealing furnace 4 was not supported and clamped the glass.

[0032] During this high-temperature washing process, a serious material blocking accident occurred. Due to the high temperature of the glass ribbon, the glass ribbon was wrapped around the traction roller 5 at the traction roller 5 in the 402 area of ​​the annealing furnace 4C2. The glass ribbon accumulated and blocked the annealing furnace 4. In addition, the personnel did not handle it in time, and the glass piled up more and more. The annealing furnace 4C1 area 401 and the shaping furnace 2B area were all blocked with glass. The situation was very dangerous. The kiln was ordered to stop feeding, and the platinum channel was unloaded from the mixing barrel, and no more material was fed to the molding. Then the molding was cooled down, and the glass in the shaping furnace 2 and the annealing furnace 4 was processed. It took nearly a shift to clean up the broken glass, and then the temperature was raised again to continue the high-temperature washing operation. This high-temperature washing process was very dangerous.

[0033] Example 3

[0034] In the process of high temperature wetting overflow bricks in producing G8.5 generation liquid crystal substrates in this embodiment, the parameters are set as follows: the diameter of the cooling water pipe 3 inserted in the B2 zone 202 of the setting furnace 2 is 22 mm, the temperature of the B1 zone 201 of the setting furnace 2 is 1080°C, the temperature of the B2 zone 202 is 1000°C, the temperature of the C1 zone 401 of the annealing furnace 4 is 900°C, and the temperature of the C2 zone 402 is 800°C. At the same time, the traction rollers 5 on the left and right sides of the annealing furnace 4 are supported, so that the spacing between the two traction rollers 5 is 13 mm, the support height of the rocker arm outside the traction roller 5 is 20 mm, and the rotation speed of the traction roller 5 is 6500 mm / min.

[0035] After the high-temperature wetting overflow brick was completed, the forming lead plate was produced normally. It was found that the forming quality was very stable, no other quality defects occurred, and the yield rate was quickly improved.

[0036] Comparative Example 3

[0037] Comparative Example 3 produces G8.5 generation liquid crystal substrates. During the high-temperature wetting overflow brick process, the difference from Example 3 is that the cooling water pipe 3 inserted in the B2 zone 202 of the shaping furnace 2 has a diameter of 27 mm, so that the temperature of the B1 zone 201 of the shaping furnace 2 is 1050°C, the temperature of the B2 zone 202 is 950°C, the temperature of the C1 zone 401 of the annealing furnace 4 is 850°C, and the temperature of the C2 zone 402 is 760°C.

[0038] After the wetting was completed and the forming lead plate was produced, it was found that there were several light and dark lines on the surface of the glass plate. These light and dark lines seriously affected the quality of the glass plate. Some were within the specifications, but one light and dark line could not be judged as good. Then the forming countermeasures took a long time before it was judged as a good product.

[0039] It can be seen from the above embodiments that no matter it is high-temperature flushing or high-temperature wetting operation for overflow bricks, the parameters are set as follows: inserting a 20-25mm Ø cooling water pipe 3 into the B2 zone 202 of the setting furnace 2, making the temperature of the B1 zone 201 of the setting furnace 2 1080±20℃, the temperature of the B2 zone 202 980±20℃, the temperature of the C1 zone 401 of the annealing furnace 4 900±20℃, the temperature of the C2 zone 402 800±20℃; the setting of the traction roller 5: the spacing between the two traction rollers 5 is 10-15mm, the support height of the rocker arm outside the traction roller 5 is 15-25mm; the rotation speed of the traction roller 5 is: 5000-8000mm / min. Setting the above parameters can achieve the flushing effect of overflow bricks, will not cause blockage in the annealing furnace 4, and will not cause some defects that affect the quality of the glass plate. It can be seen from the above comparative examples that if the parameters exceed the above range, many problems will arise, the most serious of which is blockage. The flushing will not achieve the desired effect and will have to be flushed again. In addition, new defects that affect the quality of the glass plate will appear, which will seriously affect normal production and the improvement of the glass plate yield rate.

Claims

1. A method for preventing glass plate blocking during high-temperature washing or high-temperature wetting of muffle furnace overflow bricks, characterized in that: A cooling water pipe (3) is inserted into the B2 zone (202) of the shaping furnace (2) to make the temperature of the B1 zone (201) of the shaping furnace (2) 1080±20°C, the temperature of the B2 zone (202) 980±20°C, the temperature of the C1 zone (401) of the annealing furnace (4) 900±20°C, and the temperature of the C2 zone (402) 800±20°C.

2. The method for preventing glass plate blocking during high temperature washing or high temperature wetting of muffle furnace overflow bricks according to claim 1, characterized in that: The cooling water pipe (3) spans across the B2 zone (202) of the shaping furnace (2).

3. The method for avoiding glass plate blocking during high temperature washing or high temperature wetting of muffle furnace overflow bricks according to claim 1, characterized in that: The diameter of the cooling water pipe (3) is 20-25 mm.

4. The method for preventing glass plate blocking during high temperature washing or high temperature wetting of muffle furnace overflow bricks according to claim 1, characterized in that: During high temperature flushing or high temperature wetting, the traction rollers (5) on the left and right sides of the annealing furnace (4) are supported so that the distance between the two traction rollers (5) is 10-15 mm and the support height of the rocker arm outside the traction roller (5) is 15-25 mm.

5. The method for preventing glass plate blocking during high temperature washing or high temperature wetting of muffle furnace overflow bricks according to claim 4, characterized in that: The rotation speed of the traction roller (5) is 5000-8000 mm / min.

Citation Information

Patent Citations

  • Method for cleaning materials in moulding furnace body

    CN106542722A

  • Overflow brick forming quality stability control method

    CN111807684A

  • Molding system and method for substrate glass warping stress partition control

    CN112811792A

  • Forming device for photoelectric display glass

    CN117125879A

  • Overflow brick washing device applied to muffle furnace

    CN209077349U