Glass ceramic, glass ceramic product and manufacturing method thereof

By rationally designing the component ratios of SiO2, Al2O3, Li2O, ZnO, TiO2 and other components in glass ceramics, the spinel crystal phase is formed, and through the chemical strengthening process, the problem of insufficient mechanical properties of existing glass ceramics after chemical strengthening is solved. problem, achieving excellent properties suitable for cover plate materials.

CN118851571APending Publication Date: 2024-10-29CDGM OPTICAL GLASS

Patent Information

Application Number
CN202310470758.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The mechanical properties of existing glass ceramics after chemical strengthening are difficult to meet the requirements for cover plate materials, and they are not easy to be chemically strengthened.

Method used

By rationally designing the component ratio, glass ceramics containing SiO2, Al2O3, Li2O, ZnO, TiO2 and other components can form a spinel crystal phase, and the mechanical properties can be improved through chemical strengthening processes.

Benefits of technology

Glass-ceramic products with excellent mechanical properties are obtained to meet the application needs of display devices or electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004203889110000381
    Figure BDA0004203889110000381
  • Figure BDA0004203889110000411
    Figure BDA0004203889110000411
  • Figure BDA0004203889110000421
    Figure BDA0004203889110000421
Patent Text Reader

Abstract

The invention provides a glass ceramic product, which comprises the following components in percentage by weight: 40 to 55 percent of SiO2; 15 to 30 percent of Al2O3; 0.1 to 6 percent of Li2O; 9 to 20 percent of ZnO; 0.1 to 6 percent of MgO; and 0.5 to 7 percent of TiO2, wherein the ratio of SiO2 to Al2O3 is 1.5 to 3.2. Through reasonable component design, the glass ceramic product obtained by the invention has excellent mechanical properties, and can be applied to the fields of display equipment or electronic equipment and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to glass ceramics, in particular to glass ceramics and glass ceramic products with excellent mechanical properties. Background Art

[0002] Glass ceramics are a type of material that is made by heat treating glass to precipitate crystals inside the glass. They have better mechanical properties than conventional glass, and their bending resistance, wear resistance, and drop resistance have obvious advantages over conventional glass. With the continuous rise and development of consumer electronic products, glass ceramics are widely used in such electronic devices. For example, devices such as LED and LCD displays and computer monitors, portable electronic products (such as mobile phones, tablet computers, and personal media terminals). Glass ceramics can further improve their mechanical properties through chemical strengthening. However, glass ceramics in the prior art are not easy to chemically strengthen, or the mechanical properties after chemical strengthening are difficult to meet the requirements for application in cover materials. Therefore, developing a glass ceramic with excellent mechanical properties and suitable for chemical strengthening has become a goal pursued by scientific and technological personnel. Summary of the invention

[0003] The technical problem to be solved by the present invention is to provide a glass ceramic having excellent mechanical properties and suitable for chemical strengthening, and a glass ceramic product made thereof.

[0004] The technical solution adopted by the present invention to solve the technical problem is:

[0005] (1) Glass-ceramic products, whose components, expressed in percentage by weight, contain: SiO 2 :40~55%;Al 2 O 3 :15~30%;Li 2 O: 0.1~6%; ZnO: 9~20%; MgO: 0.1~6%; TiO 2 :0.5~7%, of which SiO 2 / Al 2 O 3 It is 1.5 to 3.2.

[0006] (2) The glass-ceramic product according to (1), wherein the components, expressed in weight percentage, further contain: P 2 O 5 :0~5%;and / or ZrO 2 :0~5%;and / or Na 2 O: 0-6%; and / or B 2 O 3 :0~4%;and / or K 2 O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y2 O 3 : 0-6%; and / or clarifier: 0-2%.

[0007] (3) Glass ceramic products, whose components contain SiO 2 、Al 2 O 3 , ZnO and TiO 2 , the glass ceramic product contains a spinel crystal phase.

[0008] (4) Glass ceramic products, whose components contain SiO 2 、Al 2 O 3 , Li 2 O, ZnO and TiO 2 The drop ball test height of the glass ceramic product is above 1000 mm.

[0009] (5) A glass ceramic product containing a spinel crystal phase, wherein the glass ceramic product has a compressive strength of 400N or more.

[0010] (6) Glass ceramic products containing spinel crystal phase, the haze of glass ceramic products with a thickness of less than 1 mm is less than 0.3%.

[0011] (7) Glass ceramic products, the components of which contain SiO 2 、Al 2 O 3 , Li 2 O, ZnO and TiO 2 , the average optical |B| value of 400-800nm ​​for glass-ceramic products with a thickness of less than 1mm is less than 1.0.

[0012] (8) A glass ceramic product containing a spinel crystal phase, wherein the surface stress of the glass ceramic product is greater than 200 MPa.

[0013] (9) Glass ceramic products, the components of which contain SiO 2 、Al 2 O 3 , Li 2 O, ZnO and TiO 2 , the grain size of the glass ceramic product is less than 60nm.

[0014] (10) Glass ceramic products, the components of which contain SiO 2 、Al 2 O 3 , Li 2 O, ZnO and TiO 2 The ion exchange layer depth of the glass ceramic product is greater than 75 μm.

[0015] (11) Glass ceramic products containing spinel crystal phase, wherein the light transmittance of the glass ceramic products with a thickness of less than 1 mm at a wavelength of 550 nm is greater than 87.0%.

[0016] (12) Glass ceramic products, the components of which contain SiO 2 、Al 2 O 3 And ZnO, containing spinel crystal phase, the drop resistance of glass ceramic products is more than 1200mm.

[0017] (13) Glass ceramic products, the components of which contain SiO 2 、Al 2 O 3 , Li 2 O and ZnO, the Vickers hardness of the glass ceramic product is 650kgf / mm 2 above.

[0018] (14) A glass-ceramic product according to any one of (3) to (13), wherein the components thereof are expressed in weight percentage and contain: SiO 2 : 40-55%; and / or Al 2 O 3 :15~30%;and / or Li 2 O: 0.1-6%; and / or ZnO: 9-20%; and / or MgO: 0.1-6%; and / or TiO 2 :0.5~7%;and / or P 2 O 5 +ZrO 2 :0~8%;and / or Na 2 O: 0-6%; and / or B 2 O 3 :0~4%;and / or K 2 O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y 2 O 3 : 0-6%; and / or clarifier: 0-2%.

[0019] (15) Glass-ceramic products, whose components are expressed in weight percentage, are composed of SiO 2 :40~55%;Al 2 O 3 :15~30%;Li 2 O: 0.1~6%; ZnO: 9~20%; MgO: 0.1~6%; TiO 2 :0.5~7%;P 2 O 5 :0~5%;ZrO2 :0~5%;Na 2 O: 0~6%; B 2 O 3 :0~4%; K 2 O: 0~3%; CaO+BaO+SrO: 0~5%; Y 2 O 3 :0~6%;Clarifying agent:0~2%, including SiO 2 / Al 2 O 3 It is 1.5 to 3.2.

[0020] (16) A glass-ceramic product according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: SiO 2 / Al 2 O 3 1.7 to 3.0, preferably SiO 2 / Al 2 O 3 1.8 to 2.8, more preferably SiO 2 / Al 2 O 3 2.0 to 2.5; and / or Al 2 O 3 + ZnO is 26-45%, preferably Al 2 O 3 + ZnO is 30-42%, preferably Al 2 O 3 + ZnO is 32-42%, and Al is more preferred 2 O 3 + ZnO is 35-40%; and / or (TiO 2 +ZnO) / Al 2 O 3 0.4 to 1.5, preferably (TiO 2 +ZnO) / Al 2 O 3 0.5 to 1.2, more preferably (TiO 2 +ZnO) / Al 2 O 3 is 0.6 to 1.0, more preferably (TiO 2 +ZnO) / Al 2 O 3 0.6 to 0.9; and / or (Li 2 O+MgO) / TiO 2 is 0.3 to 8.0, preferably (Li 2 O+MgO) / TiO 2 is 0.5 to 5.0, more preferably (Li2 O+MgO) / TiO 2 is 1.0 to 3.0, and more preferably (Li 2 O+MgO) / TiO 2 1.2 to 2.5; and / or Al 2 O 3 / (MgO+TiO 2 ) is 1.3 to 10.0, preferably Al 2 O 3 / (MgO+TiO 2 ) is 1.5 to 8.0, and Al 2 O 3 / (MgO+TiO 2 ) is 2.5 to 6.5, and Al 2 O 3 / (MgO+TiO 2 ) is 3.0 to 5.5; and / or P 2 O 5 +ZrO 2 : 0~8%, preferably P 2 O 5 +ZrO 2 : 0.1 to 7%, more preferably P 2 O 5 +ZrO 2 :0.5~5%.

[0021] (17) A glass-ceramic product according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: Li 2 O / TiO 2 0.2 to 4.5, preferably Li 2 O / TiO 2 0.5 to 3.5, more preferably Li 2 O / TiO 2 is 0.7 to 2.5, and Li 2 O / TiO 2 0.75 to 1.5; and / or Al 2 O 3 / ZnO is 1.0 to 3.0, preferably Al 2 O 3 / ZnO is 1.2 to 2.8, and Al is more preferred 2 O 3 / ZnO is 1.25 to 2.5, and Al 2 O 3 / ZnO is 1.5 to 2.3; and / or (Al 2 O 3 +Li 2 O) / P2 O 5 5.0 to 45.0, preferably (Al 2 O 3 +Li 2 O) / P 2 O 5 7.0 to 35.0, more preferably (Al 2 O 3 +Li 2 O) / P 2 O 5 8.0 to 30.0, more preferably (Al 2 O 3 +Li 2 O) / P 2 O 5 10.0~25.0; and / or P 2 O 5 / ZrO 2 0.1~5.0, preferably P 2 O 5 / ZrO 2 0.2 to 3.0, more preferably P 2 O 5 / ZrO 2 is 0.5 to 2.0, and more preferably P 2 O 5 / ZrO 2 0.6 to 1.5; and / or (SiO 2 +Na 2 O) / ZnO is 2.2 to 6.2, preferably (SiO 2 +Na 2 O) / ZnO is 2.5 to 6.0, and more preferably (SiO 2 +Na 2 O) / ZnO is 2.8 to 5.5, and more preferably (SiO 2 +Na 2 O) / ZnO is 3.0 to 5.0; and / or (Na 2 O+K 2 O) / ZnO is less than 0.8, preferably (Na 2 O+K 2 O) / ZnO is 0.6 or less, and more preferably (Na 2 O+K 2 O) / ZnO is 0.4 or less, and more preferably (Na 2 O+K 2 O) / ZnO is less than 0.2.

[0022] (18) A glass-ceramic product according to any one of (1) to (15), wherein the components are expressed in weight percentage, wherein: SiO 2 : 45-53%, preferably SiO 2 : 48-52%; and / or Al 2 O 3 : 18-25%, preferably Al 2 O 3 :20~23%;and / or Li 2 O: 1-5%, preferably Li 2 O: 2-4%; and / or ZnO: 11-18%, preferably ZnO: 12-16%; and / or MgO: 1-5%, preferably MgO: 2-4%; and / or TiO 2 : 1-6%, preferably TiO 2 : 2-5%; and / or P 2 O 5 : 0.5~4%, preferably P 2 O 5 :1~3%; and / or ZrO 2 : 0.5-4%, preferably ZrO 2 :1~3%;and / or Na 2 O: 0-4%, preferably Na 2 O: 0-2%; and / or B 2 O 3 : 0-2%, preferably B 2 O 3 :0~1%;and / or K 2 O: 0-2%, preferably K 2 O: 0-1%; and / or CaO+BaO+SrO: 0-4%, preferably CaO+BaO+SrO: 0-2%; and / or Y 2 O 3 : 0-4%, preferably Y 2 O 3 : 0-2%; and / or clarifier: 0-1%, preferably clarifier: 0-0.5%.

[0023] (19). The glass ceramic product according to any one of (1) to (15), wherein the glass ceramic product contains a spinel crystalline phase, and preferably the spinel crystalline phase has a higher weight percentage than other crystalline phases. More preferably, the spinel crystalline phase accounts for 20 to 60% of the weight of the glass ceramic product. Further preferably, the spinel crystalline phase accounts for 25 to 50% of the weight of the glass ceramic product. Further preferably, the spinel crystalline phase accounts for 25 to 45% of the weight of the glass ceramic product. Further preferably, the spinel crystalline phase accounts for 30 to 45% of the weight of the glass ceramic product.

[0024] (20). According to any one of the glass ceramic products described in (1) to (15), the glass ceramic product contains a quartz crystal phase, preferably the weight percentage of the quartz crystal phase in the glass ceramic product is less than 20%, more preferably the weight percentage of the quartz crystal phase in the glass ceramic product is less than 10%, further preferably the weight percentage of the quartz crystal phase in the glass ceramic product is less than 5%, and further preferably the glass ceramic product does not contain a quartz crystal phase.

[0025] (21) A glass ceramic product according to any one of (1) to (15), wherein the grain size of the glass ceramic product is 60 nm or less, preferably 45 nm or less, and more preferably 10 to 30 nm; and / or the ion exchange layer depth is 75 μm or more, preferably 80 to 150 μm, and more preferably 100 to 125 μm; and / or the surface stress is 200 MPa or more, preferably 250 to 400 MPa, and more preferably 300 to 400 MPa; and / or the drop ball test height is 1000 mm or more, preferably 1200 mm or more, and more preferably 1500 mm or more; and / or the drop resistance is 1200 mm or more, preferably 1300 mm or more, and more preferably 1400 mm or more; and / or the fracture toughness is 1.0 MPa·m 1 / 2 Above, preferably 1.2 MPa·m 1 / 2 More preferably, 1.2 to 1.6 MPa·m 1 / 2 ; and / or a four-point bending strength of 500 MPa or more, preferably 600 MPa or more, more preferably 700-1000 MPa; and / or an extrusion strength of 400 N or more, preferably 400-550 N, more preferably 450-550 N; and / or a Vickers hardness of 650 kgf / mm 2 Above, preferably 660kgf / mm 2 More preferably, 680 to 750 kgf / mm 2 .

[0026] (22). According to any one of the glass ceramic products described in (1) to (15), the haze of the glass ceramic product with a thickness of less than 1 mm is less than 0.3%, preferably less than 0.25%, and more preferably 0.05-0.2%; and / or the average light transmittance at a wavelength of 400-800 nm is greater than 87.0%, preferably greater than 88.5%, and more preferably greater than 89.5%; and / or the light transmittance at a wavelength of 550 nm is greater than 87.0%, preferably greater than 88.0%, and more preferably greater than 89.0%; and / or the average light |B| value at 400-800 nm is less than 1.0, preferably less than 0.8, and more preferably 0.3-0.6.

[0027] (23). The glass-ceramic article according to (22), wherein the thickness of the glass-ceramic article is 0.2 to 1 mm, preferably 0.3 to 0.9 mm, more preferably 0.5 to 0.8 mm, and further preferably 0.55 mm or 0.6 mm or 0.68 mm or 0.7 mm or 0.75 mm.

[0028] (24). The glass-ceramic article according to any one of (1) to (14), wherein, expressed in weight percentage, the components thereof contain: NiO: 0 to 4%; and / or Ni 2 O 3 : 0 to 4%; and / or CoO: 0 to 2%; and / or Co 2 O 3 : 0 to 2%; and / or Fe 2 O 3 : 0 to 7%; and / or MnO 2 : 0 to 4%; and / or Er 2 O 3 : 0 to 8%; and / or Nd 2 O 3 : 0 to 8%; and / or Cu 2 O: 0 to 4%; and / or Pr 2 O 3 : 0 to 8%; and / or CeO 2 : 0 to 4%.

[0029] (25). The glass-ceramic article according to any one of (1) to (14), wherein, expressed in weight percentage, the components thereof contain: NiO: 0.1 to 4%; and / or Ni 2 O 3 : 0.1 to 4%; and / or CoO: 0.05 to 2%; and / or Co 2 O 3 : 0.05 to 2%; and / or Fe 2 O 3 : 0.2 to 7%; and / or MnO 2 : 0.1 to 4%; and / or Er 2 O 3 : 0.4 to 8%; and / or Nd 2 O 3 : 0.4 to 8%; and / or Cu 2 O: 0.5 to 4%; and / or Pr 2 O 3 : 0.4 to 8%; and / or CeO 2 : 0.5 to 4%.

[0030] (26). The glass-ceramic article according to any one of (1) to (14), wherein, expressed in weight percentage, the components thereof contain: NiO: 0.1 to 3%; and / or Ni2 O 3 : 0.1 - 3%; and / or CoO: 0.05 - 1.8%; and / or Co 2 O 3 : 0.05 - 1.8%; and / or Fe 2 O 3 : 0.2 - 5%; and / or MnO 2 : 0.1 - 3%; and / or Er 2 O 3 : 0.4 - 6%; and / or Nd 2 O 3 : 0.4 - 6%; and / or Cu 2 O: 0.5 - 3%; and / or Pr 2 O 3 : 0.4 - 6%; and / or CeO 2 : 0.5 - 3%.

[0031] (27). The glass - ceramic product according to any one of (1) - (14), in terms of weight percentage, contains: NiO: 0.1 - 3%; and / or Ni 2 O 3 : 0.1 - 3%.

[0032] (28). The glass - ceramic product according to any one of (1) - (14), in terms of weight percentage, contains: CoO: 0.05 - 1.8%; and / or Co 2 O 3 : 0.05 - 1.8%.

[0033] (29). The glass - ceramic product according to any one of (1) - (14), in terms of weight percentage, contains: Cu 2 O: 0.5 - 3%; and / or CeO 2 : 0.5 - 3%.

[0034] (30). The glass - ceramic product according to any one of (1) - (14), in terms of weight percentage, contains: Fe 2 O 3 : 0.2 - 5%, CoO: 0.05 - 0.3%; or Fe 2 O 3 : 0.2 - 5%, Co 2 O 3 : 0.05 - 0.3%; or Fe 2 O 3 : 0.2 - 5%, CoO: 0.05 - 0.3%, NiO: 0.1 - 1%; or Fe 2 O 3 : 0.2 - 5%, Co2 O 3 : 0.05~0.3%, NiO: 0.1~1%.

[0035] (31) A glass-ceramic product according to any one of (1) to (14), wherein the components are expressed in weight percentage and contain: Pr 2 O 3 :0.4~6%;or Fe 2 O 3 :0.2~5%; or MnO 2 :0.1~3%; or Er 2 O 3 :0.4~6%;or Nd 2 O 3 :0.4~6%.

[0036] (32) A glass-ceramic product according to any one of (1) to (14), wherein the components are expressed in weight percentage and contain: Er 2 O 3 :0.4~6%、Nd 2 O 3 :0.4~4%、MnO 2 :0.1~2%.

[0037] (33) Glass-ceramics, whose components, expressed in percentage by weight, contain: SiO 2 :40~55%;Al 2 O 3 :15~30%;Li 2 O: 0.1~6%; ZnO: 9~20%; MgO: 0.1~6%; TiO 2 :0.5~7%, of which SiO 2 / Al 2 O 3 It is 1.5 to 3.2.

[0038] (34) The glass-ceramic according to (33), wherein the components are expressed in weight percentage and further contain: P 2 O 5 :0~5%;and / or ZrO 2 :0~5%;and / or Na 2 O: 0-6%; and / or B 2 O 3 :0~4%;and / or K 2 O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y 2 O 3 : 0-6%; and / or clarifier: 0-2%.

[0039] (35) Glass ceramics, whose components contain SiO 2 、Al 2 O 3 , ZnO and TiO 2 The glass ceramic contains a spinel crystal phase, and the haze of the glass ceramic with a thickness of less than 1 mm is less than 0.3%.

[0040] (36) Glass ceramics, whose components contain SiO 2 、Al 2 O 3 , Li 2 O, ZnO and TiO 2 , the glass-ceramic contains a spinel crystal phase.

[0041] (37) Glass ceramics containing spinel crystal phase, wherein the grain size of the glass ceramics is less than 60 nm.

[0042] (38) Glass ceramics, whose components contain SiO 2 、Al 2 O 3 , Li 2 O, ZnO and TiO 2 , the Vickers hardness of glass ceramics is 550kgf / mm 2 above.

[0043] (39) Glass ceramics containing spinel crystal phases, wherein the light transmittance at a wavelength of 550 nm of the glass ceramics having a thickness of less than 1 mm is greater than 87.0%.

[0044] (40) Glass ceramics, whose components contain SiO 2 、Al 2 O 3 , Li 2 O, ZnO and TiO 2 , the Young's modulus of the glass ceramic is 80 to 110 GPa.

[0045] (41) Glass ceramics, whose components contain SiO 2 、Al 2 O 3 , Li 2 For glass ceramics with a thickness of less than 1 mm, the average optical |B| value at 400 to 800 nm is less than 1.0.

[0046] (42) Glass ceramics, whose components contain SiO 2 、Al 2 O 3 The average light transmittance of the glass ceramic with a thickness of less than 1 mm and ZnO at a wavelength of 400 to 800 nm is 87.0% or more.

[0047] (43) According to any one of (35) to (42), the glass-ceramic, wherein the components are expressed in weight percentage and contain: SiO 2 : 40-55%; and / or Al 2 O 3 :15~30%;and / or Li 2 O: 0.1-6%; and / or ZnO: 9-20%; and / or MgO: 0.1-6%; and / or TiO 2 :0.5~7%;and / or P 2 O 5 +ZrO 2 :0~8%;and / or Na 2 O: 0-6%; and / or B 2 O 3 :0~4%;and / or K 2 O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y 2 O 3 : 0-6%; and / or clarifier: 0-2%.

[0048] (44) Glass ceramics, whose components are expressed in weight percentage, are composed of SiO 2 :40~55%;Al 2 O 3 :15~30%;Li 2 O: 0.1~6%; ZnO: 9~20%; MgO: 0.1~6%; TiO 2 :0.5~7%;P 2 O 5 :0~5%;ZrO 2 :0~5%;Na 2 O: 0~6%; B 2 O 3 :0~4%; K 2 O: 0~3%; CaO+BaO+SrO: 0~5%; Y 2 O 3 :0~6%;Clarifying agent:0~2%, including SiO 2 / Al 2 O 3 It is 1.5 to 3.2.

[0049] (45) A glass-ceramic according to any one of (33) to (44), wherein the components are expressed in weight percentage, wherein: SiO 2 / Al 2 O 3 1.7 to 3.0, preferably SiO 2 / Al2 O 3 1.8 to 2.8, more preferably SiO 2 / Al 2 O 3 2.0 to 2.5; and / or Al 2 O 3 + ZnO is 26-45%, preferably Al 2 O 3 + ZnO is 30-42%, more preferably Al 2 O 3 + ZnO is 32-42%, and Al is more preferred 2 O 3 + ZnO is 35-40%; and / or (TiO 2 +ZnO) / Al 2 O 3 0.4 to 1.5, preferably (TiO 2 +ZnO) / Al 2 O 3 0.5 to 1.2, more preferably (TiO 2 +ZnO) / Al 2 O 3 is 0.6 to 1.0, more preferably (TiO 2 +ZnO) / Al 2 O 3 0.6 to 0.9; and / or (Li 2 O+MgO) / TiO 2 is 0.3 to 8.0, preferably (Li 2 O+MgO) / TiO 2 is 0.5 to 5.0, more preferably (Li 2 O+MgO) / TiO 2 is 1.0 to 3.0, and more preferably (Li 2 O+MgO) / TiO 2 1.2 to 2.5; and / or Al 2 O 3 / (MgO+TiO 2 ) is 1.3 to 10.0, preferably Al 2 O 3 / (MgO+TiO 2 ) is 1.5 to 8.0, and Al 2 O 3 / (MgO+TiO 2 ) is 2.5 to 6.5, and Al 2 O 3 / (MgO+TiO 2 ) is 3.0 to 5.5; and / or P2 O 5 +ZrO 2 : 0~8%, preferably P 2 O 5 +ZrO 2 : 0.1 to 7%, more preferably P 2 O 5 +ZrO 2 :0.5~5%.

[0050] (46) A glass-ceramic according to any one of (33) to (44), wherein the components are expressed in weight percentage, wherein: Li 2 O / TiO 2 0.2 to 4.5, preferably Li 2 O / TiO 2 0.5 to 3.5, more preferably Li 2 O / TiO 2 is 0.7 to 2.5, and Li 2 O / TiO 2 0.75 to 1.5; and / or Al 2 O 3 / ZnO is 1.0 to 3.0, preferably Al 2 O 3 / ZnO is 1.2 to 2.8, and Al is more preferred 2 O 3 / ZnO is 1.25 to 2.5, and Al 2 O 3 / ZnO is 1.5 to 2.3; and / or (Al 2 O 3 +Li 2 O) / P 2 O 5 5.0 to 45.0, preferably (Al 2 O 3 +Li 2 O) / P 2 O 5 7.0 to 35.0, more preferably (Al 2 O 3 +Li 2 O) / P 2 O 5 8.0 to 30.0, more preferably (Al 2 O 3 +Li 2 O) / P 2 O 5 10.0~25.0; and / or P 2 O 5 / ZrO 20.1~5.0, preferably P 2 O 5 / ZrO 2 0.2 to 3.0, more preferably P 2 O 5 / ZrO 2 is 0.5 to 2.0, and more preferably P 2 O 5 / ZrO 2 0.6 to 1.5; and / or (SiO 2 +Na 2 O) / ZnO is 2.2 to 6.2, preferably (SiO 2 +Na 2 O) / ZnO is 2.5 to 6.0, and more preferably (SiO 2 +Na 2 O) / ZnO is 2.8 to 5.5, and more preferably (SiO 2 +Na 2 O) / ZnO is 3.0 to 5.0; and / or (Na 2 O+K 2 O) / ZnO is less than 0.8, preferably (Na 2 O+K 2 O) / ZnO is 0.6 or less, and more preferably (Na 2 O+K 2 O) / ZnO is 0.4 or less, and more preferably (Na 2 O+K 2 O) / ZnO is less than 0.2.

[0051] (47) A glass-ceramic according to any one of (33) to (44), wherein the components are expressed in weight percentage, wherein: SiO 2 : 45-53%, preferably SiO 2 : 48-52%; and / or Al 2 O 3 : 18-25%, preferably Al 2 O 3 :20~23%;and / or Li 2 O: 1-5%, preferably Li 2 O: 2-4%; and / or ZnO: 11-18%, preferably ZnO: 12-16%; and / or MgO: 1-5%, preferably MgO: 2-4%; and / or TiO 2 : 1-6%, preferably TiO 2 : 2-5%; and / or P 2 O 5 : 0.5~4%, preferably P 2 O 5:1~3%; and / or ZrO 2 : 0.5-4%, preferably ZrO 2 :1~3%;and / or Na 2 O: 0-4%, preferably Na 2 O: 0-2%; and / or B 2 O 3 : 0-2%, preferably B 2 O 3 :0~1%;and / or K 2 O: 0-2%, preferably K 2 O: 0-1%; and / or CaO+BaO+SrO: 0-4%, preferably CaO+BaO+SrO: 0-2%; and / or Y 2 O 3 : 0-4%, preferably Y 2 O 3 : 0-2%; and / or clarifier: 0-1%, preferably clarifier: 0-0.5%.

[0052] (48). The glass-ceramic according to any one of (33) to (44), wherein the glass-ceramic contains a spinel crystalline phase, and preferably the spinel crystalline phase has a higher weight percentage than other crystalline phases. More preferably, the spinel crystalline phase accounts for 20 to 60% of the weight of the glass-ceramic. Further preferably, the spinel crystalline phase accounts for 25 to 50% of the weight of the glass-ceramic. Further preferably, the spinel crystalline phase accounts for 25 to 45% of the weight of the glass-ceramic. Even more preferably, the spinel crystalline phase accounts for 30 to 45% of the weight of the glass-ceramic.

[0053] (49). According to any one of the glass ceramics described in (33) to (44), the glass ceramic contains a quartz crystal phase, and preferably the weight percentage of the quartz crystal phase in the glass ceramic is less than 20%, more preferably the weight percentage of the quartz crystal phase in the glass ceramic is less than 10%, further preferably the weight percentage of the quartz crystal phase in the glass ceramic is less than 5%, and further preferably the glass ceramic does not contain a quartz crystal phase.

[0054] (50) According to any one of (33) to (44), the glass ceramic has a grain size of 60 nm or less, preferably 45 nm or less, and more preferably 10 to 30 nm; and / or a Young's modulus of 80 to 110 GPa, preferably 85 to 105 GPa, and more preferably 90 to 105 GPa; and / or a Vickers hardness of 550 kgf / mm 2 Above, preferably 580kgf / mm 2 More preferably, 600 to 650 kgf / mm 2 .

[0055] (51). For the glass-ceramic according to any one of (33) to (44), the haze of the glass-ceramic with a thickness of 1 mm or less is 0.3% or less, preferably 0.25% or less, more preferably 0.05 to 0.2%; and / or the average light transmittance at a wavelength of 400 to 800 nm is 87.0% or more, preferably 88.5% or more, more preferably 89.5% or more; and / or the light transmittance at a wavelength of 550 nm is 87.0% or more, preferably 88.0% or more, more preferably 89.0% or more; and / or the average light |B| value at 400 to 800 nm is 1.0 or less, preferably 0.8 or less, more preferably 0.3 to 0.6.

[0056] (52). For the glass-ceramic according to (51), the thickness of the glass-ceramic is 0.2 to 1 mm, preferably 0.3 to 0.9 mm, more preferably 0.5 to 0.8 mm, and further preferably 0.55 mm or 0.6 mm or 0.68 mm or 0.7 mm or 0.75 mm.

[0057] (53). For the glass-ceramic according to any one of (33) to (43), its components are expressed by weight percentage and contain: NiO: 0 to 4%; and / or Ni 2 O 3 : 0 to 4%; and / or CoO: 0 to 2%; and / or Co 2 O 3 : 0 to 2%; and / or Fe 2 O 3 : 0 to 7%; and / or MnO 2 : 0 to 4%; and / or Er 2 O 3 : 0 to 8%; and / or Nd 2 O 3 : 0 to 8%; and / or Cu 2 O: 0 to 4%; and / or Pr 2 O 3 : 0 to 8%; and / or CeO 2 : 0 to 4%.

[0058] (54). For the glass-ceramic according to any one of (33) to (43), its components are expressed by weight percentage and contain: NiO: 0.1 to 4%; and / or Ni 2 O 3 : 0.1 to 4%; and / or CoO: 0.05 to 2%; and / or Co 2 O 3 : 0.05 to 2%; and / or Fe 2 O 3 : 0.2 to 7%; and / or MnO 2 : 0.1 to 4%; and / or Er 2O 3 : 0.4 - 8%; and / or Nd 2 O 3 : 0.4 - 8%; and / or Cu 2 O: 0.5 - 4%; and / or Pr 2 O 3 : 0.4 - 8%; and / or CeO 2 : 0.5 - 4%.

[0059] (55). The glass - ceramic according to any one of (33) - (43), its components are expressed by weight percentage and contain: NiO: 0.1 - 3%; and / or Ni 2 O 3 : 0.1 - 3%; and / or CoO: 0.05 - 1.8%; and / or Co 2 O 3 : 0.05 - 1.8%; and / or Fe 2 O 3 : 0.2 - 5%; and / or MnO 2 : 0.1 - 3%; and / or Er 2 O 3 : 0.4 - 6%; and / or Nd 2 O 3 : 0.4 - 6%; and / or Cu 2 O: 0.5 - 3%; and / or Pr 2 O 3 : 0.4 - 6%; and / or CeO 2 : 0.5 - 3%.

[0060] (56). The glass - ceramic according to any one of (33) - (43), its components are expressed by weight percentage and contain: NiO: 0.1 - 3%; and / or Ni 2 O 3 : 0.1 - 3%.

[0061] (57). The glass - ceramic according to any one of (33) - (43), its components are expressed by weight percentage and contain: CoO: 0.05 - 1.8%; and / or Co 2 O 3 : 0.05 - 1.8%.

[0062] (58). The glass - ceramic according to any one of (33) - (43), its components are expressed by weight percentage and contain: Cu 2 O: 0.5 - 3%; and / or CeO 2 : 0.5 - 3%.

[0063] (59) A glass-ceramic according to any one of (33) to (43), wherein the composition, expressed in weight percentage, comprises: Fe 2 O 3 :0.2~5%、CoO:0.05~0.3%;or Fe 2 O 3 :0.2~5%、Co 2 O 3 :0.05~0.3%;or Fe 2 O 3 :0.2~5%、CoO:0.05~0.3%、NiO:0.1~1%;or Fe 2 O 3 :0.2~5%、Co 2 O 3 : 0.05~0.3%, NiO: 0.1~1%.

[0064] (60) A glass-ceramic according to any one of (33) to (43), wherein the components are expressed in weight percentage and contain: Pr 2 O 3 :0.4~6%;or Fe 2 O 3 :0.2~5%; or MnO 2 :0.1~3%; or Er 2 O 3 :0.4~6%;or Nd 2 O 3 :0.4~6%.

[0065] (61) According to any one of (33) to (43) described glass ceramics, its components expressed in weight percentage, containing: Er 2 O 3 :0.4~6%、Nd 2 O 3 :0.4~4%、MnO 2 :0.1~2%.

[0066] (62) A glass ceramic formed body comprising the glass ceramic described in any one of (33) to (61).

[0067] (63) A glass cover plate comprising the glass ceramic product described in any one of (1) to (32), and / or the glass ceramic described in any one of (33) to (61), and / or the glass ceramic formed body described in (62).

[0068] (64) A glass component comprising a glass ceramic product as described in any one of (1) to (32), and / or a glass ceramic as described in any one of (33) to (61), and / or a glass ceramic formed body as described in (62).

[0069] (65) An electronic device comprising a glass ceramic product as described in any one of (1) to (32), and / or a glass ceramic as described in any one of (33) to (61), and / or a glass ceramic formed body as described in (62), and / or a glass cover as described in (63), and / or a glass component as described in (64).

[0070] (66) A display device comprising a glass ceramic product as described in any one of (1) to (32), and / or a glass ceramic as described in any one of (33) to (61), and / or a glass ceramic formed body as described in (62), and / or a glass cover as described in (63), and / or a glass component as described in (64).

[0071] (67). A method for manufacturing a glass ceramic product as described in any one of (1) to (32), the method comprising the following steps: forming a matrix glass, forming a glass ceramic by a crystallization process of the matrix glass, and then forming a glass ceramic product by a chemical strengthening process of the glass ceramic.

[0072] (68). According to the manufacturing method of glass ceramic products described in (67), the formation of matrix glass includes the following steps: mixing the raw materials evenly according to the component ratio, then putting them into a crucible, melting them in an electric furnace or a gas furnace at a temperature range of 1350 to 1550°C for 5 to 24 hours, preferably the melting temperature is 1450 to 1550°C, and then clarifying, homogenizing, molding, and annealing to obtain the matrix glass, the clarification temperature is greater than 1550°C but less than or equal to 1650°C, and the annealing temperature is 450 to 600°C.

[0073] (69). According to the manufacturing method of glass ceramic products described in (67), the crystallization process includes the following steps: heating to a specified crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down, the crystallization treatment temperature is 600-800°C, preferably 650-750°C, and the holding time at the crystallization treatment temperature is 1-10 hours, preferably 3-6 hours.

[0074] (70) According to the method for manufacturing a glass ceramic product described in (67), the crystallization process includes the following steps: performing a nucleation process at a first temperature and then performing a crystal growth process at a second temperature.

[0075] (71). According to the manufacturing method of the glass ceramic product described in (70), the crystallization process includes: the first temperature is 600-700°C, the second temperature is greater than 700°C but less than or equal to 800°C, the holding time at the first temperature is 1 to 6 hours, and the holding time at the second temperature is 2 to 5 hours.

[0076] (72). According to the manufacturing method of glass ceramic products described in (67), the chemical strengthening process includes: immersing the glass ceramic in a salt bath of molten Na salt at 350-470°C for 1-36 hours, preferably in the temperature range of 400-460°C, and preferably in the time range of 2-15 hours; and / or immersing the glass ceramic in a mixed salt bath of molten K salt and Na salt at 360-450°C for 1-36 hours, preferably in the time range of 2-24 hours.

[0077] (73). A method for manufacturing a glass ceramic as described in any one of (33) to (61), the method comprising the following steps: forming a matrix glass, and then forming the matrix glass into a glass ceramic through a crystallization process.

[0078] (74). According to the manufacturing method of glass ceramics described in (73), the formation of matrix glass includes the following steps: mixing the raw materials evenly according to the component ratio, then putting them into a crucible, melting them in an electric furnace or a gas furnace at a temperature range of 1350 to 1550°C for 5 to 24 hours, preferably the melting temperature is 1450 to 1550°C, and then clarifying, homogenizing, molding, and annealing to obtain the matrix glass, the clarification temperature is greater than 1550°C but less than or equal to 1650°C, and the annealing temperature is 450 to 600°C.

[0079] (75). According to the manufacturing method of glass ceramics described in (73), the crystallization process includes the following steps: heating to a specified crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down. The crystallization treatment temperature is 600-800°C, preferably 650-750°C, and the holding time at the crystallization treatment temperature is 1-10 hours, preferably 3-6 hours.

[0080] (76) According to the method for manufacturing glass ceramics described in (73), the crystallization process includes the following steps: performing a nucleation process at a first temperature and then performing a crystal growth process at a second temperature.

[0081] (77). According to the manufacturing method of glass ceramics described in (76), the crystallization process includes: the first temperature is 600-700°C, the second temperature is greater than 700°C but less than or equal to 800°C, the holding time at the first temperature is 1 to 6 hours, and the holding time at the second temperature is 2 to 5 hours.

[0082] (78) A method for manufacturing a glass ceramic formed body as described in (62), the method comprising grinding or polishing the glass ceramic to form a glass ceramic formed body, or subjecting the matrix glass or glass ceramic to a heat bending process or a press molding process at a certain temperature to form a glass ceramic formed body.

[0083] (79). According to the method for manufacturing a glass ceramic formed body described in (78), the method includes the following steps: subjecting the matrix glass to a crystallization heat treatment process, including heating, heat preservation for nucleation, heating, heat preservation for crystallization, and cooling to room temperature to form pre-crystallized glass; and subjecting the pre-crystallized glass to heat processing and molding to obtain a glass ceramic formed body.

[0084] (80) A method for manufacturing a glass ceramic formed body according to (78), the method comprising the following steps:

[0085] 1) Heating and preheating: Place the matrix glass or pre-crystallized glass or glass ceramic in the mold. The mold passes through each heating station in the hot bending machine in turn and stays at each station for a certain period of time to keep warm. The temperature in the preheating zone is 400-800°C, the pressure is 0.01-0.05MPa, and the time is 40-200s;

[0086] 2) Pressurized molding: After preheating, the mold is transferred to the molding station. The hot bending machine applies a certain pressure to the mold. The pressure range is 0.1-0.8Mpa. The temperature range of the molding station is 600-850℃, and the molding time range is 40-200s.

[0087] 3) Maintaining pressure and cooling: The mold is transferred to the cooling station for cooling step by step. The cooling temperature range is 750-500°C, the pressure is 0.01-0.05Mpa, and the time is 40-200s.

[0088] The beneficial effects of the present invention are: through reasonable component design, the glass ceramics obtained by the present invention have excellent mechanical properties and are suitable for chemical strengthening, and the glass ceramic products obtained by the present invention have excellent mechanical properties and meet the application in the fields of display devices or electronic devices. DETAILED DESCRIPTION

[0089] The glass ceramics and glass ceramic products of the present invention are materials having a crystalline phase (sometimes also referred to as crystals) and a glass phase. The crystalline phase of the glass ceramics and glass ceramic products can be identified by the peak angles appearing in the X-ray diffraction pattern of X-ray diffraction analysis and / or measured by TEMEDX.

[0090] After repeated experiments and studies, the inventors of the present invention obtained the glass ceramics or glass ceramic products of the present invention by regulating the content and content ratio of specific components constituting glass ceramics and glass ceramic products to specific values ​​and making them contain specific crystal phases.

[0091] Below, the scope of each component (ingredient) of the matrix glass, glass ceramic and glass ceramic product of the present invention is described. In this specification, if there is no special explanation, the content of each component is all expressed by weight percentage (wt%) relative to the total amount of matrix glass, glass ceramic or glass ceramic product material converted into oxide composition. Here, the "composition converted into oxide" refers to the case where the oxide, composite salt and hydroxide used as the raw material of the matrix glass, glass ceramic or glass ceramic product of the present invention decompose and transform into oxide when melted, and the total amount of the oxide material is taken as 100%. In addition, in this specification, when it is only referred to as glass, it is the matrix glass before crystallization (i.e. crystallization process treatment), the matrix glass is called glass ceramic after crystallization (i.e. crystallization process treatment), and the glass ceramic product refers to the product obtained after the glass ceramic is chemically strengthened.

[0092] Unless otherwise indicated in specific cases, the numerical ranges listed herein include upper and lower limits, and "above" and "below" include the endpoints, as well as all integers and fractions within the range, without limitation to the specific values ​​listed when defining the range. The term "about" as used herein means that the formula, parameters and other quantities and features are not and need not be exact, and may be approximate and / or larger or lower if necessary, reflecting tolerances, conversion factors and measurement errors, etc. "And / or" as used herein is inclusive, for example, "A; and / or B" means only A, or only B, or both A and B.

[0093] In some embodiments of the present invention, the crystalline phase in the glass ceramic or glass ceramic product contains a spinel crystalline phase. Preferably, the spinel crystalline phase includes a zinc aluminum spinel crystalline phase (ZnAl 2 O 4). In some embodiments, the spinel crystalline phase has a higher weight percentage than other crystalline phases. In some embodiments, the spinel crystalline phase accounts for 20-60% by weight of the glass ceramic or glass ceramic product, preferably the spinel crystalline phase accounts for 25-50% by weight of the glass ceramic or glass ceramic product, more preferably the spinel crystalline phase accounts for 25-45% by weight of the glass ceramic or glass ceramic product, and further preferably the spinel crystalline phase accounts for 30-45% by weight of the glass ceramic or glass ceramic product. In some embodiments, the spinel crystalline phase accounts for 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60% by weight of the glass-ceramic or glass-ceramic article.

[0094] In some embodiments of the present invention, the crystalline phase in the glass ceramic or glass ceramic product contains a quartz crystalline phase (including quartz and quartz solid solution), preferably, the quartz crystalline phase includes a β-quartz solid solution. In some embodiments, the quartz crystalline phase accounts for less than 20% by weight of the glass ceramic or glass ceramic product, preferably the quartz crystalline phase accounts for less than 10% by weight of the glass ceramic or glass ceramic product, more preferably the quartz crystalline phase accounts for less than 5% by weight of the glass ceramic or glass ceramic product, and further preferably the glass ceramic or glass ceramic product does not contain a quartz crystalline phase. In some embodiments, the quartz crystalline phase accounts for 0%, greater than 0%, 0.1%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, or 20% of the weight of the glass-ceramic or glass-ceramic article.

[0095] SiO 2 It is a network former of the glass ceramic and glass ceramic products of the present invention, SiO 2 The structural components of silicon-oxygen tetrahedrons can be used to form a network structure to form the basic structure of silicates. In some embodiments, SiO 2 It is also a necessary component for the formation of quartz crystal phase. 2If the content is too low, the chemical stability of glass ceramics and glass ceramic products will deteriorate; if SiO 2 If the content is too high, the viscosity of the glass will be greatly increased, the melting temperature will be increased, the material will be difficult to smelt, and the difficulty of forming the matrix glass will be increased. 2 The content of SiO2 is 40-55%, preferably 45-53%, and more preferably 48-52%. In some embodiments, the SiO2 may include about 40%, 40.5%, 41%, 41.5%, 42%, 42.5%, 43%, 43.5%, 44%, 44.5%, 45%, 45.5%, 46%, 46.5%, 47%, 47.5%, 48%, 48.5%, 49%, 49.5%, 50%, 50.5%, 51%, 51.5%, 52%, 52.5%, 53%, 53.5%, 54%, 54.5%, 55%. 2 .

[0096] Al 2 O 3 It is beneficial to improve the mechanical properties and chemical stability of the glass ceramics and glass ceramic products of the present invention, and is also an essential component for forming the spinel crystal phase of the present invention. 2 O 3 Can form [AlO 4 ]tetrahedron, substituted part of [SiO 4 ]tetrahedrons form a network structure. [AlO 4 The volume of a tetrahedron molecule is 41 cm 3 / mol, [SiO 4 The molecular volume of a tetrahedron is 27.2 cm 3 / mol, [AlO 4 ]tetrahedral substitution part [SiO 4 ] After the tetrahedron is formed, the molecular volume increases and the structural network space expands, which is conducive to the diffusion of alkali metal ions during chemical strengthening and is also conducive to the acceptance of a large amount of Na + , promoting ion exchange. Al 2 O 3 Too low a content is not conducive to the improvement of the strengthening effect and the precipitation of crystals, and the mechanical properties and chemical stability of the glass are poor. 2 O 3 If the content is too high, the glass will be difficult to melt, the melting temperature will be high, and stones will easily precipitate on the surface during molding. 2 O 3The content of Al is 15-30%, preferably 18-25%, and more preferably 20-23%. In some embodiments, the Al content may be about 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20%, 20.5%, 21%, 21.5%, 22%, 22.5%, 23%, 23.5%, 24%, 24.5%, 25%, 25.5%, 26%, 26.5%, 27%, 27.5%, 28%, 28.5%, 29%, 29.5%, 30%. 2 O 3 .

[0097] In some embodiments, SiO 2 The content of Al 2 O 3 The ratio between the content of SiO 2 / Al 2 O 3 Controlling the SiO2 content in the range of 1.5 to 3.2 is beneficial to improving the drop ball test height and four-point bending strength of glass ceramics and glass ceramic products, and improving the ion exchange layer depth and surface stress of glass ceramic products. 2 / Al 2 O 3 1.5 to 3.2, more preferably SiO 2 / Al 2 O 3 is 1.7 to 3.0, and SiO is more preferred 2 / Al 2 O 3 is 1.8 to 2.8, and SiO is more preferred 2 / Al 2 O 3 In some embodiments, SiO 2 / Al 2 O 3 The values ​​are 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2.0, 2.05, 2.1, 2.15, 2.2, 2.25, 2.3, 2.35, 2.4, 2.45, 2.5, 2.55, 2.6, 2.65, 2.7, 2.75, 2.8, 2.85, 2.9, 2.95, 3.0, 3.05, 3.1, 3.15, 3.2.

[0098] Li 2 O can lower the melting point of glass and is also a necessary component for chemical strengthening and improving the mechanical properties of glass-ceramic products. 2 O can provide free oxygen and reduce TiO2 Coloring. 2 If the O content is too high, the crystals in the glass ceramics and glass ceramic products will grow easily, and the crystal growth will be unstable, which will affect the transmittance of the glass ceramics and glass ceramic products and make the chemical stability worse. 2 The content of O is 0.1-6%, preferably 1-5%, and more preferably 2-4%. In some embodiments, about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6% Li 2 O.

[0099] ZnO is an essential component for forming the spinel phase in the present invention, which can be controlled by 2 O 3 The content of ZnO is regulated by adjusting the spinel crystal phase content, taking into account the transmittance under the premise of ensuring mechanical strength. If the ZnO content is low, the crystal phase content in glass ceramics and glass ceramic products is low, and the mechanical properties such as Vickers hardness and Young's modulus are poor. If the ZnO content is too high, the residual Zn in the glass phase 2+ It hinders ion exchange during chemical strengthening and is not conducive to obtaining high-performance glass-ceramic products. Therefore, the content of ZnO is 9-20%, preferably 11-18%, and more preferably 12-16%. In some embodiments, about 9%, 9.5%, 10%, 10.5%, 11%, 11.5%, 12%, 12.5%, 13%, 13.5%, 14%, 14.5%, 15%, 15.5%, 16%, 16.5%, 17%, 17.5%, 18%, 18.5%, 19%, 19.5%, 20% ZnO may be included.

[0100] In some embodiments, controlling Al 2 O 3 The total content of Al and ZnO 2 O 3 + ZnO in the range of 26-45% is conducive to the glass ceramics and glass ceramic products to obtain the desired content of spinel crystal phase, while improving the drop resistance and drop ball test height of the glass ceramics and glass ceramic products, while preventing the surface stress of the glass ceramic products from deteriorating. Therefore, Al 2 O 3 + ZnO is 26-45%, preferably Al 2 O 3 + ZnO is 30-42%, and Al is more preferred 2 O 3 + ZnO is 32-42%, and Al is more preferred 2 O 3+ ZnO is 35-40%. In some embodiments, Al 2 O 3 +ZnO is 26%, 26.5%, 27%, 27.5%, 28%, 28.5%, 29%, 29.5%, 30%, 30.5%, 31%, 31.5%, 32%, 32.5%, 33%, 33.5%, 34%, 34.5%, 35%, 35.5%, 36%, 36.5%, 37%, 37.5%, 38%, 38.5%, 39%, 39.5%, 40%, 40.5%, 41%, 41.5%, 42%, 42.5%, 43%, 43.5%, 44%, 44.5%, 45%.

[0101] In some embodiments, controlling Al 2 O 3 The ratio of Al content to ZnO content 2 O 3 / ZnO in the range of 1.0 to 3.0 is beneficial to improve the hardness of glass ceramics and glass ceramic products, optimize Young's modulus, and prevent the transmittance of glass ceramics and glass ceramic products from decreasing and the haze from deteriorating. 2 O 3 / ZnO is 1.0 to 3.0, and Al is more preferred 2 O 3 / ZnO is 1.2 to 2.8, and Al 2 O 3 / ZnO is 1.25 to 2.5, and Al is more preferably 2 O 3 / ZnO is 1.5 to 2.3. In some embodiments, Al 2 O 3 / ZnO is 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1.65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2.0, 2.05, 2.1, 2.15, 2.2, 2.25, 2.3, 2.35, 2.4, 2.45, 2.5, 2.55, 2.6, 2.65, 2.7, 2.75, 2.8, 2.85, 2.9, 2.95, 3.0.

[0102] TiO 2 It is a nucleating agent for the glass ceramics and glass ceramic products of the present invention. If TiO 2 Too high a content will cause serious coloring (brown-yellow) of glass ceramics and glass ceramic products, reduce the transmittance of glass ceramics and glass ceramic products in the visible light region, and increase the haze and |B| value. 2If the content is too high, the glass will easily become milky during molding and crystallization, making the glass opaque. 2 The content of TiO is 0.5-7%, preferably 1-6%, and more preferably 2-5%. In some embodiments, the TiO may contain about 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, 5%, 5.5%, 6%, 6.5%, 7%. 2 .

[0103] In some embodiments, controlling Li 2 O content and TiO 2 The ratio between the content of Li 2 O / TiO 2 In the range of 0.2 to 4.5, Ti in glass ceramics and glass ceramic products can be effectively reduced. 3+ The coloring of ions improves the transmittance of glass ceramics and glass ceramic products, and optimizes the haze and |B| value of glass ceramics and glass ceramic products. Therefore, Li 2 O / TiO 2 0.2 to 4.5, more preferably Li 2 O / TiO 2 is 0.5 to 3.5, and Li is more preferably 2 O / TiO 2 is 0.7 to 2.5, and Li is more preferred 2 O / TiO 2 In some embodiments, Li 2 O / TiO 2 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5, 1.55, 1.6, 1. 65, 1.7, 1.75, 1.8, 1.85, 1.9, 1.95, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5.

[0104] In some embodiments, controlling TiO 2 Total content of TiO and ZnO 2 +ZnO and Al 2 O 3 The ratio between the contents of TiO2 +ZnO) / Al 2 O 3 In the range of 0.4 to 1.5, the chemical strengthening performance of glass ceramics can be optimized, the ion exchange layer depth of glass ceramic products can be increased, and the fracture toughness, four-point bending strength and drop ball test height can be improved. 2 +ZnO) / Al 2 O 3 0.4 to 1.5, more preferably (TiO 2 +ZnO) / Al 2 O 3 is 0.5 to 1.2, and more preferably (TiO 2 +ZnO) / Al 2 O 3 is 0.6 to 1.0, and more preferably (TiO 2 +ZnO) / Al 2 O 3 In some embodiments, (TiO 2 +ZnO) / Al 2 O 3 It is 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1.0, 1.05, 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4, 1.45, 1.5.

[0105] ZrO 2 It can be used as a nucleating agent for glass ceramics and glass ceramic products. 2 Using them together can make the glass ceramic crystal nuclei as large as possible. More crystal nuclei are conducive to stable crystal growth and uniform grain size. 2 If the content is too high, the melting of glass will be more difficult. 2The content is 0-5%, preferably 0.5-4%, and more preferably 1-3%. In some embodiments, it may contain about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2% , 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5% ZrO 2 .

[0106] ZrO 2 The solubility is low in the glass system of the present invention. In some embodiments, by containing a certain amount of P 2 O 5 , which can increase the ZrO 2 Solubility in glass; however, if it contains too much P 2 O 5 , the glass is easily separated into phases during forming, resulting in reduced chemical stability of glass ceramics and glass ceramic products. 2 O 5 The content is 0-5%, preferably 0.5-4%, and more preferably 1-3%. In some embodiments, it may contain about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 3.1%, 3.2%, 3. %, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5% of P 2 O 5 .

[0107] In some embodiments, Al 2 O 3 and Li 2 Total content of OAl 2 O 3+Li 2 O and P 2 O 5 The ratio between the contents of Al 2 O 3 +Li 2 O) / P 2 O 5 Controlling the ratio within the range of 5.0 to 45.0 is beneficial to improving the four-point bending strength and drop resistance of glass ceramics and glass ceramic products, and improving the surface stress of glass ceramic products. 2 O 3 +Li 2 O) / P 2 O 5 5.0 to 45.0, more preferably (Al 2 O 3 +Li 2 O) / P 2 O 5 7.0 to 35.0, more preferably (Al 2 O 3 +Li 2 O) / P 2 O 5 8.0 to 30.0, more preferably (Al 2 O 3 +Li 2 O) / P 2 O 5 In some embodiments, (Al 2 O 3 +Li 2 O) / P 2 O 5 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10.0, 10.5, 11.0, 11.5, 12.0, 12.5, 13.0, 13.5, 14.0, 14.5, 15.0, 15.5, 16.0, 16.5, 17.0, 17.5, 18.0, 18.5, 19.0, 19.5, 20.0, 20 .5, 21.0, 21.5, 22.0, 22.5, 23.0, 23.5, 24.0, 24.5, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, 40.0, 41.0, 42.0, 43.0, 44.0, 45.0.

[0108] In some embodiments, controlling P 2 O 5and ZrO 2 Total content P 2 O 5 +ZrO 2 In the range of 0 to 8%, it is beneficial for glass ceramics and glass ceramic products to obtain uniform grains and smaller grain sizes, and optimize the transmittance of glass ceramics and glass ceramic products. 2 O 5 +ZrO 2 0 to 8%, more preferably P 2 O 5 +ZrO 2 0.1 to 7%, more preferably P 2 O 5 +ZrO 2 In some embodiments, P 2 O 5 +ZrO 2 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5. 8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6%, 6.1%, 6.2%, 6.3%, 6.4%, 6.5%, 6.6%, 6.7%, 6.8%, 6.9%, 7%, 7.1%, 7.2%, 7.3%, 7.4%, 7.5%, 7.6%, 7.7%, 7.8%, 7.9%, 8%.

[0109] In some embodiments, controlling P 2 O 5 The content of ZrO 2 The ratio between the contents of 2 O 5 / ZrO 2 In the range of 0.1 to 5.0, it is beneficial to improve the hardness and fracture toughness of glass ceramics and glass ceramic products, and prevent the drop resistance and Young's modulus from deteriorating. 2 O 5 / ZrO 20.1 to 5.0, more preferably P 2 O 5 / ZrO 2 is 0.2 to 3.0, and more preferably P 2 O 5 / ZrO 2 is 0.5 to 2.0, and more preferably P 2 O 5 / ZrO 2 In some embodiments, P 2 O 5 / ZrO 2 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0.

[0110] MgO helps to reduce the viscosity of the glass, inhibits glass crystallization during molding and refines the grains during crystallization, and also has the effect of improving low-temperature solubility. In some embodiments, MgO has the effect of promoting the formation of quartz solid solution crystalline phase. If the MgO content is too high, a quartz solid solution crystalline phase is easily generated during glass crystallization, and the quartz solid solution crystalline phase has larger grains, which will reduce the transmittance of glass ceramics and glass ceramic products. Therefore, the content of MgO is 0.1-6%, preferably 1-5%, and more preferably 2-4%. In some embodiments, the present invention may comprise about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9 %, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6% MgO.

[0111] In some embodiments, controlling Li 2 Total content of O and MgO Li2 O+MgO and TiO 2 The ratio between the contents of 2 O+MgO) / TiO 2 In the range of 0.3 to 8.0, the grains can be refined, the transmittance and drop resistance of glass ceramics and glass ceramic products can be improved, and the haze and |B| value of glass ceramics and glass ceramic products can be optimized. Therefore, it is preferred that (Li 2 O+MgO) / TiO 2 is 0.3 to 8.0, more preferably (Li 2 O+MgO) / TiO 2 is 0.5 to 5.0, and more preferably (Li 2 O+MgO) / TiO 2 is 1.0 to 3.0, and more preferably (Li 2 O+MgO) / TiO 2 is 1.2 to 2.5. In some embodiments, (Li 2 O+MgO) / TiO 2 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1 , 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0.

[0112] In some embodiments, Al 2 O 3 The content of MgO and TiO 2 Total content of MgO+TiO 2 The ratio between 2 O 3 / (MgO+TiO 2 ) is controlled within the range of 1.3 to 10.0, which is beneficial to improving the hardness and drop ball test height of glass ceramics and glass ceramic products, and optimizing the surface stress and haze of glass ceramic products. 2 O 3 / (MgO+TiO 2) is 1.3 to 10.0, and Al 2 O 3 / (MgO+TiO 2 ) is 1.5 to 8.0, and Al 2 O 3 / (MgO+TiO 2 ) is 2.5 to 6.5, and Al 2 O 3 / (MgO+TiO 2 ) is 3.0 to 5.5. In some embodiments, Al 2 O 3 / (MgO+TiO 2 ) is 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6 , 5.7, 5.8, 5.9, 6.0, 6.1, 6.2, 6.3, 6.4, 6.5, 6.6, 6.7, 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, 9.0, 9.1, 9.2, 9.3, 9.4, 9.5, 9.6, 9.7, 9.8, 9.9, 10.0.

[0113] B 2 O 3 It helps the melting of glass and improves the melting effect of glass. 2 O 3 If the content is too high, the chemical stability of the glass will deteriorate, and boron anomaly will occur easily, the boron-oxygen tetrahedron will transform into a boron-oxygen triangular structure, and the viscosity of the glass will decrease. In addition, boron volatilization will easily form stripes, causing the glass to be uneven. Therefore, B 2 O 3The content of B is 0-4%, preferably 0-2%, and more preferably 0-1%. In some embodiments, the B composition may include about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4% B 2 O 3 .

[0114] Na 2 O can promote glass melting and improve the chemical strengthening properties of glass ceramics. 2 O, which easily leads to more glass break bonds, reduces the strength of the matrix glass, and affects the strength of glass ceramics and glass ceramic products. 2 The upper limit of O content is 6%, preferably 4%, and more preferably 2%. In some embodiments, about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5.1%, 5.2%, 5.3%, 5.4%, 5.6%, 5.7%, 5.8%, 5.9%, 6. 7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4. 4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6% Na 2 O.

[0115] In some embodiments, SiO 2 and Na 2 Total content of OSiO 2 +Na 2 The ratio of O to ZnO content (SiO 2 +Na 2O) / ZnO is controlled within the range of 2.2 to 6.2, which can improve the fracture toughness and compressive strength of glass ceramics and glass ceramic products while optimizing the |B| value. 2 +Na 2 O) / ZnO is 2.2 to 6.2, and more preferably (SiO 2 +Na 2 O) / ZnO is 2.5 to 6.0, and more preferably (SiO 2 +Na 2 O) / ZnO is 2.8 to 5.5, and more preferably (SiO 2 +Na 2 O) / ZnO is 3.0 to 5.0. In some embodiments, (SiO 2 +Na 2 O) / ZnO is 2.2, 2.3, 2.4, 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4. 1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6.0, 6.1, 6.2.

[0116] K 2 O helps to lower the glass melting temperature, is beneficial to chemical strengthening, and can increase the depth of the ion exchange layer of glass ceramic products; but if it contains too much K 2 O, it is easy to reduce the chemical stability of the glass and the hardness. 2 The content of O is 3% or less, preferably 2% or less, and more preferably 1% or less. In some embodiments, the K content may include about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3% K 2 O.

[0117] In some embodiments, Na 2 O and K 2 Total content of ONa 2 O+K 2 The ratio of O to ZnO content (Na 2 O+K 2O) / ZnO is controlled below 0.8, which can refine the grains, reduce the grain size of glass ceramics and glass ceramic products, improve the transmittance and compressive strength of glass ceramics and glass ceramic products, and optimize the haze of glass ceramics and glass ceramic products. 2 O+K 2 O) / ZnO is 0.8 or less, and more preferably (Na 2 O+K 2 O) / ZnO is 0.6 or less, and more preferably (Na 2 O+K 2 O) / ZnO is 0.4 or less, and more preferably (Na 2 O+K 2 O) / ZnO is less than 0.2. In some embodiments, (Na 2 O+K 2 O) / ZnO is 0, greater than 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, and 0.8.

[0118] CaO, BaO and SrO as co-solvents do not participate in the formation of the crystal phase, but remain in the residual glass phase of the glass ceramic, which is beneficial to reduce the melting temperature and processing temperature. However, too high a content will damage the nucleation and crystallization in the process of transforming the matrix glass into glass ceramics, and have an adverse effect on the chemical stability of the glass ceramics. Therefore, the total content of CaO, BaO and SrO CaO+BaO+SrO is 0-5%, preferably 0-4%, and more preferably 0-2%. In some embodiments, CaO+BaO+SrO is 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1 %, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%.

[0119] Y 2 O 3 Can promote ZrO 2The melting of Y reduces the difficulty of glass melting. Too much Y will make it difficult to form crystals during glass crystallization, and the drop ball test height of glass ceramics and glass ceramic products will decrease. 2 O 3 The upper limit of the content is 6%, preferably 4%, and more preferably 2%. In some embodiments, the content may include about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.1%, 4.2%, 4.3%, 4.4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5. 7%, 2.8%, 2.9%, 3%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4%, 4.1%, 4.2%, 4.3%, 4 .4%, 4.5%, 4.6%, 4.7%, 4.8%, 4.9%, 5%, 5.1%, 5.2%, 5.3%, 5.4%, 5.5%, 5.6%, 5.7%, 5.8%, 5.9%, 6% Y 2 O 3 .

[0120] In some embodiments, the glass, glass ceramic or glass ceramic product may also contain 0-2% of a clarifier to improve the defoaming ability of the glass, glass ceramic or glass ceramic product. Such clarifiers include but are not limited to Sb 2 O 3 SnO 2 , SnO, CeO 2 , one or more of F (fluorine) compounds, Cl (chlorine) compounds and Br (bromine) compounds, preferably Sb 2 O 3 As a clarifier. When the above clarifiers are present alone or in combination, the upper limit of the content is preferably 2%, more preferably 1%, and further preferably 0.5%. In some embodiments, the content of one or more of the clarifiers is about 0%, greater than 0%, 0.01%, 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2%.

[0121] Without affecting the properties of the glass, glass ceramic or glass ceramic product of the present invention, other components not mentioned above, such as La 2 O 3 , Gd 2O 3 , Yb 2 O 3 , Nb 2 O 5 , WO 3 、Bi 2 O 3 、 2 O 5 、TeO 2 However, in order to maintain the excellent properties of the glass, glass ceramic or glass ceramic product of the present invention, La 2 O 3 , Gd 2 O 3 , Yb 2 O 3 , Nb 2 O 5 , WO 3 、Bi 2 O 3 、 2 O 5 、TeO 2 The individual or total content of is 5% or less, more preferably 2% or less, further preferably 1% or less, and further preferably no content is contained.

[0122] PbO and As 2 O 3 As toxic substances, even a small amount of them does not meet the requirements of environmental protection. Therefore, in some embodiments of the present invention, it is preferred that PbO and / or As are not contained. 2 O 3 .

[0123] In some embodiments of the present invention, a colored matrix glass, glass ceramic or glass ceramic product can be prepared by containing a colorant, so that the matrix glass, glass ceramic or glass ceramic product can present different colors, and the colorant contains: NiO: 0-4%; and / or Ni 2 O 3 : 0-4%; and / or CoO: 0-2%; and / or Co 2 O 3 :0~2%;and / or Fe 2 O 3 :0~7%;and / or MnO 2 :0~4%;and / or Er 2 O 3 :0~8%;and / or Nd 2 O 3 :0~8%;and / or Cu 2 O: 0-4%; and / or Pr 2 O 5:0~8%;and / or CeO 2 :0~4%. The weight percentage content of the colorant and its function are described as follows:

[0124] The brown or green matrix glass, glass ceramic or glass ceramic product prepared by the present invention uses NiO, Ni 2 O 3 or Pr 2 O 5 As colorants. NiO and Ni 2 O 3 It is a colorant used to prepare brown or green matrix glass, glass ceramics or glass ceramic products. The two components can be used alone or in combination. Their respective contents are generally less than 4%, preferably less than 3%. If the content exceeds 4%, the colorant cannot be well dissolved in the matrix glass, glass ceramics or glass ceramic products. The lower limit of their respective contents is above 0.1%. If it is less than 0.1%, the color of the matrix glass, glass ceramics or glass ceramic products is not obvious. In some embodiments, the present invention may include about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% NiO or Ni 2 O 3 When used in combination, NiO and Ni 2 O 3 The total amount is generally less than 4%, and the lower limit of the total amount is above 0.1%. In some embodiments, about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% NiO and Ni 2 O 3 . Use Pr 2 O 5As a green matrix glass, glass ceramic or glass ceramic product colorant, it is used alone, generally with a content of less than 8%, preferably less than 6%, and its lower limit is above 0.4%. If it is less than 0.4%, the color of the matrix glass, glass ceramic or glass ceramic product is not obvious. In some embodiments, the present invention may comprise about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, 8.0% Pr 2 O 5 .

[0125] The blue matrix glass, glass ceramic or glass ceramic product prepared by the present invention uses CoO or Co 2 O 3 As colorants, the two colorant components can be used alone or in combination, and their respective contents are generally less than 2%, preferably less than 1.8%. If the content exceeds 2%, the colorant cannot be well dissolved in the matrix glass, glass ceramic or glass ceramic product. The lower limit of their respective contents is above 0.05%. If it is less than 0.05%, the color of the matrix glass, glass ceramic or glass ceramic product is not obvious. In some embodiments, it may contain about 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0% CoO or Co 2 O 3 When used in combination, CoO and Co 2 O 3 The total amount does not exceed 2%, and the lower limit of the total amount is above 0.05%. In some embodiments, about 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0% of CoO and Co may be included. 2 O 3 .

[0126] The yellow matrix glass, glass ceramic or glass ceramic product prepared by the present invention uses Cu 2 O or CeO2 As a colorant, the two colorant components are used alone or in combination, and the lower limit of their respective content is above 0.5%. If it is less than 0.5%, the color of the matrix glass, glass ceramic or glass ceramic product is not obvious. 2 O is 4% or less, preferably 3% or less. If the content exceeds 4%, the matrix glass is easily crystallized. In some embodiments, about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% Cu may be included. 2 O. CeO alone 2 The content is generally below 4%, preferably below 3%. If the content exceeds 4%, the gloss of the matrix glass, glass ceramic or glass ceramic product is not good. In some embodiments, about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% CeO 2 At the same time, a small amount of CeO 2 Adding CeO to glass has the effect of removing bubbles. 2 It can also be used as a clarifier in the glass. When used as a clarifier, its content is 2% or less, preferably 1% or less, and more preferably 0.5% or less. If two colorants are mixed, their total amount is generally 4% or less, and the lower limit of the total amount is above 0.5%. In some embodiments, the CeO may include about 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% CeO 2 and Cu 2 O.

[0127] The black or smoke-grey matrix glass, glass ceramic or glass ceramic product prepared by the present invention is prepared by using Fe 2 O 3 as a colorant; or use Fe 2 O 3 and CoO as a colorant; or Fe 2 O 3 and Co 2 O 3 Two colorants mixed together; or use Fe 2 O 3 , CoO and NiO three kinds of mixed colorants; or use Fe 2 O 3 、Co 2 O 3 The colorants used in the preparation of black and smoke-gray matrix glass, glass ceramics or glass ceramic products mainly use Fe 2 O 3 Coloring, the content is 7% or less, preferably 5% or less, and the lower limit of the content is above 0.2%. In some embodiments, it can contain about 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2 .0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0%, 4.5%, 5.0%, 5.5%, 6.0%, 6.5%, 7.0% Fe 2 O 3 CoO and Co 2 O 3 It absorbs visible light and can deepen the coloring of the matrix glass, glass ceramics or glass ceramic products. It is generally related to Fe 2 O 3 When mixed, the content of each is less than 0.6%, and the lower limit is more than 0.2%. In some embodiments, about 0.2%, 0.3%, 0.4%, 0.5%, 0.6% of CoO and / or Co 2 O 3NiO absorbs visible light and can deepen the coloring of the matrix glass, glass ceramics or glass ceramic products. Generally, when mixed, its content is less than 1%, and the lower limit of the total amount is more than 0.2%. In some embodiments, about 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0% NiO may be included.

[0128] The purple matrix glass, glass ceramic or glass ceramic product prepared by the present invention uses MnO 2 As a colorant, the content is generally below 4%, preferably below 3%, and the lower limit of the content is above 0.1%. If it is below 0.1%, the color of the matrix glass, glass ceramic or glass ceramic product is not obvious. In some embodiments, the MnO may include about 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1.0%, 1.1%, 1.2%, 1.3%, 1.4%, 1.5%, 1.6%, 1.7%, 1.8%, 1.9%, 2.0%, 2.1%, 2.2%, 2.3%, 2.4%, 2.5%, 2.6%, 2.7%, 2.8%, 2.9%, 3.0%, 3.1%, 3.2%, 3.3%, 3.4%, 3.5%, 3.6%, 3.7%, 3.8%, 3.9%, 4.0% MnO 2 .

[0129] The pink matrix glass, glass ceramic or glass ceramic product prepared by the present invention uses Er 2 O 3 As a colorant, the content is generally below 8%, preferably below 6%. 2 O 3 The coloring efficiency is low. When the content exceeds 8%, the color of the matrix glass, glass ceramic or glass ceramic product cannot be further deepened, but the cost is increased. The lower limit of the content is above 0.4%. If it is lower than 0.4%, the color of the matrix glass, glass ceramic or glass ceramic product is not obvious. In some embodiments, the invention may contain about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, 8.0% of Er 2 O 3 .

[0130] The purple-red matrix glass, glass ceramic or glass ceramic product prepared by the present invention uses Nd 2 O 3 As a colorant, the content is generally below 8%, preferably below 6%. 2 O 3 The coloring efficiency is low. Even if the content exceeds 8%, the color of the matrix glass, glass ceramic or glass ceramic product cannot be further deepened, but the cost is increased. The lower limit of the content is above 0.4%. If it is lower than 0.4%, the color of the matrix glass, glass ceramic or glass ceramic product is not obvious. In some embodiments, the Nd content may be about 0.4%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.6%, 1.8%, 2.0%, 2.2%, 2.4%, 2.6%, 2.8%, 3.0%, 3.2%, 3.4%, 3.6%, 3.8%, 4.0%, 4.2%, 4.4%, 4.6%, 4.8%, 5.0%, 5.2%, 5.4%, 5.6%, 5.8%, 6.0%, 6.2%, 6.4%, 6.6%, 6.8%, 7.0%, 7.2%, 7.4%, 7.6%, 7.8%, 8.0% Nd 2 O 3 .

[0131] The red matrix glass, glass ceramic or glass ceramic product prepared by the present invention uses Er 2 O 3 、Nd 2 O 3 and MnO 2 Mixed colorants, Er ions in glass absorb at 400-500nm, Mn ions absorb mainly at 500nm, and Nd ions absorb strongly at 580nm. The mixture of the three substances can prepare red matrix glass, glass ceramics or glass ceramic products. 2 O 3 and Nd 2 O 3 It is colored by rare earth, and its coloring ability is relatively weak. 2 O 3 The usage is within 6%, Nd 2 O 3 The usage is within 4%, MnO 2 The coloring is strong, the usage amount is within the range of 2%, and the lower limit of the total amount of mixed colorants used is above 0.9%.

[0132] The "does not contain" and "0%" recorded in this article mean that the compound, molecule or element is not intentionally added as a raw material to the matrix glass, glass ceramic or glass ceramic product of the present invention; however, as raw materials and / or equipment for producing matrix glass, glass ceramic or glass ceramic products, there will be certain impurities or components that are not intentionally added, which will be contained in small amounts or trace amounts in the final matrix glass, glass ceramic or glass ceramic product, and this situation is also within the scope of protection of the patent of this invention.

[0133] In some embodiments of the present invention, the glass ceramics and glass ceramic products contain spinel crystal phases, which provide high strength for the glass ceramics and glass ceramic products of the present invention, and the fracture toughness of the glass ceramics and glass ceramic products increases; the body drop ball height of the glass ceramics and the drop ball test height and four-point bending strength of the glass ceramic products increase. The glass ceramics of the present invention have excellent chemical strengthening properties and can also be treated by chemical strengthening processes to obtain excellent mechanical strength. Through reasonable component design, the glass ceramics and glass ceramic products of the present invention can obtain a suitable grain size, so that the glass ceramics and glass ceramic products of the present invention have high strength.

[0134] The grain size and crystal phase type in the glass ceramic or glass ceramic product of the present invention will affect the haze and light transmittance of the glass ceramic or glass ceramic product. The smaller the grain, the higher the light transmittance; the smaller the haze, the higher the light transmittance. In some embodiments, the haze of the glass ceramic product or glass ceramic with a thickness of less than 1 mm is less than 0.3%, preferably less than 0.25%, and more preferably 0.05-0.2%. In some embodiments, the grain size of the glass ceramic product or glass ceramic is less than 60 nm, preferably less than 45 nm, and more preferably 10-30 nm.

[0135] In some embodiments, the crystalline content and refractive index of the glass ceramics or glass ceramic products of the present invention affect the |B| value of the glass ceramics or glass ceramic products. When observed in the visible light range, the glass ceramics or glass ceramic products appear bluish or yellowish, affecting the optical properties of the product, and are indicated by the |B| value in LAB (chromaticity value of the color of the substance). The glass ceramics or glass ceramic products of the present invention exhibit low |B| values ​​in the visible light range. In some embodiments, the average optical |B| value of 400 to 800 nm for glass ceramic products or glass ceramics with a thickness of less than 1 mm is less than 1.0, preferably less than 0.8, and more preferably 0.3 to 0.6.

[0136] In some embodiments, the glass ceramics or glass ceramic products of the present invention exhibit high transparency in the visible light range (i.e., the glass ceramics or glass ceramic products are transparent). The glass ceramics or glass ceramic products exhibit high transmittance in the visible light range. In some embodiments, the average light transmittance of the glass ceramic products or glass ceramics with a thickness of less than 1 mm at 400 to 800 nm is preferably 87.0% or more, more preferably 88.5% or more, and further preferably 89.5% or more. In some preferred embodiments, the light transmittance of the glass ceramic products or glass ceramics with a thickness of less than 1 mm at 550 nm is preferably 87.0% or more, more preferably 88.0% or more, and further preferably 89.0% or more.

[0137] In some embodiments, an antimicrobial component may be added to the matrix glass, glass ceramic, or glass ceramic article. The glass ceramic or glass ceramic article described herein may be used in applications such as kitchen or dining countertops where exposure to harmful bacteria is likely. The antimicrobial component contained in the matrix glass, glass ceramic, or glass ceramic article includes, but is not limited to, Ag, AgO, Cu, CuO, Cu 2 In some embodiments, the content of the above antimicrobial components alone or in combination is 2% or less, preferably 1% or less.

[0138] The matrix glass, glass ceramic and glass ceramic products of the present invention can be produced and manufactured by the following method:

[0139] Generating matrix glass: Mix the raw materials (oxides, hydroxides, composite salts, etc.) uniformly according to the component ratio, then put them into a crucible (e.g., a platinum or quartz crucible), and melt them in an electric furnace or a gas furnace at a temperature range of 1350 to 1550° C. for 5 to 24 hours according to the melting difficulty of the glass composition, preferably at a melting temperature of 1450 to 1550° C.; then clarify, homogenize, shape, and anneal to obtain the matrix glass. The clarifying temperature is preferably greater than 1550° C. but less than or equal to 1650° C., and the annealing temperature is preferably 450 to 600° C.

[0140] The matrix glass of the present invention can be formed by a well-known method.

[0141] The matrix glass of the present invention is subjected to crystallization treatment by crystallization process after forming or after forming processing, and crystallization is uniformly separated out inside the glass to make glass ceramics. The crystallization treatment can be carried out by 1 stage, or by 2 stages, and preferably by 2 stages. The crystallization treatment carried out in the 2 stages is the treatment of nucleation process at the 1st temperature, and then the treatment of crystal growth process at the 2nd temperature. The crystallization treatment carried out at the 1st temperature is referred to as the 1st crystallization treatment, and the crystallization treatment carried out at the 2nd temperature is referred to as the 2nd crystallization treatment.

[0142] In order to obtain the desired physical and chemical properties of glass ceramics, the preferred crystallization process is:

[0143] The above-mentioned crystallization treatment is carried out in one stage, and the nucleation process and the crystal growth process can be carried out continuously. That is, the temperature is raised to a specified crystallization treatment temperature, and after reaching the crystallization treatment temperature, the temperature is maintained for a certain period of time, and then the temperature is lowered. The crystallization treatment temperature is preferably 600 to 800°C, and in order to precipitate the desired crystalline phase, it is more preferably 650 to 750°C. The holding time at the crystallization treatment temperature is preferably 1 to 10 hours, and more preferably 3 to 6 hours.

[0144] When the crystallization treatment is carried out in two stages, the first temperature is preferably 600-700°C, the second temperature is preferably greater than 700°C but less than or equal to 800°C, the holding time at the first temperature is preferably 1-6 hours, and the holding time at the second temperature is preferably 2-5 hours.

[0145] In some embodiments, the matrix glass or glass ceramic described herein can be manufactured into a formed body by various processes, including but not limited to sheets, and the processes include but are not limited to slit drawing, float process, rolling and other processes for forming sheets known in the art. Alternatively, the matrix glass or glass ceramic can be formed by float process or rolling process known in the art. The formed body of the present invention also includes lenses, prisms, etc.

[0146] The matrix glass or glass ceramic of the present invention can be processed by grinding or polishing to produce a glass molded body or glass ceramic molded body in the form of a sheet, but the method for producing the glass molded body or glass ceramic molded body is not limited to these methods.

[0147] The matrix glass or glass ceramic of the present invention can be prepared into glass molded bodies or glass ceramic molded bodies of various shapes by a heat bending process or a press molding process at a certain temperature, but is not limited to these methods.

[0148] In some embodiments, a glass forming body or a glass ceramic forming body can be formed by a hot bending process. The hot bending process is a process in which a 2D or 2.5D glass or glass ceramic is placed in a mold and a 3D curved glass forming body or a glass ceramic forming body is formed by sequentially performing steps including heating preheating, pressurizing, and cooling under pressure in a hot bending machine.

[0149] In some embodiments, the glass-ceramic formed body has a 2.5D or 3D configuration, i.e., the glass-ceramic formed body has a non-planar configuration. As used herein, "non-planar configuration" means that in a 2.5D or 3D shape, at least a portion of the glass-ceramic formed body extends outward or extends along an angle with a plane defined by the original, laid-out configuration of the 2D matrix glass. A 2.5D or 3D glass-ceramic formed body formed from a matrix glass may have one or more protrusions or curved portions.

[0150] In some embodiments, in combination with the growth of the crystal phase and the transformation of the crystal phase in the glass ceramic, the manufacturing method of the glass ceramic formed body is a hot bending process method. Specifically, the method includes pre-crystallization and hot working forming. The pre-crystallization of the present invention is to form a pre-crystallized glass by controlling the crystallization process of the matrix glass, and the crystallinity of the pre-crystallized glass does not reach the crystallinity required by the performance index of the target glass ceramic formed body. The pre-crystallized glass is then formed into a glass ceramic formed body by a hot working forming process.

[0151] In some embodiments, a method for making a glass-ceramic formed body comprises the following steps:

[0152] 1) subjecting the matrix glass to a crystallization heat treatment process, including heating, heat preservation nucleation, heating, heat preservation crystallization, and cooling to room temperature to form pre-crystallized glass;

[0153] 2) The pre-crystallized glass is thermally processed to obtain a glass ceramic formed body.

[0154] The crystallization heat treatment process of the present invention comprises: heating the matrix glass at a certain temperature T h and time t h Under the condition of nucleation, then at a certain temperature T c and time t c The crystallinity of the obtained pre-crystallized glass did not reach the crystallinity required by the performance index of the target glass-ceramic formed body. Using the XRD test data, the total content of the main crystalline phase in the crystallinity of the pre-crystallized glass was calculated by the Rietveld full spectrum fitting refinement method. c1 . The pre-crystallization of the present invention is a complete process in terms of the process, including a nucleation process, one, two or three or more crystallization processes, etc. It is a complete process of heating, heat preservation, heating again, heat preservation..., and then cooling to room temperature according to the process. Different from the primary crystallization, secondary crystallization... mentioned in some documents or patents, the present invention is actually only the first crystallization, the second crystallization... in a complete crystallization process, and the middle is continuous, and there is no process of heating up again after cooling to room temperature.

[0155] The hot working forming of the present invention refers to the hot working process forming the pre-crystallized glass under certain conditions of temperature, time, pressure, etc., and the hot working forming includes more than one hot working process, and the hot working process includes but is not limited to pressing, bending or drawing the pre-crystallized glass under certain conditions of temperature, time, pressure, etc. In the hot working forming process, sometimes a molded body with a complex shape cannot be completed by one hot working, and may need to be completed by multiple hot workings of more than two times.

[0156] In some embodiments, the method for manufacturing the glass-ceramic formed body is a hot bending process. Specifically, in some embodiments, the method for manufacturing the glass-ceramic formed body comprises the following steps:

[0157] 1) Preheating: Place the matrix glass or pre-crystallized glass or glass ceramic in the mold, and the mold passes through each heating station in the heat bending machine in turn, and stays at each station for a certain period of time to keep warm. The temperature in the preheating zone is 400-800°C, the pressure is 0.01-0.05MPa, and the time is 40-200s. In some embodiments, for a heat bending machine with 5 preheating stations, the initial temperature rise is generally set to about 500°C, and the subsequent stations gradually increase the temperature. The temperature gradient between two adjacent stations gradually decreases from low temperature to high temperature, and the temperature difference between the last preheating station and the first molding station is within 20°C.

[0158] 2) Pressurized molding: After preheating, the mold is transferred to the molding station. The hot bending machine applies a certain pressure to the mold. The pressure range is 0.1-0.8Mpa. The pressure is determined according to factors such as glass thickness and curvature. The molding station temperature range is 600-850℃, and the molding time range is 40-200s.

[0159] 3) Maintaining pressure and cooling: The mold is transferred to the cooling station and cooled down step by step. The cooling temperature range is controlled at 750-500℃, the pressure is 0.01-0.05Mpa, and the time is 40-200s.

[0160] In addition to controlling the appearance quality of ordinary high-aluminum glass, the hot bending process of glass-ceramic formed bodies also requires controlling the impact of crystal growth and development on the performance of glass-ceramic during the hot bending process. For example, 3D curved glass-ceramic used for display devices or electronic equipment casings requires close attention to light transmittance, haze, |B| value and uniformity after hot bending.

[0161] The matrix glasses, glass-ceramics and glass-ceramic articles described herein can have any reasonably useful thickness.

[0162] In addition to improving mechanical properties by crystallization, the glass ceramics of the present invention can also obtain more excellent mechanical properties by forming a compressive stress layer, thereby making glass ceramic products.

[0163] In some embodiments, the matrix glass or glass ceramic can be processed into sheets and / or shaped (such as punching, hot bending, etc.), polished and / or swept after shaping, and then chemically strengthened through a chemical strengthening process.

[0164] The chemical strengthening described in the present invention is an ion exchange method. During the ion exchange process, smaller metal ions in the matrix glass or glass ceramic are replaced or "exchanged" by larger metal ions with the same valence state near the matrix glass or glass ceramic. The replacement of smaller ions with larger ions builds up compressive stress in the matrix glass or glass ceramic, forming a compressive stress layer.

[0165] In some embodiments, the metal ion is a monovalent alkali metal ion (e.g., Na + , K + , Rb + , Cs + Ion exchange is performed by immersing the matrix glass or glass ceramic in a salt bath of at least one molten salt containing larger metal ions, which are used to replace smaller metal ions in the matrix glass. Alternatively, other monovalent metal ions such as Ag + , Tl + , Cu + The one or more ion exchange processes used to chemically strengthen the matrix glass or glass-ceramic may include, but are not limited to, immersing it in a single salt bath, or immersing it in multiple salt baths of the same or different compositions with washing and / or annealing steps between immersions.

[0166] In some embodiments, the matrix glass or glass ceramic may be prepared by immersing it in a molten Na salt (e.g., NaNO) at a temperature of about 350-470°C. 3 ) for about 1 to 36 hours for ion exchange, preferably in a temperature range of 400 to 460° C., and preferably in a time range of 2 to 15 hours. In this embodiment, Na ions replace part of the Li ions in the matrix glass or glass ceramic, thereby forming a surface compression layer and exhibiting high mechanical properties. In some embodiments, the matrix glass or glass ceramic can be ion exchanged by immersing in a mixed salt bath of molten K salt and Na salt at a temperature of about 360 to 450° C. for 1 to 36 hours, preferably in a time range of 2 to 24 hours.

[0167] The glass ceramics involved in the present invention have efficient low-temperature ion exchange performance. In some embodiments, at a lower ion exchange temperature and a shorter exchange time, the exchange layer depth of Na ions can reach more than 75μm. After ion exchange, the hardness of the glass ceramic product is significantly improved. The main reason is that the ion exchange forms a higher compressive stress on the surface of the glass ceramic product through the "crowding effect", which increases the deformation resistance of the glass ceramic product and improves the hardness. In some embodiments, after the glass ceramics of the present invention are chemically strengthened, the Vickers hardness of the obtained glass ceramic product can reach 650kgf / mm 2 above.

[0168] The various performance indicators of the glass ceramics and / or glass ceramic products of the present invention are tested by the following methods:

[0169] [Haze]

[0170] A haze tester, Minolta CM3600A, was used to prepare samples with a thickness of less than 1 mm and the test was carried out according to the standard of GB2410-80.

[0171] [Grain size]

[0172] The glass ceramics were surface treated in HF acid, gold was sprayed on the surface of the glass ceramics, and the surface was scanned under the SEM scanning electron microscope to determine the size of the grains.

[0173] [Light transmittance]

[0174] The light transmittances described in this article are all external transmittances, sometimes referred to as transmittance.

[0175] The sample was processed to a thickness of less than 1 mm and the opposite surfaces were polished parallel to each other, and the average light transmittance at 400 to 800 nm was measured using a Hitachi U-41000 spectrophotometer.

[0176] The sample was processed to a thickness of less than 1 mm and the opposite surfaces were polished parallel to each other, and the light transmittance at 550 nm was measured using a Hitachi U-41000 spectrophotometer.

[0177] [Depth of ion exchange layer]

[0178] The depth of the ion exchange layer was measured using a glass surface stress meter SLP-2000.

[0179] The calculation was performed under the measurement conditions that the refractive index of the sample was 1.56 and the photoelastic constant was 29 [(nm / cm) / Mpa].

[0180] [Surface stress]

[0181] The surface stress was measured using a glass surface stress meter SLP-2000.

[0182] The calculation was performed under the measurement conditions that the refractive index of the sample was 1.56 and the photoelastic constant was 29 [(nm / cm) / Mpa].

[0183] [Drop resistance]

[0184] Use directional drop tester WH-2101 to carry out drop resistance test.By loading the same specification glass products on 2D glass ceramic products (each piece weighs 20g, load 2 pieces), laying 60-80 mesh sandpaper on the base, free fall from a specified height, the sample directly hits the sandpaper, and the height of the impact that can be sustained without breaking is drop resistance.Specifically, the test is implemented from a height of 600mm, and the height is changed in sequence by 700mm, 800mm, 900mm, 1000mm and above without breaking.For the embodiment with "drop resistance", glass ceramic products are used as test objects.The test data recorded as 1000mm in the embodiment indicates that even if the glass ceramic products with load from a height of 1000mm do not break and withstand the impact, the highest experimental height of the drop tester WH-2101 is 2000mm.

[0185] [Drop ball test height]

[0186] A glass ceramic product sample of 145mm×67mm×0.7mm is placed on a glass supporting fixture, and a 132g steel ball is dropped from a specified height, with the drop point being the center point of the sample. The maximum drop ball test height at which the sample can withstand the impact without breaking. Specifically, the drop ball test height starts at 400mm, and the ball is dropped once at each height. If the sample does not break, the test is continued by rising 100mm in sequence until the sample breaks. For the embodiments with a "drop ball test height", glass ceramic products are used as test objects. The test data recorded as 1700mm in the embodiments indicates that even if a steel ball is dropped from a height of 1700mm, the glass ceramic product will not break and will withstand the impact. The drop ball test height in the present invention is sometimes referred to as the drop ball height.

[0187] [Fracture toughness]

[0188] The method of directly measuring the size of the indentation crack extension was used. The sample size was 2mm×4mm×20mm. After chamfering, grinding and polishing, the sample preparation was completed. A force of 49N was applied to the sample with a Vickers hardness indenter and maintained for 30s. After the indentation was made, the fracture strength was determined by the three-point bending method.

[0189] [Four-point bending strength]

[0190] A microcomputer-controlled electronic universal testing machine CMT6502 is used, and the sample specification is less than 1 mm thick (preferably 0.7 mm thick), and the test is performed according to the standard of "ASTM C 158-2002". In the present invention, the four-point bending strength is sometimes referred to as bending strength.

[0191] [Vickers hardness]

[0192] The load (N) when a diamond quadrangular pyramid indenter with an angle of 136° between the opposite faces is pressed into a pyramid-shaped depression on the test surface is divided by the surface area (mm2) calculated by the length of the depression. 2 ) value. The test load was 100 (N) and the holding time was 15 (seconds). In the present invention, Vickers hardness may be simply referred to as hardness.

[0193] [Compression strength]

[0194] Using a microcomputer-controlled electronic universal testing machine CMT6502, place a 145mm×67mm×0.7mm glass-ceramic product sample on a glass supporting fixture. The extrusion rod adopts a mushroom head design with a diameter of ¢10mm and a downward pressure speed of 5mm / min until the sample is broken. Calibration with a fixture is required before the test, and the test point is at the center position. Click the test button until the glass-ceramic product sample is squeezed and broken, and record the pressure (N) when the sample is broken. For the embodiments with "anti-extrusion strength", glass-ceramic products are used as test objects. The test data recorded as 500N in the embodiment indicates that the maximum extrusion force that the glass-ceramic product can withstand before breaking is 500N.

[0195] [|B|value]

[0196] Use Minolta CM-700d to test the B value. The sample specification is less than 1mm thick. Use the matching calibration long tube and short tube to perform instrument zero calibration and white plate calibration respectively. After calibration, use the long tube to perform air test again to determine the stability and calibration reliability of the instrument (B≤0.05). After the instrument is calibrated, place the product on the zero long tube for testing.

[0197] The |B| value is the absolute value of the B value.

[0198] [Young's modulus]

[0199] Young's modulus (E) is calculated using the following formula by ultrasonic testing of its longitudinal wave velocity and transverse wave velocity.

[0200]

[0201] G=V S 2 ρ

[0202] Where: E is Young's modulus, Pa;

[0203] G is the shear modulus, Pa;

[0204] V T is the shear wave velocity, m / s;

[0205] V S is the longitudinal wave velocity, m / s;

[0206] ρ is the glass density, g / cm 3 .

[0207] The glass ceramic product of the present invention has the following properties:

[0208] 1) In some embodiments, the grain size of the glass ceramic product is less than 60 nm, preferably less than 45 nm, and more preferably 10 to 30 nm.

[0209] 2) In some embodiments, the ion exchange layer of the glass ceramic product has a depth of 75 μm or more, preferably 80 to 150 μm, and more preferably 100 to 125 μm.

[0210] 3) In some embodiments, the surface stress of the glass ceramic product is greater than 200 MPa, preferably 250 to 400 MPa, and more preferably 300 to 400 MPa.

[0211] 4) In some embodiments, the drop ball test height of the glass ceramic product is greater than 1000 mm, preferably greater than 1200 mm, and more preferably greater than 1500 mm.

[0212] 5) In some embodiments, the drop resistance of the glass ceramic product is above 1200 mm, preferably above 1300 mm, and more preferably above 1400 mm.

[0213] 6) In some embodiments, the fracture toughness of the glass-ceramic article is 1.0 MPa·m 1 / 2 Above, preferably 1.2 MPa·m 1 / 2 More preferably, 1.2 to 1.6 MPa·m 1 / 2 .

[0214] 7) In some embodiments, the four-point bending strength of the glass ceramic product is 500 MPa or more, preferably 600 MPa or more, and more preferably 700-1000 MPa.

[0215] 8) In some embodiments, the compressive strength of the glass ceramic product is greater than 400N, preferably 400-550N, and more preferably 450-550N.

[0216] 9) In some embodiments, the Vickers hardness (Hv ) is 650kgf / mm 2 Above, preferably 660kgf / mm 2 More preferably, 680 to 750 kgf / mm 2 .

[0217] 10) In some embodiments, the haze of the glass ceramic product with a thickness of less than 1 mm is less than 0.3%, preferably less than 0.25%, more preferably 0.05-0.2%. The thickness is preferably 0.2-1 mm, more preferably 0.3-0.9 mm, further preferably 0.5-0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.

[0218] 11) In some embodiments, the glass ceramic product with a thickness of 1 mm or less has an average light transmittance of 87.0% or more at a wavelength of 400 to 800 nm, preferably 88.5% or more, and more preferably 89.5% or more. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.

[0219] 12) In some embodiments, the glass ceramic product with a thickness of 1 mm or less has a light transmittance of 87.0% or more, preferably 88.0% or more, and more preferably 89.0% or more at a wavelength of 550 nm. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.

[0220] 13) In some embodiments, for a glass ceramic product having a thickness of less than 1 mm, the average optical |B| value at 400 to 800 nm is less than 1.0, preferably less than 0.8, and more preferably 0.3 to 0.6. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.

[0221] The glass ceramics of the present invention have the following properties:

[0222] 1) In some embodiments, the grain size of the glass ceramic is less than 60 nm, preferably less than 45 nm, and more preferably 10 to 30 nm.

[0223] 2) In some embodiments, the haze of the glass ceramic with a thickness of 1 mm or less is 0.3% or less, preferably 0.25% or less, and more preferably 0.05-0.2%. The thickness is preferably 0.2-1 mm, more preferably 0.3-0.9 mm, further preferably 0.5-0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.

[0224] 3) In some embodiments, the glass ceramic with a thickness of 1 mm or less has an average light transmittance of 87.0% or more at a wavelength of 400 to 800 nm, preferably 88.5% or more, and more preferably 89.5% or more. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.

[0225] 4) In some embodiments, the glass ceramic with a thickness of 1 mm or less has a light transmittance of 87.0% or more, preferably 88.0% or more, and more preferably 89.0% or more at a wavelength of 550 nm. The thickness is preferably 0.2 to 1 mm, more preferably 0.3 to 0.9 mm, further preferably 0.5 to 0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.

[0226] 5) In some embodiments, for glass ceramics with a thickness of less than 1 mm, the average optical |B| value at 400-800 nm is less than 1.0, preferably less than 0.8, and more preferably 0.3-0.6. The thickness is preferably 0.2-1 mm, more preferably 0.3-0.9 mm, further preferably 0.5-0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm, or 0.75 mm.

[0227] 6) In some embodiments, the Young's modulus (E) of the glass ceramic is 80 to 110 GPa, preferably 85 to 105 GPa, and more preferably 90 to 105 GPa.

[0228] 7) In some embodiments, the Vickers hardness (H v ) is 550kgf / mm 2 Above, preferably 580kgf / mm 2 More preferably, 600 to 650 kgf / mm 2 .

[0229] The glass ceramics, glass ceramic products, matrix glass, glass formed bodies, and glass ceramic formed bodies of the present invention can be widely made into glass cover plates or glass components due to the above-mentioned excellent properties; at the same time, the glass ceramics, glass ceramic products, matrix glass, glass formed bodies, and glass ceramic formed bodies of the present invention can be applied to electronic devices or display devices, such as mobile phones, watches, computers, touch screens, etc., for manufacturing protective glass for mobile phones, smart phones, tablet computers, laptop computers, PDAs, televisions, personal computers, MTA machines, or industrial displays, or for manufacturing touch screens, protective windows, car windows, train windows, aviation machinery windows, touch screen protective glass, or for manufacturing hard disk substrates or solar cell substrates, or for manufacturing white household appliances, such as for manufacturing refrigerator parts or kitchen utensils.

[0230] Example

[0231] In order to further clearly illustrate and describe the technical solution of the present invention, the following non-limiting examples are provided. The present invention embodiments have been tried to ensure the accuracy of the values ​​(such as quantity, temperature, etc.), but some errors and deviations must be taken into account. The composition itself is given in weight % based on the oxide and has been standardized to 100%.

[0232] <Glass Ceramic Example>

[0233] This embodiment adopts the manufacturing method of the above-mentioned glass ceramic to obtain glass ceramics having the composition shown in Tables 1 to 4. In addition, the characteristics of each glass ceramic are measured by the test method described in the present invention, and the measurement results are shown in Tables 1 to 4. In the following embodiments, the thickness of the test sample for haze, average light transmittance at wavelengths of 400 to 800 nm, light transmittance at wavelengths of 550 nm, and average light |B| value at wavelengths of 400 to 800 nm is 0.7 mm.

[0234] Table 1.

[0235]

[0236]

[0237] Table 2.

[0238]

[0239]

[0240] Table 3.

[0241]

[0242]

[0243] Table 4.

[0244]

[0245]

[0246] <Glass Ceramic Product Example>

[0247] In this embodiment, the manufacturing method of the glass ceramic product is used to obtain glass ceramic products having the compositions shown in Tables 5 to 8. In addition, the properties of each glass ceramic product are measured by the test method described in the present invention, and the test results are shown in Tables 5 to 8. In the following embodiments, the thickness of the test sample for haze, average light transmittance at wavelengths of 400 to 800 nm, light transmittance at wavelengths of 550 nm, and average light |B| value at wavelengths of 400 to 800 nm is 0.7 mm.

[0248] Table 5.

[0249]

[0250]

[0251] Table 6.

[0252]

[0253]

[0254] Table 7.

[0255]

[0256]

[0257]

[0258] Table 8.

[0259]

[0260]

Claims

1. A glass ceramic product, characterized in that: Its components, expressed in weight percentage, contain: SiO2: 40-55%; Al2O3: 15-30%; Li2O: 0.1-6%; ZnO: 9~20%; MgO: 0.1~6%; TiO2: 0.5~7%, of which SiO2 / Al2O3 is 1.5~3.

2.

2. The glass ceramic product according to claim 1, characterized in that: Its components, expressed in weight percentage, also contain: P2O5: 0-5%; and / or ZrO2: 0-5%; and / or Na2O: 0-6%; and / or B2O3: 0-4%; and / or K2O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y2O3: 0-6%; and / or clarifier: 0-2%.

3. A glass ceramic product, characterized in that: Its components, expressed by weight percentage, are SiO2: 40-55%; Al2O3: 15-30%; Li2O: 0.1-6%; ZnO: 9~20%; MgO: 0.1~6%; TiO2: 0.5~7%; P2O5: 0~5%; ZrO2: 0~5%; Na2O: 0~6%; B2O3: 0~4%; K2O: 0~3%; CaO+BaO+SrO: 0~5%; Y2O3: 0~6%; Clarifier: 0~2%, of which SiO2 / Al2O3 is 1.5~3.

2.

4. The glass ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed in weight percentage, wherein: SiO2 / Al2O3 is 1.7-3.0, preferably SiO2 / Al2O3 is 1.8-2.8, more preferably SiO2 / Al2O3 is 2.0-2.5; and / or Al2O3+ZnO is 26-45%, preferably Al2O3+ZnO is 30-42%, more preferably Al2O3+ZnO is 32-42%, and further preferably Al2O3+ZnO is 35-40%; and / or (TiO2+ZnO) / Al2O3 is 0.4-1.5, preferably (TiO2+ZnO) / Al2O3 is 0.5-1.2, more preferably (TiO2+ZnO) / Al2O3 is 0.6-1.0, and further preferably (TiO2+ZnO) / Al2O3 is 0.6-0.9; and / or ( Li2O+MgO) / TiO2 is 0.3~8.0, preferably (Li2O+MgO) / TiO2 is 0.5~5.0, more preferably (Li2O+MgO) / TiO2 is 1.0~3.0, and further preferably (Li2O+MgO) / TiO2 is 1.2~2.5; and / or Al2O3 / (MgO+TiO2) is 1.3~10.0, preferably Al2O3 / (MgO+TiO2) is 1.5~8.0, more preferably Al2O3 / (MgO+TiO2) is 2.5~6.5, and further preferably Al2O3 / (MgO+TiO2) is 3.0~5.5; and / or P2O5+ZrO2: 0~8%, preferably P2O5+ZrO2: 0.1~7%, more preferably P2O5+ZrO2: 0.5~5%.

5. The glass ceramic product according to any one of claims 1 to 3, characterized in that: The components are expressed in weight percentage, wherein: Li2O / TiO2 is 0.2-4.5, preferably Li2O / TiO2 is 0.5-3.5, more preferably Li2O / TiO2 is 0.7-2.5, and further preferably Li2O / TiO2 is 0.75-1.5; and / or Al2O3 / ZnO is 1.0-3.0, preferably Al2O3 / ZnO is 1.2-2.8, and more preferably Al2O3 / ZnO is 1.5-2.0; and / or Al2O3 / ZnO is 1.0-3.0, preferably Al2O3 / ZnO is 1.2-2.8, and further ... nO is 1.25 to 2.5, and more preferably Al2O3 / ZnO is 1.5 to 2.3; and / or (Al2O3+Li2O) / P2O5 is 5.0 to 45.0, and preferably (Al2O3+Li2O) / P2O5 is 7.0 to 35.0, and more preferably (Al2O3+Li2O) / P2O5 is 8.0 to 30.0, and more preferably (Al2O3+Li2O) / P2O5 is 10 .0~25.0; and / or P2O5 / ZrO2 is 0.1~5.0, preferably P2O5 / ZrO2 is 0.2~3.0, more preferably P2O5 / ZrO2 is 0.5~2.0, and further preferably P2O5 / ZrO2 is 0.6~1.5; and / or (SiO2+Na2O) / ZnO is 2.2~6.2, preferably (SiO2+Na2O) / ZnO is 2.5~6.0, and more preferably (SiO2+Na2O) / ZnO is 2.8~5.5, and more preferably (SiO2+Na2O) / ZnO is 3.0~5.0; and / or (Na2O+K2O) / ZnO is below 0.8, preferably (Na2O+K2O) / ZnO is below 0.6, more preferably (Na2O+K2O) / ZnO is below 0.4, and further preferably (Na2O+K2O) / ZnO is below 0.

2.

6. The glass ceramic product according to any one of claims 1 to 3, characterized in that: Its components are expressed by weight percentage, wherein: SiO2: 45-53%, preferably SiO2: 48-52%; and / or Al2O3: 18-25%, preferably Al2O3: 20-23%; and / or Li2O: 1-5%, preferably Li2O: 2-4%; and / or ZnO: 11-18%, preferably ZnO: 12-16%; and / or MgO: 1-5%, preferably MgO: 2-4%; and / or TiO2: 1-6%, preferably TiO2: 2-5%; and / or P2O5: 0.5-4%, preferably P2O5: 1~3%; and / or ZrO2: 0.5~4%, preferably ZrO2: 1~3%; and / or Na2O: 0~4%, preferably Na2O: 0~2%; and / or B2O3: 0~2%, preferably B2O3: 0~1%; and / or K2O: 0~2%, preferably K2O: 0~1%; and / or CaO+BaO+SrO: 0~4%, preferably CaO+BaO+SrO: 0~2%; and / or Y2O3: 0~4%, preferably Y2O3: 0~2%; and / or clarifier: 0~1%, preferably clarifier: 0~0.5%.

7. The glass ceramic product according to any one of claims 1 to 3, characterized in that: The glass ceramic product contains a spinel crystal phase, and preferably the spinel crystal phase has a higher weight percentage than other crystal phases. More preferably, the spinel crystal phase accounts for 20-60% of the weight percentage of the glass ceramic product. Further preferably, the spinel crystal phase accounts for 25-50% of the weight percentage of the glass ceramic product. Further preferably, the spinel crystal phase accounts for 25-45% of the weight percentage of the glass ceramic product. Even more preferably, the spinel crystal phase accounts for 30-45% of the weight percentage of the glass ceramic product.

8. The glass ceramic product according to any one of claims 1 to 3, characterized in that: The glass ceramic product contains a quartz crystal phase, and preferably the weight percentage of the quartz crystal phase in the glass ceramic product is less than 20%, more preferably the weight percentage of the quartz crystal phase in the glass ceramic product is less than 10%, further preferably the weight percentage of the quartz crystal phase in the glass ceramic product is less than 5%, and further preferably the glass ceramic product does not contain a quartz crystal phase.

9. The glass ceramic product according to any one of claims 1 to 3, characterized in that: The glass ceramic product has a grain size of 60 nm or less, preferably 45 nm or less, more preferably 10-30 nm; and / or an ion exchange layer depth of 75 μm or more, preferably 80-150 μm, more preferably 100-125 μm; and / or a surface stress of 200 MPa or more, preferably 250-400 MPa, more preferably 300-400 MPa; and / or a drop ball test height of 1000 mm or more, preferably 1200 mm or more, more preferably 1500 mm or more; and / or a drop resistance of 1200 mm or more, preferably 1300 mm or more, more preferably 1400 mm or more; and / or a fracture toughness of 1.0 MPa·m 1 / 2 Above, preferably 1.2 MPa·m 1 / 2 More preferably, 1.2 to 1.6 MPa·m 1 / 2 ; and / or a four-point bending strength of 500 MPa or more, preferably 600 MPa or more, more preferably 700-1000 MPa; and / or an anti-compression strength of 400 N or more, preferably 400-550 N, more preferably 450-550 N; and / or a Vickers hardness of 650 kgf / mm 2 Above, preferably 660kgf / mm 2 More preferably, 680 to 750 kgf / mm 2 .

10. The glass ceramic product according to any one of claims 1 to 3, characterized in that: The haze of glass ceramic products with a thickness of less than 1 mm is less than 0.3%, preferably less than 0.25%, more preferably 0.05-0.2%; and / or the average light transmittance at a wavelength of 400-800 nm is greater than 87.0%, preferably greater than 88.5%, more preferably greater than 89.5%; and / or the light transmittance at a wavelength of 550 nm is greater than 87.0%, preferably greater than 88.0%, more preferably greater than 89.0%; and / or the average light |B| value at 400-800 nm is less than 1.0, preferably less than 0.8, more preferably 0.3-0.

6.

11. The glass ceramic product according to claim 10, characterized in that: The thickness of the glass ceramic product is 0.2-1 mm, preferably 0.3-0.9 mm, more preferably 0.5-0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm or 0.75 mm.

12. The glass ceramic product according to claim 1 or 2, characterized in that: Its components, expressed in weight percentage, include: NiO: 0-4%; and / or Ni2O3: 0-4%; and / or CoO: 0-2%; and / or Co2O3: 0-2%; and / or Fe2O3: 0-7%; and / or MnO2: 0-4%; and / or Er2O3: 0-8%; and / or Nd2O3: 0-8%; and / or Cu2O: 0-4%; and / or Pr2O3: 0-8%; and / or CeO2: 0-4%.

13. Glass ceramics, characterized in that Its components, expressed in weight percentage, contain: SiO2: 40-55%; Al2O3: 15-30%; Li2O: 0.1-6%; ZnO: 9~20%; MgO: 0.1~6%; TiO2: 0.5~7%, of which SiO2 / Al2O3 is 1.5~3.

2.

14. The glass ceramic according to claim 13, characterized in that Its components, expressed in weight percentage, also contain: P2O5: 0-5%; and / or ZrO2: 0-5%; and / or Na2O: 0-6%; and / or B2O3: 0-4%; and / or K2O: 0-3%; and / or CaO+BaO+SrO: 0-5%; and / or Y2O3: 0-6%; and / or clarifier: 0-2%.

15. Glass ceramics, characterized in that Its components, expressed by weight percentage, are SiO2: 40-55%; Al2O3: 15-30%; Li2O: 0.1-6%; ZnO: 9~20%; MgO: 0.1~6%; TiO2: 0.5~7%; P2O5: 0~5%; ZrO2: 0~5%; Na2O: 0~6%; B2O3: 0~4%; K2O: 0~3%; CaO+BaO+SrO: 0~5%; Y2O3: 0~6%; Clarifier: 0~2%, of which SiO2 / Al2O3 is 1.5~3.

2.

16. The glass ceramic according to any one of claims 13 to 15, characterized in that: Its components are expressed in weight percentage, wherein: SiO2 / Al2O3 is 1.7-3.0, preferably SiO2 / Al2O3 is 1.8-2.8, more preferably SiO2 / Al2O3 is 2.0-2.5; and / or Al2O3+ZnO is 26-45%, preferably Al2O3+ZnO is 30-42%, more preferably Al2O3+ZnO is 32-42%, and further preferably Al2O3+ZnO is 35-40%; and / or (TiO2+ZnO) / Al2O3 is 0.4-1.5, preferably (TiO2+ZnO) / Al2O3 is 0.5-1.2, more preferably (TiO2+ZnO) / Al2O3 is 0.6-1.0, and further preferably (TiO2+ZnO) / Al2O3 is 0.6-0.9; and / or ( Li2O+MgO) / TiO2 is 0.3~8.0, preferably (Li2O+MgO) / TiO2 is 0.5~5.0, more preferably (Li2O+MgO) / TiO2 is 1.0~3.0, and further preferably (Li2O+MgO) / TiO2 is 1.2~2.5; and / or Al2O3 / (MgO+TiO2) is 1.3~10.0, preferably Al2O3 / (MgO+TiO2) is 1.5~8.0, more preferably Al2O3 / (MgO+TiO2) is 2.5~6.5, and further preferably Al2O3 / (MgO+TiO2) is 3.0~5.5; and / or P2O5+ZrO2: 0~8%, preferably P2O5+ZrO2: 0.1~7%, more preferably P2O5+ZrO2: 0.5~5%.

17. The glass ceramic according to any one of claims 13 to 15, characterized in that: The components are expressed in weight percentage, wherein: Li2O / TiO2 is 0.2-4.5, preferably Li2O / TiO2 is 0.5-3.5, more preferably Li2O / TiO2 is 0.7-2.5, and further preferably Li2O / TiO2 is 0.75-1.5; and / or Al2O3 / ZnO is 1.0-3.0, preferably Al2O3 / ZnO is 1.2-2.8, and more preferably Al2O3 / ZnO is 1.5-2.0; and / or Al2O3 / ZnO is 1.0-3.0, preferably Al2O3 / ZnO is 1.2-2.8, and further ... nO is 1.25 to 2.5, and more preferably Al2O3 / ZnO is 1.5 to 2.3; and / or (Al2O3+Li2O) / P2O5 is 5.0 to 45.0, and preferably (Al2O3+Li2O) / P2O5 is 7.0 to 35.0, and more preferably (Al2O3+Li2O) / P2O5 is 8.0 to 30.0, and more preferably (Al2O3+Li2O) / P2O5 is 10 .0~25.0; and / or P2O5 / ZrO2 is 0.1~5.0, preferably P2O5 / ZrO2 is 0.2~3.0, more preferably P2O5 / ZrO2 is 0.5~2.0, and further preferably P2O5 / ZrO2 is 0.6~1.5; and / or (SiO2+Na2O) / ZnO is 2.2~6.2, preferably (SiO2+Na2O) / ZnO is 2.5~6.0, and more preferably (SiO2+Na2O) / ZnO is 2.8~5.5, and more preferably (SiO2+Na2O) / ZnO is 3.0~5.0; and / or (Na2O+K2O) / ZnO is below 0.8, preferably (Na2O+K2O) / ZnO is below 0.6, more preferably (Na2O+K2O) / ZnO is below 0.4, and further preferably (Na2O+K2O) / ZnO is below 0.

2.

18. The glass ceramic according to any one of claims 13 to 15, characterized in that: Its components are expressed by weight percentage, wherein: SiO2: 45-53%, preferably SiO2: 48-52%; and / or Al2O3: 18-25%, preferably Al2O3: 20-23%; and / or Li2O: 1-5%, preferably Li2O: 2-4%; and / or ZnO: 11-18%, preferably ZnO: 12-16%; and / or MgO: 1-5%, preferably MgO: 2-4%; and / or TiO2: 1-6%, preferably TiO2: 2-5%; and / or P2O5: 0.5-4%, preferably P2O5: 1~3%; and / or ZrO2: 0.5~4%, preferably ZrO2: 1~3%; and / or Na2O: 0~4%, preferably Na2O: 0~2%; and / or B2O3: 0~2%, preferably B2O3: 0~1%; and / or K2O: 0~2%, preferably K2O: 0~1%; and / or CaO+BaO+SrO: 0~4%, preferably CaO+BaO+SrO: 0~2%; and / or Y2O3: 0~4%, preferably Y2O3: 0~2%; and / or clarifier: 0~1%, preferably clarifier: 0~0.5%.

19. The glass ceramic according to any one of claims 13 to 15, characterized in that: The glass ceramic contains a spinel crystal phase, and the spinel crystal phase preferably has a higher weight percentage than other crystal phases. More preferably, the spinel crystal phase accounts for 20-60% of the weight percentage of the glass ceramic. Further preferably, the spinel crystal phase accounts for 25-50% of the weight percentage of the glass ceramic. Further preferably, the spinel crystal phase accounts for 25-45% of the weight percentage of the glass ceramic. Further preferably, the spinel crystal phase accounts for 30-45% of the weight percentage of the glass ceramic.

20. The glass ceramic according to any one of claims 13 to 15, characterized in that: The glass ceramic contains a quartz crystal phase, and preferably the weight percentage of the quartz crystal phase in the glass ceramic is less than 20%, more preferably the weight percentage of the quartz crystal phase in the glass ceramic is less than 10%, further preferably the weight percentage of the quartz crystal phase in the glass ceramic is less than 5%, and further preferably the glass ceramic does not contain a quartz crystal phase.

21. The glass ceramic according to any one of claims 13 to 15, characterized in that: The glass ceramic has a grain size of 60 nm or less, preferably 45 nm or less, more preferably 10 to 30 nm; and / or a Young's modulus of 80 to 110 GPa, preferably 85 to 105 GPa, more preferably 90 to 105 GPa; and / or a Vickers hardness of 550 kgf / mm 2 Above, preferably 580kgf / mm 2 More preferably, 600 to 650 kgf / mm 2 .

22. The glass ceramic according to any one of claims 13 to 15, characterized in that: The haze of glass ceramics with a thickness of less than 1 mm is less than 0.3%, preferably less than 0.25%, more preferably 0.05-0.2%; and / or the average light transmittance at a wavelength of 400-800 nm is greater than 87.0%, preferably greater than 88.5%, more preferably greater than 89.5%; and / or the light transmittance at a wavelength of 550 nm is greater than 87.0%, preferably greater than 88.0%, more preferably greater than 89.0%; and / or the average light |B| value at 400-800 nm is less than 1.0, preferably less than 0.8, more preferably 0.3-0.

6.

23. The glass ceramic according to claim 22, characterized in that The thickness of the glass ceramic is 0.2-1 mm, preferably 0.3-0.9 mm, more preferably 0.5-0.8 mm, and further preferably 0.55 mm, 0.6 mm, 0.68 mm, 0.7 mm or 0.75 mm.

24. The glass ceramic according to claim 13 or 14, characterized in that: Its components, expressed in weight percentage, include: NiO: 0-4%; and / or Ni2O3: 0-4%; and / or CoO: 0-2%; and / or Co2O3: 0-2%; and / or Fe2O3: 0-7%; and / or MnO2: 0-4%; and / or Er2O3: 0-8%; and / or Nd2O3: 0-8%; and / or Cu2O: 0-4%; and / or Pr2O3: 0-8%; and / or CeO2: 0-4%.

25. A glass ceramic formed body, characterized in that: Contains the glass ceramic according to any one of claims 13 to 24.

26. A glass cover plate, characterized in that: A glass ceramic product comprising any one of claims 1 to 12, and / or a glass ceramic according to any one of claims 13 to 24, and / or a glass ceramic formed body according to claim 25.

27. A glass component, characterized in that: A glass ceramic product comprising any one of claims 1 to 12, and / or a glass ceramic according to any one of claims 13 to 24, and / or a glass ceramic formed body according to claim 25.

28. An electronic device, characterized in that A glass ceramic product comprising any one of claims 1 to 12, and / or a glass ceramic according to any one of claims 13 to 24, and / or a glass ceramic formed body according to claim 25, and / or a glass cover plate according to claim 26, and / or a glass component according to claim 27.

29. A display device, characterized in that A glass ceramic product comprising any one of claims 1 to 12, and / or a glass ceramic according to any one of claims 13 to 24, and / or a glass ceramic formed body according to claim 25, and / or a glass cover plate according to claim 26, and / or a glass component according to claim 27.

30. The method for manufacturing a glass ceramic product according to any one of claims 1 to 12, characterized in that: The method comprises the following steps: forming a matrix glass, subjecting the matrix glass to a crystallization process to form a glass ceramic, and then subjecting the glass ceramic to a chemical strengthening process to form a glass ceramic product.

31. The method for manufacturing a glass ceramic product according to claim 30, characterized in that: The forming of the matrix glass comprises the following steps: The raw materials are mixed uniformly according to the component ratio, then put into a crucible, and melted in an electric furnace or a gas furnace at a temperature range of 1350 to 1550° C. for 5 to 24 hours, preferably at a melting temperature of 1450 to 1550° C., and then clarified, homogenized, formed, and annealed to obtain a matrix glass, wherein the clarification temperature is greater than 1550° C. but less than or equal to 1650° C., and the annealing temperature is 450 to 600° C.

32. The method for manufacturing a glass ceramic product according to claim 30, characterized in that: The crystallization process includes the following steps: heating to a prescribed crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down. The crystallization treatment temperature is 600-800°C, preferably 650-750°C, and the holding time at the crystallization treatment temperature is 1-10 hours, preferably 3-6 hours.

33. The method for manufacturing a glass ceramic product according to claim 30, characterized in that: The crystallization process includes the following steps: performing a nucleation process at a first temperature, and then performing a crystal growth process at a second temperature.

34. The method for manufacturing a glass ceramic product according to claim 33, characterized in that: The crystallization process includes: a first temperature of 600-700° C., a second temperature of greater than 700° C. but less than or equal to 800° C., a holding time of 1-6 hours at the first temperature, and a holding time of 2-5 hours at the second temperature.

35. The method for manufacturing a glass ceramic product according to claim 30, characterized in that: The chemical strengthening process includes: immersing the glass ceramic in a salt bath of molten Na salt at 350-470°C for 1-36 hours, preferably in a temperature range of 400-460°C, and preferably in a time range of 2-15 hours; and / or immersing the glass ceramic in a mixed salt bath of molten K salt and Na salt at 360-450°C for 1-36 hours, preferably in a time range of 2-24 hours.

36. The method for producing a glass ceramic according to any one of claims 13 to 24, characterized in that: The method comprises the following steps: forming a matrix glass, and then forming a glass ceramic by a crystallization process of the matrix glass.

37. The method for manufacturing glass ceramics according to claim 36, characterized in that: The forming of the matrix glass comprises the following steps: The raw materials are mixed uniformly according to the component ratio, then put into a crucible, and melted in an electric furnace or a gas furnace at a temperature range of 1350 to 1550° C. for 5 to 24 hours, preferably at a melting temperature of 1450 to 1550° C., and then clarified, homogenized, formed, and annealed to obtain a matrix glass, wherein the clarification temperature is greater than 1550° C. but less than or equal to 1650° C., and the annealing temperature is 450 to 600° C.

38. The method for manufacturing glass ceramics according to claim 36, characterized in that: The crystallization process includes the following steps: heating to a prescribed crystallization treatment temperature, maintaining the temperature for a certain period of time after reaching the crystallization treatment temperature, and then cooling down. The crystallization treatment temperature is 600-800°C, preferably 650-750°C, and the holding time at the crystallization treatment temperature is 1-10 hours, preferably 3-6 hours.

39. The method for manufacturing a glass ceramic product according to claim 36, characterized in that: The crystallization process includes the following steps: performing a nucleation process at a first temperature, and then performing a crystal growth process at a second temperature.

40. The method for manufacturing a glass ceramic product according to claim 39, characterized in that: The crystallization process includes: a first temperature of 600-700° C., a second temperature of greater than 700° C. but less than or equal to 800° C., a holding time of 1-6 hours at the first temperature, and a holding time of 2-5 hours at the second temperature.

41. The method for producing a glass ceramic formed body according to claim 25, characterized in that: The method comprises grinding or polishing the glass ceramic to form a glass ceramic formed body, or subjecting the matrix glass or glass ceramic to a heat bending process or a press molding process at a certain temperature to form a glass ceramic formed body.

42. The method for manufacturing a glass ceramic formed body according to claim 41, characterized in that: The method comprises the following steps: subjecting the matrix glass to a crystallization heat treatment process, including heating, heat preservation nucleation, heating, heat preservation crystallization, and cooling to room temperature to form pre-crystallized glass; and subjecting the pre-crystallized glass to heat processing and molding to obtain a glass ceramic formed body.

43. The method for manufacturing a glass ceramic formed body according to claim 41, characterized in that: The method comprises the following steps: 1) Heating and preheating: Place the matrix glass or pre-crystallized glass or glass ceramic in the mold. The mold passes through each heating station in the hot bending machine in turn and stays at each station for a certain period of time to keep warm. The temperature in the preheating zone is 400-800°C, the pressure is 0.01-0.05MPa, and the time is 40-200s; 2) Pressurized molding: After preheating, the mold is transferred to the molding station. The hot bending machine applies a certain pressure to the mold. The pressure range is 0.1-0.8Mpa. The temperature range of the molding station is 600-850℃, and the molding time range is 40-200s. 3) Maintaining pressure and cooling: The mold is transferred to the cooling station for cooling step by step. The cooling temperature range is 750-500°C, the pressure is 0.01-0.05Mpa, and the time is 40-200s.

Citation Information

Patent Citations

  • Crystallized glass substrate for information recording medium and method of producing the same

    CN101905952A

  • Microcrystalline glass, microcrystalline glass product and manufacturing method thereof

    CN111807705A

  • Glass ceramics and glass ceramic articles having spinel crystalline phases

    CN111908793A

  • Glass ceramic, glass ceramic product and manufacturing method thereof

    CN114907014A

  • Tempered glass, microcrystalline glass and preparation method and application thereof

    CN115286251A

Cited By

  • Window glass for aerospace and preparation method thereof

    CN119930145A