Glass frit composition and conductive paste composition comprising same
By using a first glass powder composed of bismuth oxide and zinc oxide and a second glass powder composition composed of lead oxide, the problem of poor weather resistance of high-lead system glass powder in solar cells is solved, and high photoelectric conversion efficiency is achieved And acetic acid resistance, reducing the efficiency decay rate.
Patent Information
- Application Number
- CN202310477592.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-28
- Publication Date
- 2024-10-29
AI Technical Summary
After the existing high-lead system glass powder is used in solar cells, it easily reacts with acetic acid, resulting in poor weather resistance and efficiency attenuation. Reducing the amount of lead will lead to increased corrosion of the glass on the silicon base, resulting in loss of open circuit voltage and efficiency.
A composition is used that includes a first glass powder that is substantially free of lead and a second glass powder that is high in lead. The first glass powder contains 50-80 mol% of bismuth oxide and 20-40 mol% of zinc oxide. The second glass powder is The powder contains at least 25 mol% lead oxide, which is used to reduce the lead content in the conductive slurry, and uses high-lead glass powder to open the passivation film during the high-temperature metallization process to reduce corrosion of the passivation film layer.
It achieves high solar photoelectric conversion efficiency and excellent acetic acid resistance, reduces the efficiency attenuation rate, and improves the long-term reliability of solar cells.
Smart Images

Figure BDA0004206027570000181
Abstract
Description
Technical Field
[0001] The present invention relates to a glass powder composition comprising a first glass powder and a second glass powder, a conductive paste composition comprising the glass powder composition, and a solar cell comprising an electrode formed by curing the conductive paste composition of the present invention. The present invention also relates to use of the glass powder composition or the conductive paste composition in acetic acid resistance. Background Art
[0002] The existing glass powder used for silver-aluminum paste is usually a high-lead system glass powder. The high-lead system glass powder is used to open the passivation film so that aluminum and silicon form contact. In the silver-aluminum paste used on the front of general N-type solar cells, due to the use of high lead oxide and aluminum powder in the glass powder, the acetic acid produced by the EVA (ethylene-vinyl acetate) film used in the downstream photovoltaic modules after encountering water vapor easily reacts with lead oxide and aluminum, resulting in poor weather resistance of the modules and large efficiency attenuation. The current commercial high-efficiency N-type silver-aluminum paste products have a large efficiency attenuation after the recognized acetic acid test, which cannot meet the long-term reliability requirements of solar cell modules; while acetic acid-resistant silver-aluminum paste products reduce the amount of lead, while causing increased corrosion of glass to the silicon base, resulting in loss of open circuit voltage and efficiency.
[0003] Therefore, developing new glass powder compositions to improve acetic acid resistance and reduce efficiency attenuation has become an urgent problem to be solved by those skilled in the art. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention provides a glass powder composition comprising a first glass powder (substantially free of lead) and a second glass powder (high in lead). In the application of solar cells, the glass powder composition reduces the lead content in the conductive paste, and during the high-temperature metallization process of the solar cell, a portion of the high-lead glass flows first to open the passivation film to achieve contact, and the other portion flows later, inhibiting the flow of the glass body and reducing the corrosion of the passivation film layer, thereby ultimately achieving high solar photovoltaic conversion efficiency and excellent acetic acid resistance.
[0005] In one aspect of the present invention, the present invention relates to a glass powder composition comprising
[0006] (i) a first glass powder, wherein the first glass powder is substantially lead-free, and the first glass powder comprises:
[0007] 50-80 mol% bismuth oxide,
[0008] 20-40 mol% zinc oxide, and
[0009] 1-10 mol% antimony oxide,
[0010] in each case based on the total amount of the first glass frit; and
[0011] (ii) a second glass frit, wherein the second glass frit comprises at least 25 mol % of lead oxide based on the total amount of the second glass frit.
[0012] In another aspect of the present invention, the present invention relates to a conductive paste composition comprising the glass frit composition according to the present invention.
[0013] In another aspect of the present invention, the present invention relates to a solar cell, comprising a substrate and an electrode bonded to the substrate and formed by curing the conductive paste composition of the present invention.
[0014] In another aspect of the present invention, the present invention relates to use of the glass powder composition according to the present invention, or the conductive paste composition according to the present invention in resisting acetic acid. DETAILED DESCRIPTION
[0015] Glass powder composition
[0016] The present invention relates to a glass powder composition comprising
[0017] (i) a first glass powder, wherein the first glass powder is substantially lead-free, and the first glass powder comprises:
[0018] 50-80 mol% bismuth oxide,
[0019] 20-40 mol% zinc oxide, and
[0020] 1-10 mol% antimony oxide,
[0021] in each case based on the total amount of the first glass frit; and
[0022] (ii) a second glass frit, wherein the second glass frit comprises at least 25 mol % of lead oxide based on the total amount of the second glass frit.
[0023] In one embodiment of the present invention, the glass powder composition has a particle size d50 of 0.1-5 μm (e.g., 0.2 μm, 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm or 4.5 μm), preferably 0.2-3 μm or 0.5-2 μm.
[0024] Particle size is a well-known particle property by those skilled in the art. Particle size d50 is the median particle size or middle value of the particle size distribution. It is the particle size value at the 50% position in the cumulative distribution.
[0025] Particle size distribution may be measured via laser diffraction, dynamic light scattering, imaging, electrophoretic light scattering, or any other method known in the art.
[0026] According to the present invention, the glass powder composition of the present invention is used for silver-aluminum paste, preferably for silver-aluminum paste for N-type solar cells, especially for silver-aluminum paste for the front side of N-type solar cells.
[0027] First glass powder
[0028] In the first glass frit, the amount of the bismuth oxide is 50-80 mol %, preferably 55-75 mol % or 60-75 mol %, based on the total amount of the first glass frit.
[0029] In the first glass powder, the amount of the zinc oxide is 20-40 mol %, preferably 22-35 mol %, based on the total amount of the first glass powder.
[0030] In the first glass frit, the amount of the antimony oxide is 1-10 mol %, preferably 2-8 mol %, based on the total amount of the first glass frit.
[0031] In one embodiment of the present invention, the first glass powder comprises:
[0032] 55-75 mol% bismuth oxide,
[0033] 22-35 mol% zinc oxide, and
[0034] 2-8mol% antimony oxide,
[0035] In each case based on the total amount of the first glass frit.
[0036] According to the present invention, the bismuth oxide is Bi 2 O 3 The antimony oxide is Sb 2 O 3 .
[0037] In one embodiment of the present invention, the particle size d50 of the first glass powder is 0.1-5 μm (for example, 0.2 μm, 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm or 4.5 μm), preferably a particle size d50 of 0.2-3 μm or 0.5-2 μm.
[0038] As used herein, the term “substantially lead-free” generally means that the lead content does not exceed 0.5 mol %, or does not exceed 0.4 mol %, 0.3 mol %, 0.2 mol %, 0.1 mol %, 0.05 mol %, 0.01 mol %, based on the total amount of glass powder.
[0039] Second glass powder
[0040] In one embodiment of the present invention, the second glass powder contains at least 25 mol % of lead oxide, preferably 25-80 mol %, or 30-70 mol %, or 35-60 mol %, or 40-50 mol % of lead oxide, based on the total amount of the second glass powder.
[0041] In one embodiment, the second glass powder comprises one or more of silicon oxide, zinc oxide, boron oxide, calcium carbonate and aluminum oxide.
[0042] In one embodiment of the present invention, the second glass powder contains silicon oxide, and the amount of silicon oxide may be 5-15 mol % based on the total amount of the second glass powder.
[0043] In one embodiment of the present invention, the second glass powder contains zinc oxide, and the amount of zinc oxide may be 15-20 mol %, based on the total amount of the second glass powder.
[0044] In one embodiment of the present invention, the second glass powder contains boron oxide. The amount of boron oxide may be 10-30 mol % or 15-25 mol % based on the total amount of the second glass powder.
[0045] In one embodiment of the present invention, the second glass powder contains calcium carbonate. The amount of calcium carbonate may be 1-10 mol % or 2-8 mol %, based on the total amount of the second glass powder.
[0046] In one embodiment of the present invention, the second glass powder comprises:
[0047] at least 35 mol%, preferably 35-60 mol%, more preferably 35-60 mol% or 40-50 mol% lead oxide,
[0048] Silicon oxide,
[0049] Zinc oxide, and
[0050] Boron oxide,
[0051] In each case based on the total amount of the second glass frit.
[0052] In one embodiment of the present invention, the second glass powder comprises:
[0053] at least 35 mol%, preferably 35-60 mol%, more preferably 35-60 mol% or 40-50 mol% lead oxide,
[0054] Silicon oxide,
[0055] Zinc oxide,
[0056] Boron oxide, and
[0057] Calcium carbonate,
[0058] In each case based on the total amount of the second glass frit.
[0059] In one embodiment of the present invention, the second glass powder comprises:
[0060] at least 35 mol % lead oxide,
[0061] 5-15 mol% silicon oxide,
[0062] 15-20 mol% zinc oxide, and
[0063] 10-30 mol% boron oxide,
[0064] In each case based on the total amount of the second glass frit.
[0065] In one embodiment of the present invention, the second glass powder comprises:
[0066] 35-60 mol% lead oxide,
[0067] 5-15 mol% silicon oxide,
[0068] 15-20 mol% zinc oxide, and
[0069] 10-30 mol% boron oxide,
[0070] In each case based on the total amount of the second glass frit.
[0071] In one embodiment of the present invention, the second glass powder comprises:
[0072] 35-60 mol% lead oxide,
[0073] 5-15 mol% silicon oxide,
[0074] 15-20 mol% zinc oxide,
[0075] 10-30 mol% boron oxide, and
[0076] 1-10 mol% calcium carbonate
[0077] In each case based on the total amount of the second glass frit.
[0078] In one embodiment of the present invention, the second glass powder contains aluminum oxide. The amount of aluminum oxide may be 0-5 mol % or 0.5-3 mol %, based on the total amount of the second glass powder.
[0079] In one embodiment of the present invention, the second glass powder comprises:
[0080] 35-60 mol% lead oxide,
[0081] 5-15 mol% silicon oxide,
[0082] 15-20 mol% zinc oxide,
[0083] 10-30 mol% boron oxide,
[0084] 1-10 mol% calcium carbonate, and
[0085] 0-5 mol% alumina,
[0086] In each case based on the total amount of the second glass frit.
[0087] In one embodiment of the present invention, the second glass powder comprises:
[0088] 40-50 mol% lead oxide,
[0089] 5-15 mol% silicon oxide,
[0090] 15-20 mol% zinc oxide,
[0091] 10-30 mol% boron oxide,
[0092] 1-10 mol% calcium carbonate, and
[0093] 0-5 mol% alumina,
[0094] In each case based on the total amount of the second glass frit.
[0095] In one embodiment of the present invention, the second glass powder comprises:
[0096] 40-50 mol% lead oxide,
[0097] 5-15 mol% silicon oxide,
[0098] 15-20 mol% zinc oxide,
[0099] 10-30 mol% boron oxide,
[0100] 1-10 mol% calcium carbonate, and
[0101] 0.5-3 mol% alumina,
[0102] In each case based on the total amount of the second glass frit.
[0103] According to the present invention, the lead oxide is lead oxide (PbO). Boron oxide is B 2 O 3 . Alumina is Al 2 O 3 .
[0104] In one embodiment of the present invention, the second glass powder has a particle size d50 of 0.1-5 μm (e.g., 0.2 μm, 0.5 μm, 0.8 μm, 1 μm, 1.2 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 3.5 μm, 4 μm or 4.5 μm), preferably 0.2-3 μm or 0.5-2 μm.
[0105] In one embodiment of the present invention, the weight ratio of the first glass powder to the second glass powder is 1:10-10:1, or 1:8-8:1, or 1:6-6:1, or 1:10-1:1, 1:8-1:1, 1:5-1:1 or 1:8-1:2.
[0106] Conductive paste composition
[0107] One aspect of the present invention relates to a conductive paste composition, which includes the glass frit composition according to the present invention.
[0108] In one embodiment of the present invention, the conductive paste composition comprises:
[0109] Silver powder,
[0110] Aluminum powder,
[0111] The glass powder composition according to the present invention, and
[0112] Organic carrier.
[0113] Silver powder and aluminum powder
[0114] The conductive paste composition of the present invention may include 75-92 wt %, preferably 78-91 wt % or 80-90 wt % of silver powder, based on the total weight of the conductive paste composition.
[0115] The conductive paste composition of the present invention may include 0.6-5 wt %, preferably 0.7-4.5 wt % or 0.8-4 wt % or 1-3 wt % of aluminum powder.
[0116] The particle size d50 of the silver powder and the aluminum powder may be 0.1-3 μm, preferably 0.1-1.5 μm or 0.1-1 μm.
[0117] In one embodiment, the conductive paste composition is a silver-aluminum paste for N-type solar cells.
[0118] Amount of glass powder composition
[0119] The conductive paste composition of the present invention may include 2-15 wt %, preferably 2.2-10 wt % or 2.5-8 wt % of the glass frit composition according to the present invention, based on the total weight of the conductive paste composition.
[0120] In one embodiment, the conductive paste composition of the present invention may include 0.1-5 wt %, preferably 0.15-4 wt % or 0.18-3 wt % or 0.2-2.5 wt % of the first glass powder according to the present invention, based on the total weight of the conductive paste composition.
[0121] In one embodiment, the conductive paste composition of the present invention may include 1-10 wt %, preferably 1.2-8 wt % or 1.8-6 wt % of the second glass frit, based on the total weight of the conductive paste composition.
[0122] In the conductive paste composition, the weight ratio of the first glass powder to the second glass powder may be 1:10-10:1, or 1:6-6:1, or 1:10-1:1, or 1:8-1:2, or other weight ratios mentioned for the glass powder composition.
[0123] Organic carrier
[0124] The preferred organic vehicle in the present invention is a solution, emulsion or dispersant based on one or more solvents (preferably organic solvents) which ensures that the components of the conductive paste are present in dissolved, emulsified or dispersed form. The preferred organic vehicle is an organic vehicle that provides optimal stability of the components within the conductive paste and imparts viscosity to the conductive paste that allows effective printability.
[0125] In one embodiment, the amount of the organic vehicle may be 2-20 wt %, more preferably 3-15 wt %, most preferably 5-10 wt %, based on the total weight of the conductive paste composition.
[0126] In one embodiment, the organic vehicle comprises an organic solvent, a binder (eg, a polymer, a resin), a surfactant, or a thixotropic agent, or any combination thereof. For example, in one embodiment, the organic vehicle comprises one or more binders in an organic solvent.
[0127] The binder may be present in an amount of 0.1-10 wt %, preferably 0.1-8 wt %, more preferably 0.5-7 wt %, based on the total weight of the organic vehicle. Preferred binders in the present invention are binders that promote the formation of conductive pastes with favorable stability, printability, viscosity and sintering properties. Preferred binders according to the present invention (which generally belong to the category referred to as "resins") are polymeric binders, monomeric binders and binders that are combinations of polymers and monomers. The polymeric binder may also be a copolymer.
[0128] Preferred polymeric binders include binders carrying functional groups in the polymer backbone, binders carrying functional groups outside the backbone, and binders carrying functional groups inside and outside the backbone. Preferred polymers carrying functional groups in the backbone include, for example, polyesters, substituted polyesters, polycarbonates, substituted polycarbonates, polymers carrying cyclic groups in the backbone, polysaccharides, substituted polysaccharides, polyurethanes, substituted polyurethanes, polyamides, substituted polyamides, phenolic resins, substituted phenolic resins, copolymers of monomers of one or more previous polymers (optionally, with other comonomers) or a combination of at least two thereof. According to one embodiment, the binder may be polyvinyl butyral or polyethylene.
[0129] Preferred polymers carrying cyclic groups in the main chain include, for example, polyvinyl butyral (PVB) and its derivatives and polypinene and its derivatives or mixtures thereof. Preferred polysaccharides include, for example, ethyl cellulose, cellulose and its alkyl derivatives, methyl cellulose, hydroxyethyl cellulose, propyl cellulose, hydroxypropyl cellulose, butyl cellulose, its derivatives and mixtures of at least two thereof. Other preferred polymers include, for example, cellulose ester resins, such as cellulose acetate propionate, cellulose acetate butyrate and any combination thereof. Other preferred polymers are cellulose ester resins, such as cellulose acetate propionate, cellulose acetate butyrate and mixtures thereof, preferably those disclosed in U.S. Patent Application Publication No. 2013 / 0180583, which is incorporated herein by reference.
[0130] Preferred polymers carrying functional groups outside the polymer backbone are polymers carrying amide groups, polymers carrying acid and / or ester groups (commonly referred to as acrylic resins) or polymers carrying combinations of the above functional groups or combinations thereof. Preferred polymers carrying amides outside the backbone include, for example, polyvinyl pyrrolidone (PVP) and its derivatives. Preferred polymers carrying acid and / or ester groups outside the backbone include, for example, polyacrylic acid and its derivatives, polymethacrylate (PMA) and its derivatives, polymethyl methacrylate (PMMA) and its derivatives or mixtures thereof.
[0131] Preferred monomeric binders according to the present invention include, for example, monomers based on ethylene glycol, pine resins or rosin derivatives or mixtures thereof. Preferred monomeric binders based on ethylene glycol are binders with multiple ether groups, multiple ester groups or binders with one ether group and one ester group, preferably the ether groups are methyl, ethyl, propyl, butyl, amyl, hexyl and higher alkyl ethers, preferably the ester groups are acetates and their alkyl derivatives, preferably ethylene glycol monobutyl ether monoacetate or mixtures thereof. Alkylcellulose (preferably ethylcellulose), its derivatives and mixtures thereof with other binders from the previous binder list or others are the most preferred binders in the present invention.
[0132] The amount of the organic solvent may be 40-90 wt%, more preferably 35-85 wt%, based on the total weight of the organic vehicle.
[0133] Preferred solvents according to the present invention are solvents that allow the formation of conductive pastes with favorable viscosity, printability, stability and sintering characteristics. All solvents known in the art and considered suitable in the present invention can be used as solvents in the organic vehicle. According to the present invention, preferred solvents are solvents that allow the preferred high level of printability of the conductive paste as described above to be achieved. Preferred solvents according to the present invention are solvents that exist in liquid form at standard ambient temperature and pressure (SATP) (298.15K, 25°C, 77°F), 100kPa (14.504psi, 0.986atm), preferably solvents having a boiling point above about 90°C and a melting point above about -20°C.
[0134] Preferred solvents according to the invention are polar or nonpolar, protic or aprotic, aromatic or nonaromatic. Preferred solvents according to the invention include, for example, monoalcohols, diols, polyalcohols, monoesters, diesters, polyesters, monoethers, diethers, polyethers, solvents comprising at least one or more of these classes of functional groups, optionally comprising other classes of functional groups, preferably cyclic groups, aromatic groups, unsaturated bonds, alcohol groups having one or more O atoms substituted by heteroatoms, ether groups having one or more O atoms substituted by heteroatoms, ester groups having one or more O atoms substituted by heteroatoms, and mixtures of two or more of the above solvents.
[0135] The organic vehicle may further include a surfactant and / or an additive. The amount of the surfactant may be 0-10wt%, preferably 0-8wt%, more preferably about 0.01-6wt%, based on the total weight of the organic vehicle. The preferred surfactant in the present invention is a surfactant that promotes the formation of a conductive paste with favorable stability, printability, viscosity and sintering properties. All surfactants known in the art and considered to be applicable in the present invention may be used as surfactants in the organic vehicle. The preferred surfactant in the present invention is a surfactant based on a linear, branched, aromatic, fluorinated, siloxane, polyether chain and a combination thereof. The preferred surfactant is a single chain, a double chain or a polychain. The preferred surfactant according to the present invention may have a nonionic, anionic, cationic, amphoteric or zwitterionic head. The preferred surfactant is polymeric and monomeric or a mixture thereof.
[0136] Preferred additives in the organic vehicle are those additives that are different from the above vehicle components and promote the favorable properties of the conductive paste (such as favorable viscosity and adhesion to the underlying substrate). Additives known in the art and considered suitable for use in the present invention can be used as additives in the organic vehicle. Preferred additives according to the present invention are thixotropic agents, viscosity regulators, stabilizers, inorganic additives, thickeners, emulsifiers, dispersants, slip agents or pH regulators and any combination thereof. Preferred thixotropic agents herein are carboxylic acid derivatives, preferably fatty acid derivatives or combinations thereof. Preferred fatty acid derivatives are C 9 H 19 COOH (decanoic acid), C 11 H 23 COOH (lauric acid), C 13 H 27 COOH (myristic acid), C 15 H 31 COOH (palmitic acid), C 17 H 35 COOH(stearic acid), C 18 H 34 O 2 (oleic acid), C 18 H 32 O 2 (linoleic acid) or a combination thereof. A preferred combination of fatty acids in this context is castor oil.
[0137] additive
[0138] Preferred additives in the present invention are ingredients added to the conductive paste in addition to other ingredients explicitly mentioned, which promote higher performance of the conductive paste, the electrode made therefrom or the resulting solar cell. All additives known in the art and considered suitable in the present invention can be used as additives in the conductive paste. In addition to additives present in the glass powder and in the carrier, additives may also be present in the conductive paste. Preferred additives according to the present invention are thixotropic agents, viscosity regulators, emulsifiers, stabilizers or pH regulators, inorganic additives (such as silicon powder), thickeners and dispersants or a combination of at least two thereof, and inorganic additives are most preferred. Preferred inorganic additives according to the present invention are Mg, Ni, Te, W, Zn, Mg, Gd, Ce, Zr, Ti, Mn, Sn, Ru, Co, Fe, Cu and Cr or a combination of at least two thereof, preferably Zn, Sb, Mn, Ni, W, Te and Ru or a combination of at least two thereof, their oxides, compounds that can produce said metal oxides upon firing, or a mixture of at least two of the above metals, a mixture of at least two of the above oxides, a mixture of at least two of the above compounds that can produce said metal oxides upon firing, or a mixture of two or more of any of the above materials.
[0139] The amount of the inorganic additive may be 0-1 wt % (eg, 0.1 wt %, 0.5 wt % or 0.8 wt %) based on the total weight of the conductive paste composition.
[0140] In one embodiment, the conductive paste composition of the present invention comprises:
[0141] 75-92wt% silver powder,
[0142] 0.6-5wt% aluminum powder,
[0143] 2-15 wt% of the glass powder composition according to the present invention, and
[0144] 2-20wt% organic carrier,
[0145] In each case this is based on the total weight of the electroconductive paste composition.
[0146] In the conductive paste composition, the weight ratio of the first glass powder to the second glass powder may be 1:10-10:1, or 1:6-6:1, or 1:10-1:1, or other weight ratios mentioned for the glass powder composition.
[0147] In one embodiment, the conductive paste composition of the present invention comprises:
[0148] 78-91wt% silver powder,
[0149] 0.7-4.5wt% aluminum powder,
[0150] 2.2-10 wt% of the glass powder composition according to the present invention, and
[0151] 3-15wt% organic carrier,
[0152] In each case this is based on the total weight of the electroconductive paste composition.
[0153] In the conductive paste composition, the weight ratio of the first glass powder to the second glass powder may be 1:10-10:1, or 1:6-6:1, or 1:10-1:1, or other weight ratios mentioned for the glass powder composition.
[0154] In one embodiment, the conductive paste composition of the present invention comprises:
[0155] 80-90wt% silver powder,
[0156] 1-3wt% aluminum powder,
[0157] 2.5-8 wt % of the glass powder composition according to the present invention, and
[0158] 5-10wt% organic carrier,
[0159] In each case this is based on the total weight of the electroconductive paste composition.
[0160] In the conductive paste composition, the weight ratio of the first glass powder to the second glass powder may be 1:10-10:1, or 1:6-6:1, or 1:10-1:1, or other weight ratios mentioned for the glass powder composition.
[0161] In one embodiment, the conductive paste composition of the present invention comprises:
[0162] 75-92wt% silver powder,
[0163] 0.6-5wt% aluminum powder,
[0164] 2-15 wt% of the glass powder composition according to the present invention,
[0165] 2-20 wt% organic carrier, and
[0166] 0-1wt% inorganic additives,
[0167] In each case this is based on the total weight of the electroconductive paste composition.
[0168] In one embodiment, the conductive paste composition of the present invention comprises:
[0169] 80-90wt% silver powder,
[0170] 1-3wt% aluminum powder,
[0171] 2.5-8wt% of the glass powder composition according to the present invention,
[0172] 5-10 wt% organic carrier, and
[0173] 0-1wt% inorganic additives,
[0174] In each case this is based on the total weight of the electroconductive paste composition.
[0175] In one embodiment, the conductive paste composition of the present invention comprises:
[0176] 75-92wt% silver powder,
[0177] 0.6-5wt% aluminum powder,
[0178] 0.1-5wt% first glass powder,
[0179] 1-10wt% second glass powder,
[0180] 2-20 wt% organic carrier, and
[0181] 0-1wt% inorganic additives,
[0182] In each case this is based on the total weight of the electroconductive paste composition.
[0183] In one embodiment, the conductive paste composition of the present invention comprises:
[0184] 80-90wt% silver powder,
[0185] 1-3wt% aluminum powder,
[0186] 0.2-2wt% first glass powder,
[0187] 1.8-6wt% second glass powder,
[0188] 5-10 wt% organic carrier, and
[0189] 0-1wt% inorganic additives,
[0190] In each case this is based on the total weight of the electroconductive paste composition.
[0191] Forming a conductive paste composition
[0192] To form the conductive paste composition, the glass powder material can be combined with the silver and aluminum powders and the organic vehicle and optional additives using any method known in the art for preparing a paste composition. The preparation method is not critical as long as it produces a homogeneously dispersed paste. The components can be mixed, such as with a mixer, and then passed through a three-roll mill, for example, to make a dispersed uniform paste.
[0193] Solar Cells
[0194] One aspect of the present invention relates to a solar cell, which comprises a substrate and an electrode bonded to the substrate and formed by curing the conductive paste composition of the present invention.
[0195] In other areas of the solar cell, the substrate of the present invention, preferably a silicon wafer, has a region that can efficiently absorb light to generate electron-hole pairs and efficiently separate holes and electrons across a boundary, preferably across a pn junction boundary.
[0196] The pn junction boundary is located where the front doped layer of the wafer meets the back doped layer. In an n-type solar cell, the back doped layer is doped with an electron-donating n-type dopant and the front doped layer is doped with an electron-withdrawing or hole-donating p-type dopant. In a p-type solar cell, the back doped layer is doped with a p-type dopant and the front doped layer is doped with an n-type dopant. According to a preferred embodiment of the present invention, a wafer having a pn junction boundary is prepared by first providing a doped silicon substrate and then applying a doped layer of the opposite type to one face of the substrate.
[0197] Dopant
[0198] Preferred dopants are dopants that form pn junction boundaries by introducing electrons or holes into the band structure when added to the silicon wafer. It is preferred according to the present invention to specifically select the types and concentrations of these dopants to adjust the band structure profile of the pn junction and set the light absorptivity and conductivity profile as required. Preferred p-type dopants according to the present invention are dopants that add holes to the band structure of the silicon wafer. All dopants known in the art and considered suitable in the present invention can be used as p-type dopants. Preferred p-type dopants according to the present invention are trivalent elements, especially trivalent elements of Group 13 in the periodic table. Preferred Group 13 elements in the periodic table herein include, but are not limited to, B, Al, Ga, In, Tl or a combination of at least two thereof, wherein B is particularly preferred.
[0199] Preferred n-type dopants according to the present invention are dopants that add electrons to the band structure of the silicon wafer. All dopants known in the art and considered suitable in the present invention can be used as n-type dopants. Preferred n-type dopants according to the present invention are elements of the fifth group of the periodic table. Preferred elements of the fifth group of the periodic table herein include N, P, As, Sb, Bi or a combination of at least two thereof, wherein P is particularly preferred.
[0200] Solar cell structure
[0201] A preferred solar cell according to the present invention is a solar cell with high efficiency in terms of the ratio of the total energy of incident light converted to electrical energy output. Lightweight and durable solar cells are also preferred. At a minimum, the solar cell comprises: (i) a front electrode, (ii) a front doped layer, (iii) a pn junction boundary, (iv) a back doped layer and (v) a back electrode and a passivation layer. The solar cell may also include additional layers for chemical / mechanical protection.
[0202] Anti-reflective layer
[0203] According to the present invention, an antireflection layer may be applied as an outer layer before the electrode is applied to the front side of the solar cell. A preferred antireflection layer according to the present invention is an antireflection layer that reduces the proportion of incident light reflected by the front side and increases the proportion of incident light that will be absorbed by the wafer across the front side. An antireflection layer that produces a favorable absorptivity / reflectivity ratio is susceptible to etching by the conductive paste, is further resistant to the temperature required for firing the conductive paste, and does not promote greater recombination of electrons and holes near the electrode interface. All antireflection layers known in the art and considered suitable in the present invention can be used. A preferred antireflection layer according to the present invention is SiN x 、SiO 2 、Al 2 O 3 、TiO 2 Or a mixture of at least two thereof and / or a combination of at least two thereof. According to a preferred embodiment, the antireflection layer is Si x N y , especially wherein a silicon wafer is employed, wherein x is approximately 2-4 and y is approximately 3-5.
[0204] Passivation layer
[0205] According to the present invention, one or more passivation layers can be applied to the substrate, preferably the front side and / or back side of the silicon wafer as the outer layer. The passivation layer can be applied before forming the front electrode or before applying the anti-reflection layer (if one of them exists). Preferably, the passivation layer is a passivation layer that reduces the electron / hole recombination rate near the electrode interface. Any passivation layer known in the art and considered to be applicable in the present invention can be used. The passivation layer according to the present invention can be silicon nitride, aluminum oxide, silicon dioxide and titanium dioxide. According to the most preferred embodiment, aluminum oxide is used. Preferably, the passivation layer has a thickness of 0.1nm to 2μm, more preferably 1nm to 1μm, and most preferably 1nm to 200nm.
[0206] Additional layer of protection
[0207] In addition to the above-mentioned layers which directly contribute to the fundamental function of the solar cell, further layers can be added for mechanical and chemical protection.
[0208] The battery can be encapsulated to provide chemical protection. Encapsulation is well known in the art and any encapsulation suitable for the present invention can be used. According to a preferred embodiment, a transparent polymer (commonly referred to as a transparent thermoplastic resin) is used as an encapsulation material, provided that such an encapsulation exists. Preferred transparent polymers herein are silicone rubber and polyethylene vinyl acetate (PVA).
[0209] A transparent glass sheet may also be added to the front side of the solar cell to provide mechanical protection to the front side of the cell.Transparent glass sheets are well known in the art and any transparent glass sheet suitable for use in the present invention may be employed.
[0210] A backside protection material may be added to the back side of the solar cell to provide mechanical protection. Backside protection materials are well known in the art and any backside protection material deemed suitable in the present invention may be used. A preferred backside protection material according to the present invention is a backside protection material having good mechanical properties and weatherability. A preferred backside protection material according to the present invention is polyethylene terephthalate with a polyvinyl fluoride layer. It is preferred according to the present invention that the backside protection material is present below the encapsulation layer (in the case where a backside protection layer and encapsulation are present).
[0211] Frame materials may be added to the outside of the solar cell to impart mechanical support. Frame materials are well known in the art and any frame material deemed suitable for use in the present invention may be employed. A preferred frame structure according to the present invention is aluminum.
[0212] Method for preparing solar cell
[0213] Electrodes can be formed by applying the conductive paste composition of the present invention to a substrate, such as a semiconductor substrate (such as a silicon wafer). The conductive paste can be applied in any manner known in the art and considered suitable in the present invention. Examples include, but are not limited to, dipping, impregnation, pouring, dripping, injection, spraying, blade coating, shower coating, brush coating or printing or a combination of at least two thereof. Preferably, the printing technique is inkjet printing, screen printing, flexographic printing, offset printing, relief printing or stencil printing or a combination of at least two thereof. According to the present invention, it is preferred to apply the conductive paste by printing, preferably by screen printing.
[0214] Firing is required to sinter the printed electrodes to form a solid conductor. Firing is well known in the art and may be achieved in any manner deemed appropriate in the present invention. It is preferred that firing is performed above the Tg of the glass frit material.
[0215] The present invention also relates to the glass powder composition of the present invention and the use of the conductive paste composition of the present invention in resisting acetic acid, for example, in the application of solar cells. The acetic acid is produced, for example, by the reaction of water vapor with EVA (polyethylene vinyl acetate).
[0216] Example
[0217] Example 1
[0218] (1) Preparation of the Second Glass Powder
[0219] A second glass powder comprising 47 mol% lead oxide, 9 mol% silicon oxide, 16 mol% zinc oxide, 22 mol% boron oxide, 1 mol% aluminum oxide and 5 mol% calcium carbonate is prepared, wherein the total amount is based on the second glass powder in each case. The mixed mixture is charged into an aluminum oxide crucible. The crucible is then placed in a muffle furnace and kept warm at 1000° C. for 60 minutes. The molten glass is then removed from the furnace and poured into a bucket containing deionized water for water quenching. The water-quenched glass slag is ground into a glass powder with a d50 of 1.5 μm using a ball mill. After grinding, the glass powder is filtered through a 325 mesh sieve and dried at 125° C. for 12 hours to obtain a second glass powder.
[0220] (2) Preparation of the first glass powder
[0221] A first glass frit including 70 mol % bismuth oxide, 25 mol % zinc oxide and 5 mol % antimony oxide, in each case based on the total amount of the first glass frit, was prepared in the same procedure as above for the preparation of the second glass frit.
[0222] (3) Preparation of solar cells
[0223] The silver-aluminum paste used to prepare solar cells has the following composition: 85wt% silver powder (d50: 2μm), 1.5wt% aluminum powder (d50: 2μm), 2wt% first glass powder, 3wt% second glass powder, 0.5wt% silicon powder (inorganic additive), 5.6wt% organic solvent, 0.6wt% resin, 0.6wt% organic dispersant, 0.6wt% thixotropic agent, and 0.6wt% lubricant. The above ingredients are mixed and ground with a three-roll mill to a uniform consistency to obtain a silver-aluminum paste for N-type solar cells, and printed on the front of an N-type TOPCon silicon wafer using a 15um knotless screen, and the electrical properties are tested after sintering.
[0224] Comparative Example 1
[0225] The preparation of the solar cell of Example 1 was repeated, except that the commercial slurry 1 was used.
[0226] Comparative Example 2
[0227] The preparation of the solar cell of Example 1 was repeated, except that the commercial paste 2 was used.
[0228] Performance Testing
[0229] The performance of the solar cells was tested using the IV test method using a commercial IV-tester "cetisPV-Celltest4-BF" from Halm Elektronik GmbH.
[0230] First measure the efficiency of the screen-printed cell, then do the acetic acid test, measure the efficiency again after the acetic acid test, and finally calculate the efficiency attenuation rate. The efficiency attenuation rate is: (Eta before the experiment - Eta after the experiment) / Eta before the experiment × 100%.
[0231] Acetic acid experiment: Add 300 ml of pure water, 180 g of potassium chloride, and 34 ml of pure acetic acid into a sealed box; place the battery cells on top of the acetic acid solution, then place the box in an 85°C oven for 4 hours, take out the battery cells and cool them to room temperature.
[0232] The electrical performance data of the embodiments and comparative examples before and after the acetic acid experiment are shown in Table 1 below:
[0233] Table 1
[0234]
[0235] Commercial pastes 1 and 2 are high-efficiency products currently on the market. Compared with the solar cell of comparative example 1 using commercial paste 1, the efficiency of the solar cell using silver-aluminum paste of Example 1 of the present invention is higher before the acetic acid test than that of the solar cell of comparative example 1 using commercial paste 1. After the acetic acid test, the efficiency attenuation rate of the solar cell of comparative example 1 is as high as 20%, while the efficiency attenuation rate of the solar cell of Example 1 of the present invention is only 5%, which is only one-fourth of that of comparative example 1.
[0236] Compared with the solar cell of comparative example 2 using commercial paste 2, the efficiency of the solar cell using silver aluminum paste of embodiment 1 of the present invention before the acetic acid test is slightly higher than that of the solar cell of comparative example 2 using commercial paste 2. After the acetic acid test, the efficiency attenuation rate of the solar cell of comparative example 2 is as high as 30%, while the efficiency attenuation rate of the solar cell of embodiment 1 of the present invention is only 5%, that is, only one sixth of that of comparative example 2.
[0237] The results show that the glass powder composition of the present invention can achieve higher efficiency than commercially available high-efficiency products, and its resistance to acetic acid is greatly improved. The efficiency attenuation rate after the acetic acid test is significantly lower than that of commercially available high-efficiency products and can achieve higher efficiency than commercially available high-efficiency products.
[0238] Although the present invention is disclosed as above with preferred embodiments, the present invention is not limited thereto. Any changes and modifications made by any person skilled in the art without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention, so the protection scope of the present invention should be based on the scope defined by the claims.
Claims
1. A glass powder composition comprising (i) a first glass powder, wherein the first glass powder is substantially lead-free, and the first glass powder comprises: 50-80 mol% bismuth oxide, 20-40 mol% zinc oxide, and 1-10 mol% antimony oxide, in each case based on the total amount of the first glass frit; and (ii) a second glass frit, wherein the second glass frit comprises at least 25 mol % of lead oxide based on the total amount of the second glass frit.
2. The glass powder composition according to claim 1, wherein the first glass powder comprises: 55-75 mol% bismuth oxide, 25-35 mol% zinc oxide, and 2-8mol% antimony oxide, In each case based on the total amount of the first glass frit.
3. The glass powder composition according to claim 1 or 2, wherein the first glass powder and the second glass powder have a particle size d50 of 0.1-5 μm, preferably a particle size d50 of 0.2-3 μm.
4. The glass frit composition according to any one of claims 1 to 3, wherein the second glass frit comprises 25-80 mol % of lead oxide, preferably 35-60 mol % or 40-50 mol % of lead oxide, based on the total amount of the second glass frit.
5. The glass powder composition according to any one of claims 1 to 4, wherein the second glass powder further comprises: One or more of silicon oxide, zinc oxide, boron oxide, calcium carbonate and aluminum oxide; In each case based on the total amount of the second glass frit.
6. The glass frit composition according to any one of claims 1 to 5, wherein the bismuth oxide is Bi2O3, the antimony oxide is Sb2O3, and the lead oxide is PbO. 7 . The glass powder composition according to claim 1 , wherein a weight ratio of the first glass powder to the second glass powder is 1:10-10:1, or 1:6-6:1, or 1:10-1:
1.
8. A conductive paste composition comprising the glass frit composition according to any one of claims 1 to 7.
9. The conductive paste composition according to claim 8, comprising: Silver powder, Aluminum powder, The glass powder composition according to any one of claims 1 to 7, and Organic carrier.
10. The conductive paste composition according to claim 9, comprising: 75-92wt% silver powder, 0.6-5wt% aluminum powder, 2-15 wt% of the glass powder composition according to any one of claims 1 to 7, and 2-20wt% organic carrier, In each case this is based on the total weight of the electroconductive paste composition.
11. A solar cell, The conductive paste comprises a substrate and an electrode bonded to the substrate and formed by curing the conductive paste composition according to any one of claims 8 to 10.
12. Use of the glass powder composition according to any one of claims 1 to 7, or the conductive paste composition according to any one of claims 8 to 10 in resisting acetic acid.