Preparation method of graphene-Fe coated hollow and / or porous microspheres with self-assembly structure

Through self-assembled graphene-Fe-coated hollow and/or porous microspheres, the problem of limited application of existing absorbing materials in lightweight equipment is solved, and the material's efficient absorbing and heat insulation properties are achieved to meet the needs of Demand for stealth aircraft and high-energy microwave anechoic chambers.

CN118851592AActive Publication Date: 2024-10-29NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410713930.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-04
Publication Date
2024-10-29
Estimated Expiration
2044-06-04

AI Technical Summary

Technical Problem

The application of existing absorbing materials in lightweight and miniaturized electronic equipment is limited. Since it is difficult for a single dielectric loss material to achieve good impedance matching, its absorbing efficiency is limited.

Method used

The self-assembled graphene-Fe coated hollow and/or porous microspheres are coated and modified with graphene oxide and then thermally reduced to grow iron powder to form a composite material to improve impedance matching and internal loss.

Benefits of technology

It achieves excellent thermal insulation and wave-absorbing properties of the material, meets the surface absorption requirements of stealth aircraft and high-energy microwave anechoic chambers, and has low density, thermal insulation and wave-absorbing properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851592A_ABST
    Figure CN118851592A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of wave absorption and heat insulation, and relates to a preparation method of graphene-Fe coated hollow and / or porous microspheres with a self-assembly structure, and in the thermal reduction process of the graphene-Fe coated hollow and / or porous microspheres with the self-assembly structure, accumulation between graphene sheets is effectively hindered, a large number of closed-pore structures are generated in the microspheres, and the thermal reduction effect of the microspheres is improved. Electromagnetic waves can be reflected for multiple times inside, so that a good wave absorbing effect is achieved; the iron powder is synthesized on the surface of the graphene in situ, so that the dielectric loss and the magnetic loss of the material are obviously improved; and through the combined action of multiple wave absorbing mechanisms, the wave absorbing performance of the material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wave absorption and heat insulation, and relates to a method for preparing a graphene-Fe coated hollow and / or porous microsphere with a self-assembled structure. Background Art

[0002] With the development of science and technology, modern society is surrounded by a large number of electronic products and advanced communication technologies, from smart phones and tablets to various smart home devices and even widely distributed 5G base stations. The explosive growth of these technologies has brought about increasingly serious electromagnetic pollution problems.

[0003] To meet this challenge, researchers and engineers have innovatively developed absorbing materials, a high-tech product designed to alleviate electromagnetic pollution. The working principle of absorbing materials is that they can cleverly absorb harmful electromagnetic wave energy and convert it into heat or other forms of energy release, thereby effectively weakening the propagation of electromagnetic waves and reducing their impact on the surrounding environment. The two most important factors of absorbing materials are impedance matching and internal loss. Impedance matching is to allow the incident electromagnetic wave to enter the electromagnetic wave to the maximum extent and reduce reflection. Internal loss refers to the generation of more dielectric loss and magnetic loss inside the material to reduce transmission. Traditional absorbing materials include metals, metal particles, ferrites and their alloys. Due to their excellent magnetic loss characteristics, they were widely used in the early days; however, these materials usually have disadvantages such as high density (high mass), poor acid and alkali resistance and easy agglomeration, which limits their application potential in lightweight and miniaturized electronic devices. In contrast, new dielectric loss materials, such as porous carbon, conductive carbon black, graphene and carbon nanotubes, have brought innovation to the field of absorbing materials with their low weight, corrosion resistance, and excellent electrical conductivity. However, in practical applications, it is often difficult for a single dielectric loss material to independently achieve good impedance matching, which directly restricts its wave absorption efficiency. Summary of the invention

[0004] The present invention aims at the deficiencies of the absorbing materials in the prior art and provides a method for preparing a graphene-Fe coated hollow and / or porous microsphere with a self-assembled structure. The method uses the graphene coated hollow and / or porous microsphere and the reduced iron method to prepare the graphene-Fe coated hollow and / or porous microsphere with a self-assembled structure, which has excellent heat insulation and absorbing properties.

[0005] One object of the present invention is achieved by the following technical solutions:

[0006] A method for preparing a self-assembled graphene-Fe coated hollow and / or porous microsphere comprises the following steps:

[0007] Graphene oxide (GO) coated and modified hollow and / or porous microspheres;

[0008] After thermal reduction, hollow and / or porous microspheres coated with reduced graphene oxide are obtained;

[0009] The hollow and / or porous microspheres coated and modified by reduced graphene oxide are then subjected to a reduction reaction, and iron is in situ grown on the surface of the reduced graphene oxide to obtain the graphene-Fe coated hollow and / or porous microspheres with a self-assembled structure.

[0010] There is no particular limitation on the graphene oxide, and the graphene oxide may be graphene oxide with different numbers of layers, preferably graphene oxide with 3 to 30 layers.

[0011] Hollow and / or porous microspheres can be exemplified by hollow glass microspheres (HGM), hollow ceramic microspheres, hollow metal microspheres, porous carbon, and the like.

[0012] Preferably, the hollow and / or porous microspheres are hollow glass microspheres, and the particle size of the hollow glass microspheres is 5 to 500 μm and the wall thickness is 0.5 to 3 μm.

[0013] Preferably, the modified hollow and / or porous microspheres are obtained by grafting a silane coupling agent onto the hollow and / or porous microspheres.

[0014] Preferably, the modified hollow and / or porous microspheres are obtained by subjecting the hollow and / or porous microspheres to a hydroxylation treatment and then grafting a silane coupling agent thereon.

[0015] Preferably, the hollow and / or porous microspheres are placed in an alkaline solution for reaction, and after the reaction is completed, the hollow and / or porous microspheres are filtered, washed, and dried to obtain hydroxylated hollow and / or porous microspheres.

[0016] In the hydroxylation treatment step, preferably, the alkaline solution is formed by dissolving an inorganic base in water, and the inorganic base includes but is not limited to one or more of sodium hydroxide, calcium hydroxide, potassium hydroxide, lithium hydroxide, ammonium hydroxide and the like.

[0017] In the hydroxylation treatment step, preferably, the mass molar ratio of the hollow and / or porous microspheres to the base is 1 g: 0.001 to 1 mol.

[0018] In the hydroxylation step, preferably, the reaction is carried out at 45-95° C. for 0.5-10 h; more preferably, the reaction is carried out at 50-90° C. for 0.5-5 h. Still more preferably, the reaction is carried out under stirring at a stirring speed of 100-1000 r / min.

[0019] Preferably, the step of grafting the silane coupling agent comprises: adding the silane coupling agent to a solvent, adjusting the pH for hydrolysis, then adding the hollow and / or porous microspheres or the hydroxylated hollow and / or porous microspheres, reacting, and after the reaction, solid-liquid separation, washing, and drying to obtain the modified hollow and / or porous microspheres.

[0020] In the step of grafting the silane coupling agent, the silane coupling agent includes but is not limited to one or more of KH550, HK560, KH570, KH792, KH580, KH590, A-151, A-171, etc.

[0021] In the step of grafting the silane coupling agent, preferably, the solvent is a mixture of water and a polar organic solvent, and the polar organic solvent includes but is not limited to methanol, ethanol, acetone, acetonitrile, isopropanol, ethylene glycol, propylene glycol, etc. Preferably, the volume ratio of water to the polar organic solvent is 1:0.5-5.

[0022] In the step of grafting the silane coupling agent, preferably, the pH is adjusted to < 7, and more preferably, the pH is adjusted to: 5 ≤ pH ≤ 6.8. There is no special requirement for the acid solution used to adjust the pH, and any acid solution that can adjust the pH meets the requirements, such as hydrochloric acid solution, sulfuric acid solution, acetic acid solution and hypochlorous acid solution.

[0023] In the step of grafting the silane coupling agent, preferably, the hydrolysis is performed at 10 to 40° C. for 0.5 to 5 hours.

[0024] In the step of grafting the silane coupling agent, preferably, the mass ratio of the hollow and / or porous microspheres or the hydroxylated hollow and / or porous microspheres to the silane coupling agent is 1:(0.2-10).

[0025] In the step of grafting the silane coupling agent, preferably, the reaction is carried out at 45-95° C. for 0.5-10 h; more preferably, the reaction is carried out at 50-90° C. for 0.5-5 h. Still more preferably, the reaction is carried out under stirring at a stirring speed of 100-1000 r / min.

[0026] Preferably, the step of coating the modified hollow and / or porous microspheres with graphene oxide comprises: dispersing graphene oxide in water, adding the modified hollow and / or porous microspheres, reacting, and after the reaction, performing solid-liquid separation, washing, and drying to obtain the modified hollow and / or porous microspheres coated with graphene oxide.

[0027] In the step of coating the modified hollow and / or porous microspheres with graphene oxide, preferably, each gram of graphene oxide is dispersed in 10 to 1000 ml of water.

[0028] In the step of coating the modified hollow and / or porous microspheres with graphene oxide, preferably, the mass ratio of graphene oxide to the modified hollow and / or porous microspheres is 1:2-200; more preferably 1:5-100.

[0029] In the step of coating the modified hollow and / or porous microspheres with graphene oxide, preferably, the reaction is carried out at 45-95° C. for 0.5-10 h; more preferably, the reaction is carried out at 50-90° C. for 0.5-5 h. Still more preferably, the reaction is carried out under stirring at a stirring speed of 100-1000 r / min.

[0030] Preferably, the holding temperature of the thermal reduction is 200 to 400° C., more preferably 250 to 350° C.; the holding time of the thermal reduction is 20 to 100 min, more preferably 40 to 80 min.

[0031] Preferably, the temperature is increased to the heat reduction holding temperature at a rate of 5 to 15°C / min.

[0032] Preferably, the reduction reaction step comprises: placing the hollow and / or porous microspheres coated with reduced graphene oxide in a ferric salt or ferrous salt solution, and then adding a reducing agent with a higher reducing power than Fe 3+ or Fe 2+ After the reaction, let the metal powder stand, take the upper floating material, filter it, wash it and dry it.

[0033] In the step of reduction reaction, preferably, the iron salt or ferrous salt is one or more of ferric nitrate, ferrous nitrate, ferrous sulfate, ferric sulfate, ferric chloride and ferrous chloride.

[0034] In the reduction reaction step, preferably, the reducing property is higher than that of Fe 3+ or Fe 2+ The metal powder is one or more of zinc, magnesium and calcium.

[0035] In the step of reduction reaction, preferably, the mass molar ratio of the hollow and / or porous microspheres coated and modified by reduced graphene oxide to the iron salt or ferrous salt is 1 g: 0.05-1.0 mol.

[0036] In the reduction reaction step, preferably, the reducing property is higher than that of Fe 3+ or Fe 2+ The amount of metal powder added is ≥ theoretically making Fe 3+ or Fe 2+ The amount of all reduced to Fe. Theoretically here refers to the calculation based on the stoichiometric ratio, that is, the theoretical minimum amount of metal powder added is determined according to the molar ratio of each reactant to the product in the chemical reaction equation.

[0037] In the reduction reaction step, preferably, the hollow and / or porous microspheres coated with reduced graphene oxide are placed in a ferric salt or ferrous salt solution and stirred at 10 to 40° C. for 0.5 to 5 hours at a stirring speed of 100 to 800 r / min.

[0038] In the reduction reaction step, preferably, a reducing agent having a higher reducing power than Fe is added. 3+ or Fe 2+ The metal powder is stirred at 10-40°C for 0.5-5h. The stirring speed is 100-800r / min.

[0039] The solid-liquid separation methods include but are not limited to centrifugation, filtration, etc.

[0040] The drying means herein include but are not limited to vacuum drying, forced air drying, etc. Preferably, the method is vacuum drying, which is performed in a vacuum oven at 45 to 95° C. for 3 to 30 hours.

[0041] Another object of the present invention is achieved by the following technical solutions:

[0042] A graphene-Fe coated hollow and / or porous microsphere with a self-assembled structure is prepared by the above preparation method.

[0043] Compared with the prior art, the present invention has the following beneficial effects:

[0044] 1. The present invention loads graphene oxide on the hollow and / or porous microspheres through surface modification of hollow and / or porous microspheres, and then reduces the graphene oxide to rGO through high-temperature thermal reduction. Since the graphene oxide is coated on the hollow and / or porous microspheres, the accumulation between graphene sheets is effectively hindered; finally, iron powder is in situ grown on the graphene surface through a reduction reaction, and a graphene-Fe coated hollow and / or porous microsphere composite material with the characteristics of self-assembly structure and light weight is effectively prepared;

[0045] 2. The present invention first performs hydroxylation treatment on the hollow and / or porous microspheres, so that the surface of the hollow and / or porous microspheres is hydroxylated, thereby increasing the grafting amount of the silane coupling agent;

[0046] 3. The pore size of the hollow and / or porous microspheres will affect the wave absorption and thermal insulation properties of the composite material. Generally speaking, within a certain range, the smaller the pore size of the hollow and / or porous microspheres, the more times the electromagnetic waves are reflected inside, which is more conducive to improving the wave absorption performance; and the smaller the pore size, the greater the thermal resistance and the better the thermal insulation performance;

[0047] 4. The present invention synthesizes iron powder in situ on the graphene surface, which significantly improves the dielectric loss and magnetic loss of the material, promotes impedance matching on the material surface, enables more electromagnetic waves to enter the interior of the material, and improves the overall wave absorption performance; the graphene oxide coated hollow glass microspheres of the present invention effectively hinders the accumulation of graphene sheets during the thermal reduction process, generates a large number of closed-cell structures inside, and electromagnetic waves can be reflected multiple times inside, thereby achieving a good wave absorption effect; and the interior contains abundant closed-cell structures, which increases thermal resistance and has good thermal insulation performance; the material has a low density and excellent flame retardancy, and is in line with the surface absorption requirements of stealth aircraft and high-energy microwave darkrooms: low density, heat insulation and wave absorption. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is the SEM image of the self-assembled graphene-Fe coated hollow glass microspheres prepared in Example 1. DETAILED DESCRIPTION

[0049] The technical scheme of the present invention is further described below by specific examples and accompanying drawings. It should be understood that the specific examples described herein are only used to help understand the present invention and are not intended for specific limitations of the present invention. The accompanying drawings used herein are only for better illustrating the disclosure of the present invention and do not have a limiting effect on the scope of protection. If not otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0050] Example 1

[0051] The graphene-Fe coated hollow glass microspheres of the self-assembled structure of this embodiment are prepared by the following steps:

[0052] (1) Hydroxylation treatment of hollow glass microspheres

[0053] 200 ml of NaOH aqueous solution (0.5 M) and 10 g of HGM (particle size of 50 μm, wall thickness of 2 μm) were added to a 500 ml three-necked flask and stirred at 70°C and 300 r / min for 1 h. After the alkali washing was completed, the mixture was filtered, washed with water until neutral and filtered, and the hydroxylated HGM was dried in a vacuum oven at 70°C for 12 h to obtain OH-HGM.

[0054] (2) OH-HGM grafted KH550

[0055] 10g KH550 ethanol-water solution (V water: V ethanol = 1: 2) 200ml, add hydrochloric acid solution to adjust pH to 6.0 and hydrolyze at room temperature (25℃) for 2h. Then add 10g OH-HGM, stir and react at 80℃, 300r / min for 1.5h. After the reaction is completed, filter and remove excess KH550 with anhydrous ethanol, put the filter cake into a 70℃ vacuum oven and dry it for 12h to obtain KH550-HGM.

[0056] (3) Graphene oxide coated KH550-HGM

[0057] Weigh 0.4g GO and add it to 200ml deionized water, and ultrasonicate for 30min. Then add 10g KH550-HGM and stir at 80℃ and 400r / min for 1.5h. After the reaction is completed, filter, wash with water, and dry in a vacuum oven at 70℃ for 12h to obtain GO-HGM.

[0058] (4) High temperature reduction of graphene oxide

[0059] 10 g of GO-HGM was put into a crucible, and the temperature was increased to 300 °C in a muffle furnace at a heating rate of 10 °C / min and maintained for 30 min to obtain rGO-HGM.

[0060] (5) In-situ generation of iron from graphene oxide

[0061] Add 0.4 g rGO-HGM to 200 ml 1 mol / L FeCl2 solution, stir at room temperature (25°C) and 300 r / min for 2 h, slowly add 10 g zinc powder particles (excess), stir at room temperature (25°C) and 300 r / min for 2 h, let stand for 1 h, take the upper layer of rGO-Fe-HGM (floating), filter and remove ZnCl2 with anhydrous ethanol, put the filter cake into a 70°C vacuum oven and dry it for 12 h to obtain rGO-Fe-HGM.

[0062] Figure 1 This is the SEM image of the self-assembled graphene-Fe coated hollow glass microspheres prepared in Example 1. It can be seen that the surface of the microspheres is coated with graphene-Fe.

[0063] Example 2

[0064] The only difference between Example 2 and Example 1 is that the HGM used in Example 2 has a particle size of 80 μm and a wall thickness of 2 μm, and the rest is the same as Example 1.

[0065] Example 3

[0066] The only difference between Example 3 and Example 1 is that the HGM particle size used in Example 3 is 100 μm and the wall thickness is 2 μm, and the rest is the same as Example 1.

[0067] Example 4

[0068] The only difference between Example 4 and Example 1 is that the HGM used in Example 4 has a particle size of 120 μm and a wall thickness of 2 μm, and the rest is the same as Example 1.

[0069] Example 5

[0070] The only difference between Example 5 and Example 1 is that Example 5 is not subjected to hydroxylation treatment, and specifically comprises the following steps:

[0071] (1) OH-HGM grafted KH550

[0072] 10g KH550 ethanol-water solution (V water: V ethanol = 1: 2) 200ml, add hydrochloric acid solution to adjust pH to 6.0 and hydrolyze at room temperature (25℃) for 2h. Then add 10g HGM (particle size is 50μm, wall thickness is 2μm), stir and react at 80℃, 300r / min for 1.5h. After the reaction is completed, filter and remove the excess KH550 with anhydrous ethanol, put the filter cake into a 70℃ vacuum oven and dry it for 12h to obtain KH550-HGM.

[0073] The subsequent steps are the same as those in Example 1.

[0074] Example 6

[0075] The graphene-Fe coated hollow glass microspheres of the self-assembled structure of this embodiment are prepared by the following steps:

[0076] (1) Hydroxylation treatment of hollow glass microspheres

[0077] 500 ml of potassium hydroxide aqueous solution (0.5 M) and 20 g of HGM (particle size of 50 μm, wall thickness of 2 μm) were added to a 1000 ml three-necked flask and stirred at 80°C and 400 r / min for 1.5 h. After the alkali washing was completed, the mixture was filtered, washed with water until neutral and filtered, and the hydroxylated HGM was dried in a vacuum oven at 80°C for 12 h to obtain OH-HGM.

[0078] (2) OH-HGM grafted KH560

[0079] 500 ml of ethanol-water solution (V water: V ethanol = 1:2) of 20 g KH560 was added to a three-necked flask, and hydrochloric acid solution was added to adjust the pH to 5.5 and hydrolyzed at room temperature (25°C) for 3 hours. Then 20 g OH-HGM was added and stirred at 85°C and 200 r / min for 2 hours. After the reaction was completed, the excess KH560 was removed by suction and anhydrous ethanol, and the filter cake was placed in a vacuum oven at 80°C and dried for 12 hours to obtain KH560-HGM.

[0080] (3) Graphene oxide coated KH560-HGM

[0081] Weigh 1.0g GO and add it to 400ml deionized water, and ultrasonicate for 30min. Then add 20g KH560-HGM and stir at 85℃ and 300r / min for 2h. After the reaction is completed, filter, wash with water, and dry in a vacuum oven at 75℃ for 15h to obtain GO-HGM.

[0082] (4) High temperature reduction of graphene oxide

[0083] 20 g of GO-HGM was put into a crucible, and the temperature was increased to 280 °C in a muffle furnace at a heating rate of 8 °C / min and maintained for 50 min to obtain rGO-HGM.

[0084] (5) In-situ generation of iron from graphene oxide

[0085] Add 1.0 g rGO-HGM to 500 ml 1 mol / L FeCl3 solution, stir at room temperature (25°C) and 400 r / min for 3 h, slowly add 20 g zinc powder particles (excess), stir at room temperature (25°C) and 400 r / min for 3 h, let stand for 1 h, take the upper layer of rGO-Fe-HGM (floating), filter and remove ZnCl2 with anhydrous ethanol, put the filter cake into a 75°C vacuum oven and dry it for 12 h to obtain rGO-Fe-HGM.

[0086] Comparative Example 1

[0087] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not undergo thermal reduction and iron reduction reaction, and the specific steps are as follows:

[0088] (1) Hydroxylation treatment of hollow glass microspheres

[0089] 200 ml of NaOH aqueous solution (0.5 M) and 10 g of HGM (particle size of 50 μm, wall thickness of 2 μm) were added to a 500 ml three-necked flask and stirred at 70°C and 300 r / min for 1 h. After the alkali washing was completed, the mixture was filtered, washed with water until neutral and filtered, and the hydroxylated HGM was dried in a vacuum oven at 70°C for 12 h to obtain OH-HGM.

[0090] (2) OH-HGM grafted KH550

[0091] 10g KH550 ethanol-water solution (V water: V ethanol = 1: 2) 200ml, add hydrochloric acid solution to adjust pH to 6.0 and hydrolyze at room temperature (25℃) for 2h. Then add 10g OH-HGM, stir and react at 80℃, 300r / min for 1.5h. After the reaction is completed, filter and remove excess KH550 with anhydrous ethanol, put the filter cake into a 70℃ vacuum oven and dry it for 12h to obtain KH550-HGM.

[0092] (3) Graphene oxide coated KH550-HGM

[0093] Weigh 0.4g GO and add it to 200ml deionized water, and ultrasonicate for 30min. Then add 10g KH550-HGM and stir at 80℃ and 400r / min for 1.5h. After the reaction is completed, filter, wash with water, and dry in a vacuum oven at 70℃ for 12h to obtain GO-HGM.

[0094] Comparative Example 2

[0095] The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 does not undergo an iron reduction reaction, and the specific steps are as follows:

[0096] (1) Hydroxylation treatment of hollow glass microspheres

[0097] 200 ml of NaOH aqueous solution (0.5 M) and 10 g of HGM were added to a 500 ml three-necked flask, and stirred at 70°C and 300 r / min for 1 h. After the alkali washing, the mixture was filtered, washed with water until neutral and filtered, and the hydroxylated HGM was dried in a vacuum oven at 70°C for 12 h to obtain OH-HGM.

[0098] (2) OH-HGM grafted KH550

[0099] 10g KH550 ethanol-water solution (V water: V ethanol = 1: 2) 200ml, add hydrochloric acid solution to adjust pH to 6.0 and hydrolyze at room temperature (25℃) for 2h. Then add 10g OH-HGM, stir and react at 80℃, 300r / min for 1.5h. After the reaction is completed, filter and remove excess KH550 with anhydrous ethanol, put the filter cake into a 70℃ vacuum oven and dry it for 12h to obtain KH550-HGM.

[0100] (3) Graphene oxide coated KH550-HGM

[0101] Weigh 0.4g GO and add it to 200ml deionized water, and ultrasonicate for 30min. Then add 10g KH550-HGM and stir at 80℃ and 400r / min for 1.5h. After the reaction is completed, filter, wash with water, and dry in a vacuum oven at 70℃ for 12h to obtain GO-HGM.

[0102] (4) High temperature reduction of graphene oxide

[0103] 10 g of GO-HGM was put into a crucible, and the temperature was increased to 300 °C in a muffle furnace at a heating rate of 10 °C / min and maintained for 30 min to obtain rGO-HGM.

[0104] Comparative Example 3

[0105] The difference between Comparative Example 3 and Example 1 is that the graphene oxide in Comparative Example 3 is not reduced, and the specific steps are as follows:

[0106] (1) Hydroxylation treatment of hollow glass microspheres

[0107] 200 ml of NaOH aqueous solution (0.5 M) and 10 g of HGM were added to a 500 ml three-necked flask, and stirred at 70°C and 300 r / min for 1 h. After the alkali washing, the mixture was filtered, washed with water until neutral and filtered, and the hydroxylated HGM was dried in a vacuum oven at 70°C for 12 h to obtain OH-HGM.

[0108] (2) OH-HGM grafted KH550

[0109] 10g KH550 ethanol-water solution (V water: V ethanol = 1: 2) 200ml, add hydrochloric acid solution to adjust pH to 6.0 and hydrolyze at room temperature (25℃) for 2h. Then add 10g OH-HGM, stir and react at 80℃, 300r / min for 1.5h. After the reaction is completed, filter and remove excess KH550 with anhydrous ethanol, put the filter cake into a 70℃ vacuum oven and dry it for 12h to obtain KH550-HGM.

[0110] (3) Graphene oxide coated KH550-HGM

[0111] Weigh 0.4g GO and add it to 200ml deionized water, and ultrasonicate for 30min. Then add 10g KH550-HGM and stir at 80℃ and 400r / min for 1.5h. After the reaction is completed, filter, wash with water, and dry in a vacuum oven at 70℃ for 12h to obtain GO-HGM.

[0112] (4) In-situ generation of iron from graphene oxide

[0113] Add 0.4 g GO-HGM to 200 ml 1 mol / L FeCl2 solution, stir at room temperature (25°C) and 300 r / min for 2 h, slowly add 10 g zinc powder particles (excess), stir at room temperature (25°C) and 300 r / min for 2 h, let stand for 1 h, take the upper layer of GO-Fe-HGM (floating), filter and remove ZnCl2 with anhydrous ethanol, put the filter cake into a 70°C vacuum oven and dry it for 12 h to obtain GO-Fe-HGM.

[0114] Comparative Example 4

[0115] The difference between Comparative Example 4 and Example 1 is that the graphene oxide in Comparative Example 4 is first reduced and then coated with KH550-HGM. The specific steps are as follows:

[0116] (1) Hydroxylation treatment of hollow glass microspheres

[0117] 200 ml of NaOH aqueous solution (0.5 M) and 10 g of HGM were added to a 500 ml three-necked flask, and stirred at 70°C and 300 r / min for 1 h. After the alkali washing, the mixture was filtered, washed with water until neutral and filtered, and the hydroxylated HGM was dried in a vacuum oven at 70°C for 12 h to obtain OH-HGM.

[0118] (2) OH-HGM grafted KH550

[0119] 10g KH550 ethanol-water solution (V water: V ethanol = 1: 2) 200ml, add hydrochloric acid solution to adjust pH to 6.0 and hydrolyze at room temperature (25℃) for 2h. Then add 10g OH-HGM, stir and react at 80℃, 300r / min for 1.5h. After the reaction is completed, filter and remove excess KH550 with anhydrous ethanol, put the filter cake into a 70℃ vacuum oven and dry it for 12h to obtain KH550-HGM.

[0120] (3) High temperature reduction of graphene oxide

[0121] 10 g of GO was weighed and placed in a crucible. The temperature was raised to 300 °C in a muffle furnace at a heating rate of 10 °C / min and maintained for 30 min to obtain rGO.

[0122] (4) rGO coated KH550-HGM

[0123] Weigh 0.4g rGO and add it to 200ml deionized water, and ultrasonicate for 30min. Then add 10g KH550-HGM and stir at 80℃ and 400r / min for 1.5h. After the reaction is completed, filter, wash with water, and dry in a vacuum oven at 70℃ for 12h to obtain rGO-HGM.

[0124] (5) In-situ generation of iron from graphene oxide

[0125] Add 0.4 g rGO-HGM to 200 ml 1 mol / L FeCl2 solution, stir at room temperature (25°C) and 300 r / min for 2 h, slowly add 10 g zinc powder particles (excess), stir at room temperature (25°C) and 300 r / min for 2 h, let stand for 1 h, take the upper layer of rGO-Fe-HGM (floating), filter and remove ZnCl2 with anhydrous ethanol, put the filter cake into a 70°C vacuum oven and dry it for 12 h to obtain rGO-Fe-HGM.

[0126] Comparative Example 5

[0127] The difference between Comparative Example 5 and Example 1 is that the HGM in Comparative Example 5 is not modified, and the specific steps are as follows:

[0128] (1) Graphene oxide coated HGM

[0129] Weigh 0.4g GO and add it to 200ml deionized water, and ultrasonicate for 30min. Then add 10g HGM (particle size is 50μm, wall thickness is 2μm), and stir at 80℃ and 400r / min for 1.5h. After the reaction is completed, filter, wash with water, and dry in a vacuum oven at 70℃ for 12h to obtain GO-HGM.

[0130] (4) High temperature reduction of graphene oxide

[0131] 10 g of GO-HGM was put into a crucible, and the temperature was increased to 300 °C in a muffle furnace at a heating rate of 10 °C / min and maintained for 30 min to obtain rGO-HGM.

[0132] (5) In-situ generation of iron from graphene oxide

[0133] Add 0.4 rGO-HGM to 200 ml 1 mol / L FeCl2 solution, stir at room temperature (25°C) and 300 r / min for 2 h, slowly add 10 g zinc powder particles (excess), stir at room temperature (25°C) and 300 r / min for 2 h, let stand for 1 h, take the upper layer of rGO-Fe-HGM (floating), filter and remove ZnCl2 with anhydrous ethanol, put the filter cake into a 70°C vacuum oven and dry it for 12 h to obtain rGO-Fe-HGM.

[0134] The products of Examples 1-6 and Comparative Examples 1-5 were prepared into 4 mm thick samples (the samples and paraffin were placed in a mold at a volume ratio of 1:1 and pressed), and the absorbing properties were analyzed using a vector network analyzer at 8-18 GHz. The maximum absorbing properties and the frequency width >10 dBd are shown in Table 1.

[0135] The sample was placed on a heating platform at a constant temperature of 80°C and heated at room temperature for 1 hour. Then an infrared temperature gun was used to test the surface temperature of the material. The specific test results are shown in Table 1.

[0136] Table 1 Wave absorbing and heat insulation performance data of the materials of the embodiments and comparative examples

[0137]

[0138] As can be seen from Table 1, in Comparative Example 1 and Comparative Example 2, the wave absorption capacity of Comparative Example 2 is enhanced. Whether in terms of maximum wave absorption capacity or span >10dB, it can be seen that the material of Comparative Example 2 has better wave absorption performance. This is because the graphene oxide coated hollow glass microspheres effectively hinders the accumulation between graphene sheets during the thermal reduction process, and a large number of closed-cell structures are generated inside, thereby enhancing the wave absorption performance. It can be seen from Comparative Example 2 and Example 1 that the in-situ synthesis of iron powder on the graphene surface also has a positive effect on the real and imaginary parts of the magnetic loss, because the dielectric loss and magnetic loss of the material are significantly improved, which promotes the impedance matching of the material surface, allowing more electromagnetic waves to enter the interior of the material, reducing internal losses, and improving the wave absorption performance as a whole. It can be seen from Comparative Example 4 and Comparative Example 3 that after reduction, graphene oxide can improve the wave absorption performance of the material to a certain extent. However, by comparing Comparative Example 4 and Example 1, it can be seen that when the graphene oxide is thermally reduced without coating the hollow glass microspheres, the graphene oxide is accumulated. Therefore, although Comparative Example 4 has been thermally reduced, its wave absorption performance is still inferior to that of Example 1. By comparing Comparative Example 5 with Example 1, it can be seen that after HGM is treated with hydroxyl groups and modified with silane coupling agents, graphene oxide can be successfully coated on the surface of HGM, which hinders the accumulation of graphene sheets during the thermal reduction process, thereby improving the wave absorption performance of the material.

[0139] It can be seen in Examples 1, 2, 3 and 4 that as the pore size of the glass beads increases, the wave absorption capacity decreases. This is because a small pore size can enhance multiple reflections of electromagnetic waves inside and enhance the wave absorption performance, while a small pore size can reduce the wave absorption performance. Example 5 only uses silane coupling agent treatment, and the wave absorption performance is reduced compared to Example 1.

[0140] As can be seen from Table 1, the thermal insulation performance is mainly related to the pore size of the hollow glass microspheres. The lower the pore size, the greater the thermal resistance. Therefore, the thermal insulation performance of Comparative Example 1 and Example 1 is the same, and the thermal insulation performance of Example 1, Example 2, Example 3 and Example 4 decreases in turn. The flame retardant performance of all materials can reach V0. And the density of all materials is less than 0.3g / cm 3 , is a very light material.

[0141] The various aspects, embodiments, and features of the present invention should be considered to be illustrative in all aspects and not limiting of the present invention, the scope of which is defined solely by the claims. Other embodiments, modifications, and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0142] In the preparation method of the present invention, the order of each step is not limited to the order listed. For those skilled in the art, without creative work, the order of each step is also within the protection scope of the present invention. In addition, two or more steps or actions can be performed simultaneously.

[0143] Finally, it should be noted that the specific embodiments described herein are merely examples of the present invention, and are not intended to limit the implementation methods of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described, or replace them in a similar manner. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A method for preparing self-assembled graphene-Fe coated hollow and / or porous microspheres, characterized in that: The following steps are involved: Hollow and / or porous microspheres coated and modified with graphene oxide; After thermal reduction, hollow and / or porous microspheres coated with reduced graphene oxide are obtained; The hollow and / or porous microspheres coated and modified by reduced graphene oxide are subjected to a reduction reaction, and iron is grown in situ on the surface of the reduced graphene oxide to obtain graphene-Fe coated hollow and / or porous microspheres with a self-assembled structure; The modified hollow and / or porous microspheres are obtained by grafting silane coupling agents onto the hollow and / or porous microspheres, or the modified hollow and / or porous microspheres are obtained by hydroxylating the hollow and / or porous microspheres and then grafting silane coupling agents onto the microspheres.

2. The preparation method according to claim 1, characterized in that: The hollow and / or porous microspheres are placed in an alkaline solution for reaction, and after the reaction is completed, the hollow and / or porous microspheres are filtered, washed, and dried to obtain hydroxylated hollow and / or porous microspheres; The step of grafting silane coupling agent comprises: adding silane coupling agent into solvent, adjusting pH to hydrolyze, then adding hollow and / or porous microspheres or hydroxylated hollow and / or porous microspheres, reacting, and after completion, solid-liquid separation, washing, and drying to obtain modified hollow and / or porous microspheres.

3. The preparation method according to claim 2, characterized in that: In the hydroxylation treatment step, the mass molar ratio of the hollow and / or porous microspheres to the base is 1 g: 0.001 to 1 mol; And / or, the hydroxylation reaction is carried out at 45 to 95° C. for 0.5 to 10 h.

4. The preparation method according to claim 2, characterized in that: In the step of grafting the silane coupling agent, the solvent is a mixture of water and a polar organic solvent, and the volume ratio of water to the polar organic solvent is 1:0.5-5; and / or, adjusting the pH to: 5≤pH≤6.8; and / or, adjusting the pH to 10-40° C. and hydrolyzing for 0.5-5 h; and / or, the mass ratio of the hollow and / or porous microspheres or the hydroxylated hollow and / or porous microspheres to the silane coupling agent is 1:(0.2-10); And / or, the reaction of the grafted silane coupling agent is carried out at 45 to 95° C. for 0.5 to 10 hours.

5. The preparation method according to claim 1, characterized in that: The step of coating the modified hollow and / or porous microspheres with graphene oxide comprises: dispersing graphene oxide in water, adding the modified hollow and / or porous microspheres, reacting, and after the reaction, performing solid-liquid separation, washing, and drying to obtain the modified hollow and / or porous microspheres coated with graphene oxide.

6. The preparation method according to claim 5, characterized in that: In the step of coating the modified hollow and / or porous microspheres with graphene oxide, each gram of graphene oxide is dispersed in 10 to 1000 ml of water; and / or, the mass ratio of graphene oxide to the modified hollow and / or porous microspheres is 1:2 to 200; And / or, the reaction in the coating step is carried out at 45-95° C. for 0.5-10 h.

7. The preparation method according to claim 1, characterized in that: The holding temperature of thermal reduction is 200-400°C, and the holding time of thermal reduction is 20-100 minutes; and / or, heating to the heat reduction holding temperature at a rate of 5 to 15°C / min.

8. The preparation method according to claim 1, characterized in that: The reduction reaction steps include: placing the hollow and / or porous microspheres coated with reduced graphene oxide in a ferric salt or ferrous salt solution, and then adding a reducing agent with a higher reducing power than Fe 3+ or Fe 2+ After the reaction, let the metal powder stand, take the upper floating material, filter it, wash it and dry it.

9. The preparation method according to claim 8, characterized in that: The iron salt or ferrous salt is one or more of ferric nitrate, ferrous nitrate, ferrous sulfate, ferric sulfate, ferric chloride, and ferrous chloride; and / or, more reducible than Fe 3+ or Fe 2+ The metal powder is one or more of zinc, magnesium and calcium; and / or, the mass molar ratio of the hollow and / or porous microspheres coated and modified by reduced graphene oxide to the iron salt or ferrous salt is 1 g: 0.05 to 1.0 mol; and / or, placing the hollow and / or porous microspheres coated with reduced graphene oxide in a ferric salt or ferrous salt solution, and stirring at 10 to 40° C. for 0.5 to 5 hours; and / or, adding a reducing agent higher than Fe 3+ or Fe 2+ The metal powder is stirred and reacted at 10-40°C for 0.5-5h.

10. A self-assembled graphene-Fe coated hollow and / or porous microsphere, characterized in that: It is prepared by the preparation method described in claim 1.

Citation Information

Patent Citations

  • Metal / graphene composite material and preparation method thereof

    CN105215353A

  • Graphene clad porous granular material and preparation method thereof

    CN105226257A

  • Iron-plated graphene and preparation method

    CN106028768A

  • Preparation method of graphene-coated silicon dioxide nanoparticles

    CN106517215A