Reactive halogen-free phosphorus-nitrogen flame retardant as well as preparation method and application thereof

The halogen-free phosphorus-nitrogen flame retardant is prepared through the grafting reaction of polycyanamine and phosphorus-chloride compounds, which solves the problems of poor flame retardant effect, easy precipitation and halogen of flame retardants, and achieves efficient, long-lasting flame retardant performance and environmental friendliness. of polyurethane foam.

CN118852040AActive Publication Date: 2024-10-29JIANGSU CHANGSHUN POLYMER MATERIAL INST CO LTD

Patent Information

Application Number
CN202310478106.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-10-29
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

Existing flame retardants have problems such as poor flame retardant effect, easy precipitation of flame retardant elements, poor stability, and containing halogen. In particular, reactive flame retardants commonly available on the market are expensive and environmentally unfriendly.

Method used

A reactive halogen-free phosphorus-nitrogen flame retardant is used to form a phosphorus-nitrogen synergistic flame retardant system through the graft reaction of melamine and phosphorus-chlorine compounds under specific conditions, and through specific preparation steps such as stirring, dripping, filtration, and extraction and vacuum distillation to obtain the flame retardant. The structure contains flame retardant elements such as phosphorus, nitrogen, and benzene rings, and does not contain halogen.

Benefits of technology

Efficient flame retardant effect is achieved, the flame retardant performance is long-lasting and environmentally friendly. Only a small amount of addition can significantly increase the critical oxygen index of polyurethane foam to 27.5%, which is better than traditional flame retardants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852040A_ABST
    Figure CN118852040A_ABST
Patent Text Reader

Abstract

The invention relates to a reaction type halogen-free phosphorus-nitrogen flame retardant as well as a preparation method and application thereof, mainly solves the problems of poor flame-retardant effect, easiness in precipitation of flame-retardant elements, poor stability and environmental unfriendliness due to halogen contained in a flame retardant in the prior art, and provides the reaction type halogen-free phosphorus-nitrogen flame retardant. The preparation method comprises the following steps: (1) reacting melamine and carbonic ester in a molar ratio of 1: (6-18) at 150-200 DEG C for 3-8 hours to obtain a material I; (2) adding an acid-binding agent and a reaction solvent into the material I, and uniformly stirring in an ice bath to obtain a material II; (3) dropwise adding a phosphorus-chlorine compound into the material II according to the molar ratio of melamine to the phosphorus-chlorine compound of 1: (1-4); (4) continuing to carry out ice bath reaction for 1-3 hours, heating to room temperature, and continuing to carry out reaction for 1-12 hours; and (5) after the reaction is finished, filtering, extracting, drying and carrying out reduced pressure distillation to obtain the reaction type halogen-free phosphorus-nitrogen flame retardant, the technical problem is well solved, and the flame retardant can be used for flame retardance of polyurethane foam.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of organic synthesis, and in particular to a reactive halogen-free phosphorus-nitrogen flame retardant and a preparation method and application thereof. Background Art

[0002] Polyurethane is widely used in various fields such as home furnishing, construction, and daily necessities due to its stability and aging resistance. However, polyurethane raw material molecules contain a large number of flammable hydrocarbon segments, which are very easy to burn. With the frequent occurrence of fire accidents, various fields have higher and higher requirements for the flame retardant properties of polyurethane materials. Therefore, the social demand for flame retardants has also increased year by year in recent years. And with the continuous enhancement of environmental awareness and sustainable development awareness, the development of efficient, environmentally friendly and clean flame retardants has become a new trend.

[0003] According to different principles of use, flame retardants are mainly divided into additive type and reactive type. Additive flame retardants are directly added to polyurethane foam raw materials by mechanical mixing to achieve flame retardant effect. Its preparation method is simple, cost-effective, and widely applicable, so it is widely used; however, additive flame retardants generally have a plasticizing effect, which will affect the mechanical properties of polyurethane materials after addition, and flame retardant elements are easy to migrate out, affecting the flame retardant effect of polyurethane materials. This is also the fatal disadvantage of additive flame retardants. Reactive flame retardants react compounds containing flame retardant elements such as phosphorus and nitrogen with isocyanate segments through chemical bonds to produce polyurethane foam with flame retardant properties. It can effectively solve the problem of flame retardant element migration and has long-lasting flame retardancy. Common reactive flame retardants mainly include halogen reactive flame retardants, phosphorus reactive flame retardants, nitrogen reactive flame retardants, etc. At the same time, with the increase of environmental awareness in society, modifying compounds containing low-smoke, low-toxic flame retardant elements such as phosphorus and nitrogen with polyol segments is one of the mainstream directions of flame retardant development at present; phosphorus-nitrogen synergistic flame retardants have attracted widespread attention because they contain both phosphorus and nitrogen flame retardant elements and have better flame retardant effects than single flame retardant elements. However, the common reactive flame retardants on the market have the disadvantages of high prices and poor stability, and some flame retardants also contain halogens, which greatly limits their application scenarios.

[0004] Chinese patent application CN115679470A discloses a flame-retardant polyester fiber fabric and a preparation method thereof, wherein a dicarboxyl triazine phosphate flame retardant is synthesized, and the preparation method comprises: adding 6-(N,N-dihydroxyethyl)amino-2,4-dichloro-1,3,5-triazine, serine and N,N-diisopropylethylamine to tetrahydrofuran, stirring and dissolving, heating to 60-75°C and reacting for 6-18h, cooling after the reaction, concentrating under reduced pressure, and recrystallizing. 6-(N,N-dihydroxyethyl)amino-2,4-serine-1,3,5-triazine is obtained; and then it is reacted with 5,5-dimethyl-1,3-dioxahexanol phosphoryl chloride at 25-40° C. with stirring for 12-36 hours; the obtained triazine phosphate uses the triazine ring as a nitrogen source and the tetrafunctional dioxahexanol phosphate as a phosphorus source to form a nitrogen-phosphorus synergistic flame retardant system, which has a good flame retardant effect, but its structural formula contains a functional carboxyl group and cannot be applied to the polyurethane field. Summary of the invention

[0005] One of the technical problems to be solved by the present invention is that the flame retardants in the prior art have the problems of poor flame retardant effect, easy precipitation of flame retardant elements, poor stability, and environmental unfriendliness due to the presence of halogens. A reactive halogen-free phosphorus-nitrogen flame retardant is provided, which has the advantages of good flame retardant effect, long-lasting flame retardant performance, being halogen-free, environmentally friendly, and having economical raw materials.

[0006] The second technical problem to be solved by the present invention is to provide a method for preparing a reactive halogen-free phosphorus-nitrogen flame retardant corresponding to the first technical problem to be solved.

[0007] The third technical problem to be solved by the present invention is to provide a use corresponding to solving one of the technical problems.

[0008] In order to solve one of the above technical problems, the technical solution adopted by the present invention is as follows: a reactive halogen-free phosphorus-nitrogen flame retardant, whose structural formula is as follows:

[0009]

[0010] wherein A1-A6 is selected from one of -CH2CH2O- or -CH2CH(CH3)O-; 0≤m1+m2+m3+m4+m5+m6≤12, and m1-m6 are integers; R1-R4 is selected from -H, , and R1-R4 are not -H at the same time.

[0011] To solve the second technical problem above, the technical solution adopted by the present invention is as follows: a method for preparing a reactive halogen-free phosphorus-nitrogen flame retardant, comprising the following steps:

[0012] (1) Add melamine and carbonate in a molar ratio of 1:6-18 into a reaction vessel, stir evenly, react under normal pressure, at a reaction temperature of 150-200°C, for a reaction time of 3-8 hours, and distill under reduced pressure to obtain material I;

[0013] (2) adding an acid binding agent and a reaction solvent to material I, stirring the mixture evenly under ice bath conditions to obtain material II;

[0014] (3) adding a phosphorus-chloride compound dropwise to material II, wherein the phosphorus-chloride compound is used in a molar ratio of melamine:phosphorus-chloride compound = 1:1-4, to obtain material III;

[0015] (4) After the addition is completed, material III is allowed to continue to react in an ice bath for 1 to 3 hours, then naturally heated to room temperature and continued to react for 1 to 12 hours to obtain material IV;

[0016] (5) After the reaction is completed, the filtrate is filtered, extracted, dried, and distilled under reduced pressure to obtain the product reactive halogen-free phosphorus-nitrogen flame retardant.

[0017] In the above technical solution, preferably, the carbonate in step (1) is selected from at least one of ethylene carbonate and propylene carbonate.

[0018] In the above technical solution, preferably, the acid-binding agent in step (2) is selected from at least one of triethylamine and pyridine, and the molar ratio of the acid-binding agent to the phosphorus-chloriding compound is 1:1.

[0019] In the above technical solution, preferably, the reaction solvent in step (2) is selected from at least one of dichloromethane, chloroform or tetrahydrofuran.

[0020] In the above technical solution, preferably, the phosphorus-chlorine compound in step (3) is selected from at least one of diphenylphosphine chloride, diphenylphosphine chloride or diphenoxyphosphine chloride.

[0021] In the above technical solution, preferably, the ice bath temperature is -10 to 10°C.

[0022] In the above technical solution, preferably, the filtrate in step (5) is first extracted with chloroform and sodium chloride aqueous solution, and then dried over anhydrous sodium sulfate.

[0023] In the above technical solution, preferably, the conditions for the reduced pressure distillation in step (5) are a temperature of 40 to 70° C. and a pressure of -0.08 to -0.10 MPa, measured in gauge pressure.

[0024] To solve the third technical problem mentioned above, the technical solution adopted by the present invention is as follows: adding the prepared reactive halogen-free phosphorus-nitrogen flame retardant to the foaming formula of polyurethane foam to participate in the reaction, so as to improve the flame retardant properties of polyurethane foam.

[0025] The invention provides a reactive halogen-free phosphorus-nitrogen flame retardant. A phosphorus-chlorine compound is grafted with a melamine derivative by chemical reaction and then purified to obtain a phosphorus-nitrogen synergistic flame retardant compound. The compound structural formula simultaneously contains phosphorus, nitrogen, benzene ring, triazine ring and other elements or groups with flame retardant effect, and has good flame retardant effect. The compound structural formula also contains a reactive group -OH, belonging to a reactive flame retardant. After being added to a foaming formula of polyurethane foam, the compound can further react with -NCO in a black material. The flame retardant element is connected to the macromolecular structural formula of the polyurethane foam, is not easy to migrate out, and has a long-lasting flame retardant performance. The compound structural formula has no halogen structure and has the advantage of being environmentally friendly. The flame retardant is applied to the foaming of polyurethane foam, and the critical oxygen index of the polyurethane foam can be increased to 27.5% by adding a certain amount of the flame retardant of the invention. Good technical effects are achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Attached Figure 1 This is the H-NMR spectrum of the reactive halogen-free phosphorus-nitrogen flame retardant S1 prepared in Example 1. DETAILED DESCRIPTION

[0027] The following are only preferred implementations of the present invention, and are not intended to limit the scope of protection of the present invention. All technical solutions within the scope of the present invention should fall within the scope of protection of the present invention. For professional and technical personnel in this technical field, minor improvements and modifications to the present invention without departing from the principles of the present invention should also fall within the scope of protection of the present invention.

[0028] [Example 1]

[0029] A reactive halogen-free phosphorus-nitrogen flame retardant, the preparation method of which comprises the following steps:

[0030] (1) Melamine and ethylene carbonate were added into a reaction vessel in a molar ratio of 1:9, stirred evenly, reacted at normal pressure and 180° C. for 6 h, and distilled under reduced pressure to obtain material I;

[0031] (2) adding an acid-binding agent triethylamine and a reaction solvent chloroform to material I, wherein the molar ratio of the acid-binding agent triethylamine to the phosphorus-chloriding compound is 1:1, and stirring the mixture evenly under ice bath conditions to obtain material II;

[0032] (3) adding diphenylphosphine chloride dropwise to material II for 1 h, wherein the molar ratio of the added diphenylphosphine chloride to the melamine in step (1) is 3:1, to obtain material III;

[0033] (4) After the addition was completed, the reaction was continued in an ice bath for 1 hour, and then the temperature was naturally raised to room temperature and the reaction was continued for 10 hours to obtain material IV;

[0034] (5) After the reaction is completed, the filtrate is filtered, and the filtrate is extracted with chloroform and sodium chloride aqueous solution, dried over anhydrous sodium sulfate, and distilled under reduced pressure. The temperature of the reduced pressure distillation is 60° C. and the pressure is -0.098 MPa, as measured by gauge pressure, to obtain a reactive halogen-free phosphorus-nitrogen flame retardant S1. The physical property data of the product S1 are shown in Table 3, and the nuclear magnetic hydrogen spectrum characterization data are: 1 H-NMR (ppm, CDCl3), δ=3.04~4.07 (36H, –CH2–), 7.19~7.73 (30H, Aromatic H), the area ratio of the two hydrogens in the spectrum is consistent with the structural formula of the prepared flame retardant.

[0035] [Examples 2 to 6]

[0036] Examples 2 to 6 are carried out according to the steps in Example 1, except for the differences in reaction raw materials, raw material ratios, reaction time, and reaction temperature, as shown in Table 1; the performance data of the obtained reactive halogen-free phosphorus-nitrogen flame retardant product are shown in Table 3.

[0037] Table 1 Molar ratio of raw materials and reaction conditions in the preparation of reactive halogen-free phosphorus-nitrogen flame retardants in Examples 1 to 6

[0038]

[0039]

[0040] The main structural formula of the reactive halogen-free phosphorus-nitrogen flame retardant prepared in Examples 1 to 6 is as follows: S1: S2: S3: S4: S5: S6:

[0041] [Example 7]

[0042] The reactive halogen-free phosphorus-nitrogen flame retardant prepared in Examples 1 to 6 was added to the polyurethane foaming formula to improve the flame retardant properties of the polyurethane foam. The weight proportions of the components in the formula are shown in Table 2. The flame retardant properties of the prepared polyurethane foam, i.e., the critical oxygen index data, are shown in Table 3.

[0043] Table 2 Weight percentage of each component of the flame retardant added to the polyurethane foaming formula in Examples 1 to 6 and Comparative Example 1

[0044]

[0045]

[0046] [Comparative Example 1]

[0047] Referring to the technical scheme of Example 1 in Chinese patent application CN110283207A, the phosphorus-nitrogen flame retardant is synthesized in the following steps:

[0048] Hexamethoxymethylmelamine (HMMM, 3.9 g, 0.01 mol) and phosphate diol (di-2-hydroxyethylaminomethyl phosphonic acid diethyl ester, FRC-6, 5.1 g, 0.02 mol) were added to a 100 mL three-necked flask, and then p-toluenesulfonic acid (TsOH, about 0.005 g) and N,N-dimethylformamide (DMF, 2 g) were added. Under nitrogen protection, the ether exchange reaction was completed at 120° C. with magnetic stirring for 3 h. The reaction system was cooled to room temperature, 2 mL of ethyl acetate was added and stirred evenly, and then 12 mL of n-hexane was added under stirring conditions, and the phases were allowed to stand and separated, and the upper clear liquid was removed. After repeating this process 3 to 5 times, the viscous substance in the lower layer was evaporated at 55 to 70° C. to remove the solvent, and a brown-yellow viscous product was obtained: phosphorus-nitrogen synergistic flame retardant S, with a yield of 95%.

[0049] The prepared flame retardant is added to the polyurethane foaming formula to improve the flame retardant properties of the polyurethane foam. The weight proportions of the components in the formula are shown in Table 2. The flame retardant properties of the prepared polyurethane foam are shown in Table 3.

[0050] Table 3 Index data of phosphorus nitrogen flame retardants in Examples 1 to 6 and Comparative Example 1 and polyurethane foam in Example 7

[0051]

[0052] From the performance data of the critical oxygen index in Table 3, it can be seen that when the reactive halogen-free phosphorus-nitrogen flame retardants prepared in Examples 1 to 6 are added to the same polyurethane foam foaming formula in the same amount, the critical oxygen index of the prepared polyurethane foam is above 25%, which can reach 27.5%, and the flame retardant performance is much better than that of Comparative Example 1; and the flame retardant prepared by the present invention is a reactive flame retardant containing multiple flame retardant elements such as phosphorus, nitrogen, benzene ring, triazine ring, etc. in the compound structure. The flame retardant elements are not easy to migrate out and the flame retardant performance is more durable; the flame retardant compound structure does not contain halogen, is more environmentally friendly, has good technical effects, and can be used to improve the flame retardant performance of polyurethane foam.

Claims

1. A reactive halogen-free phosphorus-nitrogen flame retardant, the structural formula of which is as follows: in, A1-A6 is selected from one of -CH2CH2O- or -CH2CH(CH3)O-; 0≤m1+m2+m3+m4+m5+m6≤12, and m1-m6 are integers; R1-R4 is selected from -H, , and R1-R4 are not -H at the same time.

2. A method for preparing the reactive halogen-free phosphorus-nitrogen flame retardant according to claim 1, comprising the following steps: (1) Add melamine and carbonate in a molar ratio of 1:6-18 into a reaction vessel, stir evenly, react under normal pressure, at a reaction temperature of 150-200°C, for a reaction time of 3-8 hours, and distill under reduced pressure to obtain material I; (2) adding an acid binding agent and a reaction solvent to material I, stirring the mixture evenly under ice bath conditions to obtain material II; (3) adding a phosphorus-chloride compound dropwise to material II, wherein the phosphorus-chloride compound is used in a molar ratio of melamine:phosphorus-chloride compound = 1:1-4, to obtain material III; (4) After the addition is completed, material III is allowed to continue to react in an ice bath for 1 to 3 hours, then naturally heated to room temperature and continued to react for 1 to 12 hours to obtain material IV; (5) After the reaction is completed, the filtrate is filtered, extracted, dried, and distilled under reduced pressure to obtain the product reactive halogen-free phosphorus-nitrogen flame retardant.

3. The method for preparing a reactive halogen-free phosphorus-nitrogen flame retardant according to claim 2, characterized in that: The carbonate in step (1) is selected from at least one of ethylene carbonate and propylene carbonate.

4. The method for preparing a reactive halogen-free phosphorus-nitrogen flame retardant according to claim 2, characterized in that: The acid-binding agent in step (2) is selected from at least one of triethylamine and pyridine, and the molar ratio of the acid-binding agent to the phosphorus-chloriding compound is 1:

1.

5. The method for preparing a reactive halogen-free phosphorus-nitrogen flame retardant according to claim 2, characterized in that: The reaction solvent in step (2) is selected from at least one of dichloromethane, chloroform or tetrahydrofuran.

6. The method for preparing a reactive halogen-free phosphorus-nitrogen flame retardant according to claim 2, characterized in that: The phosphorus-chlorine compound in step (3) is selected from at least one of diphenylphosphine chloride, diphenylphosphine chloride or diphenoxyphosphine chloride.

7. The method for preparing a reactive halogen-free phosphorus-nitrogen flame retardant according to claim 2, characterized in that: The temperature of the ice bath is -10 to 10°C.

8. The method for preparing a reactive halogen-free phosphorus-nitrogen flame retardant according to claim 2, characterized in that: In the step (5), the filtrate is first extracted with chloroform and sodium chloride aqueous solution, and then dried over anhydrous sodium sulfate; the temperature of the reduced pressure distillation is 40 to 70° C., and the pressure is -0.08 to -0.10 MPa, measured in gauge pressure.

9. Use of the reactive halogen-free phosphorus-nitrogen flame retardant according to claim 1 in flame retardant polyurethane foam.

Citation Information

Patent Citations

  • Reaction type phosphorus-nitrogen fire retardant and synthesizing method thereof

    CN102757580A

  • Preparation method of flame-retardant melamine hard foam

    CN104250386A

  • Halogen-free phosphorus-nitrogen flame retardant, preparation method thereof, flame-retarding polyester therewith and application of the flame-retarding polyester

    CN104650349A

  • Cross-linked type insoluble halogen-free flame retardant and preparation method and application thereof

    CN105218812A

  • Phosphorus-nitrogen synergistic flame-retardant polyether polyol and preparation method thereof

    CN110283207A

Cited By

  • Reactive phosphorus-nitrogen flame retardant as well as preparation method and application thereof

    CN118852256A

  • Reactive phosphorus-nitrogen flame retardant, and preparation method and use thereof

    CN118852256B