Ink for ester organic matter sensor, ester organic matter sensor and application

By using polyphthalocyanine M, carbon nanotubes and polymer ester organic sensor inks, the problem of preparing flexible sensors in energy storage batteries is solved, high-precision, anti-interference ester gas detection is achieved, and the safe operation of the battery is ensured.

CN118852913APending Publication Date: 2024-10-29CHENGDU MINGYUAN LAKE NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410859931.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing technology makes it difficult to batch prepare flexible ester organic sensors suitable for energy storage battery operating environments, resulting in inaccurate detection of battery damage and ester chemical signal signals, affecting the safe operation of the battery.

Method used

Ink for ester organic matter sensors using components such as polyphthalocyanine M, carbon nanotubes, and polymers. The composite is generated through a composite preparation method, and is printed on a silver circuit and then dried to form a stretchable ester organic matter sensor. , capable of accurately detecting ester gases under temperature and deformation conditions.

Benefits of technology

The batch preparation of flexible and stretchable ester organic sensors is achieved. It has high detection accuracy, anti-interference ability and fast response speed. It is suitable for the deformation detection range of energy storage batteries and does not affect the battery energy density and cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118852913A_ABST
    Figure CN118852913A_ABST
Patent Text Reader

Abstract

The invention discloses ink for an ester organic matter sensor, the ester organic matter sensor and application. The ink for the ester organic matter sensor comprises polyphthalocyanine M, a carbon nanotube, a polymer and a solvent, m is at least one of nickel, cobalt, copper, manganese, iron and vanadium; the carbon nano tube is at least one of a single-wall carbon nano tube and a multi-wall carbon nano tube. When the ink is applied to the ester organic matter sensor, batch preparation of the flexible and stretchable ester organic matter sensor can be achieved, and meanwhile, the prepared ester organic matter sensor is small in influence of temperature and deformation, accurate in feedback signal and high in reliability. The ester gas can be accurately detected in an air environment and under a low-concentration ester gas condition, and the method has relatively good anti-interference capability and relatively high response speed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of flexible sensors, and in particular to ink for ester organic matter sensors, ester organic matter sensors and applications. Background Art

[0002] With the continuous development of new energy applications, energy storage batteries have been widely used in many fields. Damage to energy storage batteries will not only affect the normal operation of electrical equipment, but also lead to safety accidents in serious cases. Therefore, it is particularly necessary to monitor the damage of energy storage batteries in a timely manner.

[0003] Taking lithium-ion batteries as an example, the solvents used in lithium-ion batteries contain a large amount of ester compounds. By detecting the ester chemical signal after leakage of energy storage batteries, a battery dangerous status alarm can be issued to ensure that abnormal battery operation can be detected in time, which is crucial to the safe operation of the battery.

[0004] In view of this, in order to adapt to the actual operating environment of the battery, a flexible ester organic sensor that can be mass-produced is particularly necessary. Summary of the invention

[0005] The purpose of the present invention is to provide ink for ester organic sensor, ester organic sensor and application, which can be used for batch preparation of flexible ester organic sensor.

[0006] The present invention is achieved in that:

[0007] In a first aspect, the present invention provides an ink for an ester organic sensor, comprising:

[0008] Polyphthalocyanine M, carbon nanotubes, polymer and solvent; wherein M is at least one of nickel, cobalt, copper, manganese, iron and vanadium;

[0009] In the ink for the ester organic sensor, the concentration of polyphthalocyanine M is 1 mg / ml-100 mg / ml, the concentration of carbon nanotubes is 0.01 mg / ml-1 mg / ml, and the concentration of polymer is 0.010 wt %-1 wt %.

[0010] In an optional embodiment, the polymer is at least one of nafion, PVDF, PTFE, PVA, PEO and PEG;

[0011] And / or, M is nickel;

[0012] And / or, the carbon nanotube is at least one of a single-walled carbon nanotube or a multi-walled carbon nanotube.

[0013] In an optional embodiment, the solvent is a mixture of alcohol and water;

[0014] Preferably, the alcohol is ethanol;

[0015] Preferably, the volume ratio of the alcohol to water is 4:(15-17).

[0016] In an optional embodiment, the method for preparing the composite comprises:

[0017] The invention also includes the preparation of a composite of polyphthalocyanine M and carbon nanotubes. The preparation method of the composite comprises: using a mixed solution containing M salt, tetracyanobenzene and carbon nanotubes as raw materials to react and generate the composite.

[0018] In an optional embodiment, the reaction temperature is 50°C-200°C, and the reaction time is 0.1h-20h;

[0019] Preferably, the tetracyanobenzene is 1,2,4,5-tetracyanobenzene.

[0020] Preferably, the reaction is carried out in a high pressure hydrothermal autoclave.

[0021] In an optional embodiment, the molar ratio of the M salt to 1,2,4,5-tetracyanobenzene is 1:(3-5);

[0022] Preferably, the M salt is at least one of acetic acid M, sulfuric acid M, nitric acid M, oxalic acid M and chloride M.

[0023] In an optional embodiment, the mass ratio of the 1,2,4,5-tetracyanobenzene to the carbon nanotubes is 1:(0.01-1).

[0024] In an optional embodiment, the solvent of the mixed solution is alcohol, and the alcohol is ethanol;

[0025] After the reaction, the liquid after the reaction is washed and the solid-liquid separation is performed using hydrogen chloride solution and hot ethanol respectively, and the obtained solid phase is dried to obtain the composite.

[0026] In a second aspect, the present invention provides an ester organic sensor, which is obtained by printing or printing the ester organic sensor described in any one of the aforementioned embodiments on a silver circuit with ink and then drying it.

[0027] In a third aspect, the present invention provides an application of the ester organic sensor described in the aforementioned embodiment in detecting battery failure, wherein the battery failure includes battery damage or electrolyte leakage.

[0028] The present invention has the following beneficial effects:

[0029] The ink in this application is applied to ester organic sensors, which can realize the batch preparation of flexible and stretchable ester organic sensors. At the same time, the prepared ester organic sensors are less affected by temperature and deformation, and the feedback signal is accurate. They can accurately detect ester gas in air environment and low concentration ester gas conditions, and have good anti-interference ability and fast response speed. When applied to energy storage batteries, the detection range is suitable for the battery deformation range, the detection accuracy is high, and it is light and flexible, and does not affect the battery energy density and cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0031] Figure 1 Chemical structure characterization of nickel phthalocyanine (NiPc), polymerized nickel phthalocyanine (NiPPc) and polymerized nickel phthalocyanine multi-walled carbon tube composite (NiPPc / WMCNT) by (a) Raman spectroscopy, (b) FTIR spectroscopy and (c) UV spectroscopy.

[0032] Figure 2 The SEM images and EDS spectra of the plane and cross section of the ester organic sensor in Example 1;

[0033] Figure 3 The working principle and performance test diagram of the ester organic sensor in Example 1: a, working principle; b, response and recovery time of the DMC vapor sensor with and without polytetrafluoroethylene protective film; (c)-(h), adaptability and stability of the DMC vapor sensor to interference;

[0034] Figure 4 The local coordination environment of Ni atoms in different samples: (a) Ni K-edge XANES spectra of NiPPc, NiPPc / MWCNT and NiPPc / MWCNC_DMC, where the inset is the absorption edge region; (b) Ni K-edge EXAFS spectra of the corresponding weighted Fourier transform; (c) R value and coordination number of Ni atoms calculated in R space by FT-EXAFS fitting using Athena software; (d) R space of FT-EXAFS fitting of NiPPc; (e) R space of FT-EXAFS fitting of NiPPc / MWCNT; (f) R space of FT-EXAFS fitting of NiPPc / MWCNTDMC;

[0035] Figure 5This is the curve of the resistance change rate of the ester organic sensor in Example 1 versus temperature. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0037] The embodiment of the present invention provides an ink for an ester organic sensor.

[0038] The method comprises: polyphthalocyanine M, carbon nanotubes, polymer and solvent; wherein M is at least one of nickel, cobalt, copper, manganese, iron and vanadium;

[0039] In the ink for the flexible ester organic sensor, the concentration of polyphthalocyanine M is 1 mg / ml-100 mg / ml, the concentration of carbon nanotubes is 0.01 mg / ml-1 mg / ml, and the concentration of polymer is 0.010 wt %-1 wt %.

[0040] In the ink for the flexible ester organic sensor in the present application, polyphthalocyanine M and carbon nanotubes are combined to obtain a composite material, which can respond to changes in ester gas. The addition of the polymer is beneficial to improving the resistance change rate under different ester concentration conditions, thereby helping to improve the detection accuracy of the ester organic sensor and also improving the printing performance of the ink.

[0041] In some embodiments, the polymer is nafion, PVDF (polyvinylidene fluoride), PTFE (polytetrafluoroethylene), PVA (polyvinyl alcohol), PEO ( Polyethylene oxide ) and PEG (polyethylene glycol);

[0042] And / or, M is nickel;

[0043] and / or, the carbon nanotubes are at least one of single-walled carbon nanotubes or multi-walled carbon nanotubes. In some embodiments, the solvent is a mixture of alcohol and water;

[0044] Preferably, the alcohol is ethanol;

[0045] Preferably, the volume ratio of the alcohol to water is 4:(15-17).

[0046] In some embodiments, the ink may be prepared by adding the polymer into a solution composed of ethanol, water and 0.5 wt % Nafion solution in a volume ratio of 4:15:1.

[0047] In some embodiments, the method for preparing the composite comprises:

[0048] The invention also includes the preparation of a composite of polyphthalocyanine M and carbon nanotubes. The preparation method of the composite comprises: using a mixed solution containing M salt, tetracyanobenzene and carbon nanotubes as raw materials to react and generate the composite.

[0049] In some embodiments, the reaction temperature is 50°C-200°C, and the reaction time is 0.1h-20h;

[0050] Preferably, the tetracyanobenzene is 1,2,4,5-tetracyanobenzene.

[0051] Preferably, the reaction is carried out in a high pressure hydrothermal autoclave.

[0052] In some embodiments, the molar ratio of the M salt to 1,2,4,5-tetracyanobenzene is 1:(4-4.5);

[0053] Preferably, the M salt is at least one of acetic acid M, sulfuric acid M, nitric acid M, oxalic acid M and chloride M.

[0054] In some embodiments, the mass ratio of 1,2,4,5-tetracyanobenzene to carbon nanotubes is 1:(0.01-1);

[0055] In some embodiments, the solvent of the mixed solution is alcohol, and the alcohol is ethanol;

[0056] After the reaction, the liquid after the reaction is washed and the solid-liquid separation is performed using hydrogen chloride solution and hot ethanol respectively, and the obtained solid phase is dried to obtain the composite.

[0057] The present invention further provides an ester organic matter sensor, which is obtained by printing or printing the ester organic matter sensor described in any one of the aforementioned embodiments on a silver circuit with ink and then drying it.

[0058] In some embodiments, the printing parameters may be: needle speed 2 mm-4 mm / s, printing pressure 20-40 kPa, printing needle inner diameter 0.05-0.1 mm, printing height 0.01-0.02 mm, substrate heating temperature 40-50°C.

[0059] In some implementations, printing may be performed by screen printing or the like.

[0060] In this embodiment, after the ester molecules enter the printed layer of the ester organic sensor, they will cause a change in the distance between the local position M and the atoms around M, thereby causing a change in the resistance value. Therefore, the sensor can be used for the detection of ester gases.

[0061] The present invention also provides a use of the ester organic sensor described in the aforementioned embodiment in detecting battery damage or electrolyte leakage.

[0062] Specific application methods include, but are not limited to, encapsulating the ester organic sensor of the present invention in the outer shell of an energy storage battery. When the battery is working normally, the ester gas is isolated from the ester organic sensor. When the battery is damaged and the ester gas leaks, the flexible ester organic sensor encapsulated in the outer shell will first detect the ester gas and send out an alarm signal.

[0063] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0064] Example 1

[0065] This embodiment provides a method for preparing a flexible ester organic sensor, which specifically includes the following steps:

[0066] Preparation of the composite: Take nickel acetate tetrahydrate (0.86 mg / ml), 1,2,4,5-tetracyanobenzene (2.57 mg / ml), and MWCNT (multi-walled carbon nanotube) (0.14 mg / ml) in an ethanol solution, the ethanol solution is obtained after ultrasonic dispersion; the ethanol solution is transferred to a stainless steel autoclave with a polytetrafluoroethylene liner and heated to 160°C for reaction for 6 hours, the reaction liquid is washed and filtered with a hydrogen chloride solution and hot ethanol, respectively, to obtain a composite of polyphthalocyanine nickel and multi-walled carbon nanotubes, recorded as NiPPc / MWCNT composite, the composite is dried under vacuum at 60°C for 12 hours and set aside, wherein the chemical structures of nickel phthalocyanine (NiPc), polymerized nickel phthalocyanine (NiPPc) and polymerized nickel phthalocyanine multi-walled carbon nanotube composite (NiPPc / WMCNT) are characterized as follows Figure 1 shown.

[0067] Ink preparation: The dried composite was dissolved in a mixed solvent, wherein the mixed solvent was prepared by mixing ethanol, water and 0.5 wt % Nafion in a volume ratio of 4:15:1 to prepare an ink with a NiPPc / MWCNT composite concentration of 12 mg / ml.

[0068] Printing: Use the prepared ester organic sensor ink to print squares on the silver circuit, and then dry to obtain the ester organic sensor. The SEM images and EDS spectra of the plane and cross-section of the ester organic sensor are as follows: Figure 2 The resistance of the ester organic sensor in DMC vapor with a concentration of 0 ppm and 100 ppm is 3560Ω and 3620Ω respectively, and the resistance change rate when the DMC concentration increases from 0 ppm to 100 ppm is 1.66%.

[0069] The working principle of the ester organic sensor obtained in Example 1 is as follows Figure 3 As shown in a, the ester organic sensor is placed in air with a specified dimethyl carbonate (DMC) concentration to detect the effect of the polytetrafluoroethylene protective film on the ester organic sensor, as well as the adaptability and stability of the ester organic sensor to interference. The results are shown in Figure 3 As shown in bh.

[0070] Figure 3 b is the response and recovery time of the sensor when the surface of the ester organic matter sensor is covered with a polytetrafluoroethylene protective film and when it is not covered with a polytetrafluoroethylene protective film. It can be seen from the figure that the polytetrafluoroethylene protective film has little effect on the response and recovery time of the sensor, where the concentration of dimethyl carbonate (DMC) is 100 ppm.

[0071] Figure 3 c is the resistance change rate when the ambient temperature increases from 20°C to 60°C in 150ppm DMC vapor. As the temperature changes, it can be seen from the figure that the resistance change rate of the sensor does not change much.

[0072] Figure 3 d is the resistance change rate when the ester organic sensor is stretched in 150ppm DMC vapor and different length changes are measured. It can be seen from the figure that the resistance change rate of the sensor does not change much as the sensor length changes by 0%, 2%, 4%, 6% and 8%.

[0073] Figure 3 e is to apply 200N squeezing force to the sensor, and transfer the sensor from 0ppm environment to 150ppm DMC vapor before and after squeezing, and then transfer it to 0ppm environment, and monitor the resistance change rate. It can be seen from the figure that the resistance change rate of the sensor before and after squeezing does not change much.

[0074] Figure 3 f is the sensor immersed in 0.1 μL electrolyte. It can be seen from the figure that the sensor in this embodiment also responds to ester liquids.

[0075] Figure 3 g is to place the sensor in an environment of 100 ppm DMC, DEC, ethanol, acetone, toluene, diethyl ether vapor, 1000 ppm carbon dioxide gas, hydrogen and 5000 ppm water vapor to test the selectivity. It can be seen from the figure that the ester organic sensor is selective for ester gases.

[0076] Figure 3 h is the stability of the sensor in DMC vapor environments with concentrations of 10 ppm, 100 ppm and 500 ppm. It can be seen from the figure that the ester organic sensor has good stability.

[0077] Figure 4 is the local coordination environment of Ni atoms in different samples, from Figure 4 It can be seen that the presence of DMC will change the distance between the local Ni atoms and the adjacent atoms around Ni in NiPPc / MWCNC, confirming that the Figure 3 The principle is shown, wherein the NiPPc / MWCNC_DMC sample is a sample obtained by placing the sensor in this embodiment in a DMC vapor environment with a concentration of 100 ppm and adsorbing DMC until the resistance is stable.

[0078] Figure 5 The resistance change rate of the ester organic matter sensor prepared in Example 1 varies with the concentration of the ester organic matter. Figure 5 It can be seen that there is a good linear relationship between the resistance change rate and the ester gas concentration.

[0079] Example 2

[0080] This embodiment provides a method for preparing a flexible ester organic sensor. The only difference from Example 1 is that the concentration of NiPPc / MWCNT in the ink is adjusted to 1 mg / ml, 5 mg / ml, 10 mg / ml, or sodium carboxymethyl cellulose is added at a concentration of 1 mg / ml. The response values ​​of the ester organic sensor to DMC gas of different concentrations are shown in Table 1.

[0081] Table 1

[0082]

[0083] Example 3

[0084] This embodiment provides a method for preparing a flexible ester organic sensor, which is different from Example 1 only in that nickel in the ink is replaced by Cu, Co, Mn, or multi-walled carbon nanotubes are replaced by single-walled carbon nanotubes, and the concentration of the complex is adjusted. The response value of the obtained ester organic sensor to DMC gas is shown in Table 2.

[0085]

[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. An ink for an ester organic sensor, It is characterized in that include: Polyphthalocyanine M, carbon nanotubes, polymer and solvent; wherein M is at least one of nickel, cobalt, copper, manganese, iron and vanadium; In the ink for the ester organic sensor, the concentration of polyphthalocyanine M is 1 mg / ml-100 mg / ml, the concentration of carbon nanotubes is 0.01 mg / ml-1 mg / ml, and the concentration of polymer is 0.010 wt %-1 wt %.

2. The ink for ester organic sensor according to claim 1, It is characterized in that The polymer is at least one of nafion, PVDF, PTFE, PVA, PEO and PEG; And / or, M is nickel; And / or, the carbon nanotube is at least one of a single-walled carbon nanotube or a multi-walled carbon nanotube.

3. The ink for ester organic sensor according to claim 1, It is characterized in that The solvent is a mixture of alcohol and water; Preferably, the alcohol is ethanol; Preferably, the volume ratio of the alcohol to water is 4:(15-17).

4. The ink for ester organic sensor according to claim 1, It is characterized in that The polyphthalocyanine M and carbon nanotubes form a composite, and the preparation method of the composite comprises: using a mixed solution containing M salt, tetracyanobenzene and carbon nanotubes as raw materials to react to generate the composite; Preferably, the tetracyanobenzene is 1,2,4,5-tetracyanobenzene.

5. The ink for ester organic sensor according to claim 4, It is characterized in that The reaction temperature is 50°C-200°C, and the reaction time is 0.1h-20h; Preferably, the reaction is carried out in a high pressure hydrothermal autoclave.

6. The ink for ester organic sensor according to claim 4, It is characterized in that The molar ratio of the M salt to 1,2,4,5-tetracyanobenzene is 1:(3-5); Preferably, the M salt is at least one of acetic acid M, sulfuric acid M, nitric acid M, oxalic acid M and chloride M.

7. The ink for ester organic sensor according to claim 4, It is characterized in that The mass ratio of the 1,2,4,5-tetracyanobenzene to the carbon nanotubes is 1:(0.01-1).

8. The ink for ester organic sensor according to claim 4, It is characterized in that The solvent of the mixed solution is alcohol, and the alcohol is ethanol; After the reaction, the liquid after the reaction is washed and the solid-liquid separation is performed using hydrogen chloride solution and hot ethanol respectively, and the obtained solid phase is dried to obtain the composite.

9. An ester organic sensor, It is characterized in that The ester organic sensor according to any one of claims 1 to 8 is printed or printed on a silver circuit with ink and then dried.

10. Use of the ester organic sensor according to claim 9 in detecting battery failure, It is characterized in that The battery failure includes battery damage or electrolyte leakage.