A corrosion-resistant pipeline coating material and preparation method thereof
The combination of polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES with L-glutamic acid modifier and compound filler in epoxy resin coatings is solved The problems of micropores and cracks when curing oxygen resin coatings achieve higher corrosion resistance and impact resistance.
Patent Information
- Application Number
- CN202411349917.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-26
AI Technical Summary
Epoxy resin coatings are prone to micropores and cracks during the curing process, resulting in permeation of corrosive media and brittle fracture, reducing corrosion and impact resistance.
The combination of polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES, L-glutamic acid modified and composite filler is used to improve the dispersion and interface visibility of the coating. and fill pores and cracks on the coating surface to form a more complete protective layer.
It significantly improves the corrosion resistance and impact resistance of the coating material, enhances the adhesion and protection performance of the coating, and reduces pores and cracks during curing of epoxy resin.
Smart Images

Figure CN118852951B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of coatings, and specifically refers to a corrosion-resistant pipeline coating material and a preparation method thereof. Background Art
[0002] Pipeline transportation has become the main mode of transportation in the fields of oil and gas transportation. However, in pipeline transportation, the corrosion of metal materials is an important factor causing economic losses and safety accidents. Therefore, the continuous in-depth research and development of pipeline anti-corrosion materials is of great significance.
[0003] Since the improvement of the anti-corrosion ability of metal materials themselves has certain limitations, it is usually difficult to achieve high corrosion resistance, high strength and low cost at the same time. Therefore, in pipeline anti-corrosion, the method of coating anti-corrosion coatings on the surface of the material is often adopted. The anti-corrosion coating can prevent corrosive media from entering the metal surface and achieve the purpose of corrosion protection; common pipeline anti-corrosion coatings include epoxy resin coatings, polyurethane coatings, asphalt coatings, lacquer phenol coatings, olefin resin coatings, perchlorethylene resin coatings, chlorinated rubber coatings, etc. Among them, epoxy resin is widely used in the field of metal corrosion protection due to its good chemical resistance, acid and alkali resistance and other advantages.
[0004] The existing technology currently has the following problems:
[0005] During the curing process of epoxy resin coating, micropores and cracks will be generated as the solvent evaporates, which will not only cause the corrosive medium to penetrate into the metal surface through the coating, but also cause brittle fracture, thereby reducing the corrosion resistance and impact resistance, and adversely affecting the use effect of the coating. Summary of the invention
[0006] In view of the above situation, in order to overcome the defects of the prior art, the present invention proposes a corrosion-resistant pipeline coating material, and the raw materials for preparation include the following components in parts by weight: 8-10 parts of polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES, 15-25 parts of L-glutamic acid, 80-100 parts of epoxy resin, 15-25 parts of compound color filler, 20-30 parts of curing agent, 3-5 parts of leveling agent, and 1-3 parts of defoaming agent.
[0007] The polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES is prepared from raw materials including the following components in parts by weight: 10-12 parts of dopamine hydrochloride, 25-30 parts of hexagonal boron nitride, and 2-3 parts of 3-aminopropyltriethoxysilane coupling agent APTES.
[0008] The composite pigment and filler comprises the following components in parts by weight: 10-20 parts of porous alumina ceramic microbeads, 10-20 parts of polyethylene powder, and 10-20 parts of talc powder.
[0009] The preparation method of the polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES specifically comprises the following steps:
[0010] (1) Add 12.0 g of tris(hydroxymethyl)aminomethane) to 900 mL of deionized water, adjust the pH to 8.0-8.5 with 0.1 mol / L hydrochloric acid solution, and continue to add 2.0-2.4 g of dopamine hydrochloride and 5.0-6.0 g of hexagonal boron nitride solid powder. Hexagonal boron nitride has high permeability resistance, high hardness, insulation, excellent chemical inertness and thermal stability, and is an ideal filler candidate material in the field of corrosion protection. Ultrasonic treatment is performed for 20-30 min, and stirring is performed at room temperature for 24 h. Dopamine hydrochloride can self-polymerize to form polydopamine, which forms a uniform and stable protective layer around hexagonal boron nitride through the π-π interaction between dopamine hydrochloride and hexagonal boron nitride, thereby improving the dispersibility of hexagonal boron nitride, reducing agglomeration, and enhancing impact resistance and corrosion resistance. Vacuum filtration is performed, and the precipitate is washed with deionized water until the filtrate is colorless. The product is vacuum dried at 60 ° C for 24 h to obtain polydopamine@hexagonal boron nitride.
[0011] (2) Dissolve 10 g of polydopamine@hexagonal boron nitride described in step (1) in 100 mL of ethanol solution with a mass fraction of 98%, then add 3-aminopropyltriethoxysilane coupling agent APTES, assemble APTES on polydopamine@hexagonal boron nitride through electrostatic action, polydopamine has excellent adhesion and can improve the corrosion resistance of hexagonal boron nitride, APTES acts as an intermediate medium to improve the dispersibility and interfacial affinity of hexagonal boron nitride in the epoxy resin matrix, ultrasonically treat for 10-20 min, stir at 60-80 ° C and 400-500 rpm for 5-6 h, centrifuge at a centrifugal speed of 5000-6000 rpm for 5-10 min, wash the precipitate with anhydrous ethanol solution for 3-5 times, and then vacuum dry at 60 ° C for 24 h to obtain polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES;
[0012] The preparation method of the composite pigment and filler specifically comprises the following steps:
[0013] a. Dissolve 7.5-8.5g of alumina powder in 25mL of deionized water, add 0.5g of alumina dispersant and perform ultrasonic treatment for 30-50min, then mix with 25mL of sodium alginate aqueous solution with a mass fraction of 1.5-2.0%. Sodium alginate has good antibacterial effect and can effectively control microbial contamination, thereby preventing corrosion caused by microorganisms. Sodium alginate also has good ion exchange and adsorption capacity, and can adsorb a large amount of heavy metal ions, thereby reducing their corrosion to pigments, fillers and substrates. Then add sucrose powder and stir evenly to obtain a ceramic slurry with an alumina solid content of 15-17%. Then inject the ceramic slurry into a 20mL syringe and drip into 50mL of 0.5-1.0% aqueous solution at a drip height of 1-5cm. 0% calcium chloride solution, then the ceramic slurry is immersed in the calcium chloride solution for 12 hours, solidified to form a ball blank, washed with deionized water and then immersed in anhydrous ethanol for 24 hours, dried, and then transferred to a pressureless sintering furnace, heated to 500-600℃ at a rate of 3℃ / min, and then heated to 1250-1350℃ at a rate of 5℃ / min, and kept warm for 1 hour. The alumina porous ceramic microbeads prepared by this method are a lightweight non-metallic functional pigment filler with good thermal conductivity and heat resistance. Its hollow structure can isolate heat, reduce temperature fluctuations on the surface of an object, reduce material aging or damage caused by temperature changes, and achieve an anti-corrosion effect. The alumina porous ceramic microbeads can also reduce the density of the coating, maintain the strength and durability of the coating, and enhance the protective effect of the coating.
[0014] b. Mix the alumina porous ceramic microbeads described in step a with polyethylene powder once. During the first mixing process, the mixing speed is 60-80rpm and the mixing time is 5-10min. Polyethylene, as a plastic, has good wear resistance, corrosion resistance and certain mechanical strength, and can protect the pipeline from the erosion of chemical substances. The alumina porous ceramic microbeads, due to their high hardness, high thermal stability and good thermal conductivity, play a role in enhancing wear resistance, high temperature resistance and heat insulation in the coating. The combination of the two materials can significantly improve the performance of the pipeline coating, so that it can adapt to more complex and harsh working environments. Then, the alumina porous ceramic microbeads are mixed for a second time. During the second mixing process, the mixing speed is 100-200rpm and the mixing time is 10-15min to obtain a composite color filler. The addition of talcum powder can cooperate with the alumina porous ceramic microbeads to significantly improve the hardness, wear resistance, chemical corrosion resistance and other properties of the coating, thereby enhancing the protective effect of the pipeline coating, and reducing the high cost of using ceramic microbeads completely while ensuring the performance;
[0015] Preferably, in step a, the amount of sucrose added is 2.5-4.5 g. Sucrose acts as a pore-forming agent and volatilizes during the sintering process, thereby forming micrometer-sized channels between the alumina particles, increasing the number of pores inside the material, reducing the density, and reducing the mechanical properties.
[0016] The present invention also provides a method for preparing a corrosion-resistant pipeline coating material, which specifically comprises the following steps:
[0017] S1. Add 0.8-1.0g polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES to 160mL deionized water, ultrasonicate for 10-30min, and set aside the obtained dispersion. Weigh L-glutamic acid and dissolve it in 50mL 4mg / mL sodium hydroxide solution. L-glutamic acid is a green corrosion inhibitor. The amino and carboxyl groups in it can form complexes with iron ions, reduce the activity of iron ions, and inhibit the corrosion of metals, thereby improving the corrosion resistance. Stir mechanically for 10-20min, and add the obtained uniform solution dropwise to The dispersion was ultrasonicated for 10-20 minutes, stirred for 24 hours at room temperature under nitrogen protection, centrifuged, and the precipitate was washed with anhydrous ethanol and deionized water in turn until neutral, and dried. L-glutamic acid was attached to the surface of the structure of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES to obtain L-glutamic acid modified product. L-glutamic acid increased the interlayer spacing of the structure of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, effectively reduced the aggregation of nanoparticles, and also expanded the diffusion path of the corrosive medium, thereby improving the barrier performance.
[0018] S2, the L-glutamic acid modified substance described in step S1 is mixed evenly with epoxy resin, compound pigments and fillers, curing agent, leveling agent and defoaming agent, the amino group and polar group of the L-glutamic acid modified substance form covalent bonds with the epoxy group in the epoxy resin, and have better interfacial compatibility, which is beneficial to improve the dispersibility of the L-glutamic acid modified substance in the epoxy resin, thereby filling the tiny pores and depressions on the surface of the coating, and the coating surface is more complete, which not only improves the corrosion resistance and impact resistance, but also makes the connection between the coating and the substrate more firm, and increases the adhesion of the coating. The compound pigments and fillers further enhance the barrier effect of the coating, making it difficult for the corrosive medium to penetrate into the interior of the coating, effectively blocking the corrosion ions from invading the coating substrate, and greatly improving the corrosion resistance of the coating. The mixture is extruded into sheets in a twin-screw extruder, the temperature of zone I of the extruder is 65-85°C, and the temperature of zone II is 80-100°C, and then the sheet material is ground in a desktop knife grinder, and the mesh aperture is 100-160 mesh to obtain a corrosion-resistant pipeline coating material;
[0019] The beneficial effects achieved by the present invention are as follows:
[0020] The coating material prepared by the present invention uses a combination of L-glutamic acid-modified polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES and a composite pigment and filler, which fills the pores and cracks generated when the epoxy resin is cured, forms an effective insulating protective layer, and improves the corrosion resistance and impact resistance of the coating material. At the same time, the improvement of the coating density also enhances the adhesion between the coating material and the substrate, and further enhances the anti-corrosion protection performance of the coating material; in the polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, a thick block substance in the form of a coating film is formed, which improves the dispersibility of the hexagonal boron nitride in the epoxy resin, Among them, polydopamine has excellent adhesion properties, which can improve the adhesion of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, thereby enhancing the protection of the substrate and helping to improve corrosion resistance and impact resistance. The coupling effect of APTES enhances the bonding strength of polydopamine and hexagonal boron nitride, which is beneficial to the stability of the composite. Then, L-glutamic acid is used to modify polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES. L-glutamic acid is attached to the surface of the structure, increasing the interlayer spacing of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES. It effectively reduces the aggregation and agglomeration phenomenon, expands the diffusion path of the corrosive medium, improves the barrier performance, is conducive to isolating the contact between the substrate and the corrosive medium, and slows down the corrosion rate. In addition, the amino group of L-glutamic acid can undergo a ring-opening reaction with the epoxy group of the epoxy resin to produce a strong interface interaction, and can also increase the hydrophobicity of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, thereby significantly improving the dispersibility of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES in epoxy resin, so that it can better fill the pores and cracks on the surface of the coating during curing, making the coating surface more complete, and improving corrosion resistance and impact resistance. Ability, L-glutamic acid through the dense cross-linking degree with epoxy resin, effectively expands or blocks the diffusion path of the corrosive medium, making it difficult for the corrosive medium to pass through the coating and directly react with the substrate, thereby helping to enhance the corrosion resistance; in the composite pigment filler, the blend formed by alumina porous ceramic microbeads, polyethylene and talcum powder has the advantages of light density, good mechanical properties, and good thermal conductivity and heat resistance. It is matched with the L-glutamic acid modifier for filling, which significantly enhances the barrier effect of the coating material, making it difficult for the corrosive medium to penetrate into the coating and the substrate, which not only improves the corrosion resistance and impact resistance of the coating material, but also makes the connection between the coating material and the substrate more firm and enhances the adhesion;The present invention uses polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, L-glutamic acid, epoxy resin, compound pigment filler, curing agent, leveling agent and defoaming agent to make a corrosion-resistant pipeline coating material, which reduces the pores and cracks during the curing of epoxy resin, enhances the corrosion resistance and impact resistance, and has good adhesion to the substrate. ; BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a scanning electron micrograph of the modified L-glutamic acid prepared in Example 1 of the present invention;
[0022] Figure 2 This is a scanning electron microscope image of the brittle fracture cross section of the coating after curing of the corrosion-resistant pipeline coating material prepared in Example 1 of the present invention;
[0023] Figure 3 It is a graph showing the maximum corrosion length results of Examples 1-4 of the present invention and Comparative Examples 1-3;
[0024] Figure 4 The impact strength results of Examples 1-4 and Comparative Examples 1-3 of the present invention are shown in FIG.
[0025] Figure 5 The graph is a graph showing the adhesion results of Examples 1-4 of the present invention and Comparative Examples 1-3. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0027] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0028] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0029] The sources of the reagents used in the examples are as follows:
[0030] Tris(hydroxymethyl)aminomethane CAS No: 77-86-1, brand Innochem, product number A08772;
[0031] Hydrochloric acid CAS No: 7647-01-0, brand Innochem, product number A04558;
[0032] Dopamine hydrochloride CAS No: 335081-04-4, brand Trc, product number D533787;
[0033] Hexagonal boron nitride CAS No: 10043-11-5, brand Innochem, product number A67186;
[0034] 3-Aminopropyltriethoxysilane coupling agent APTES CAS No: 919-30-2, brand Innochem, product number A17919;
[0035] Alumina CAS No: 1344-28-1, brand Innochem, product number A10567;
[0036] Sodium alginate CAS No: 9005-38-3, brand Innochem, product number A02570;
[0037] Alumina dispersant CAS No: 1344-28-1, brand Wuhan Lanabai Pharmaceutical Chemical, item number Lnb-1522;
[0038] Sucrose CAS No: 57-50-1, brand Innochem, product number B04205;
[0039] Calcium chloride CAS No: 10043-52-4, brand Innochem, product number A01289;
[0040] Polyethylene powder CAS No: 9002-88-4, brand Alfa, item number 042607;
[0041] Talc CAS No: 14807-96-6, brand Innochem, product number A69285;
[0042] L-Glutamic acid CAS No: 56-86-0, brand Innochem, product number A57125;
[0043] Sodium hydroxide CAS No: 1310-73-2, brand Innochem, product number A36865;
[0044] Epoxy resin CAS No: 38891-59-7, brand Fusion, item number FZ-0151577-100g;
[0045] Curing agent brand: Ron, item number: R054979-5kg;
[0046] Leveling agent brand Byk, item number 3931;
[0047] Defoamer brand: Macklin, item number: O874979-1kg;
[0048] Anhydrous ethanol CAS No: 64-17-5, brand Innochem, product number G00004.
[0049] Example 1
[0050] This embodiment proposes a corrosion-resistant pipeline coating material, and the raw materials for preparation include the following components in parts by weight: 10 parts of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, 25 parts of L-glutamic acid, 100 parts of epoxy resin, 25 parts of compound color filler, 30 parts of curing agent, 5 parts of leveling agent, and 3 parts of defoaming agent.
[0051] Polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, the preparation raw materials include the following components in parts by weight: 12 parts of dopamine hydrochloride, 30 parts of hexagonal boron nitride, and 3 parts of 3-aminopropyltriethoxysilane coupling agent APTES.
[0052] The compound pigment and filler comprises the following components in parts by weight: 20 parts of porous alumina ceramic microbeads, 20 parts of polyethylene powder and 20 parts of talc powder.
[0053] The preparation method of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES specifically comprises the following steps:
[0054] (1) Add 12.0 g of tris(hydroxymethyl)aminomethane) to 900 mL of deionized water, adjust the pH to 8.5 with 0.1 mol / L hydrochloric acid solution, and continue to add 2.4 g of dopamine hydrochloride and 6.0 g of hexagonal boron nitride solid powder. Hexagonal boron nitride has high permeability resistance, high hardness, insulation, excellent chemical inertness and thermal stability, and is an ideal filler candidate material in the field of corrosion protection. Ultrasonic treatment for 30 min and stirring at room temperature for 24 h. Dopamine hydrochloride can self-polymerize to form polydopamine. Through the π-π interaction between dopamine hydrochloride and hexagonal boron nitride, a uniform and stable protective layer is formed around the hexagonal boron nitride, which not only improves the dispersibility of hexagonal boron nitride and reduces agglomeration, but also enhances the impact resistance and corrosion resistance. Vacuum filtration, the precipitate is washed with deionized water until the filtrate is colorless, and the product is vacuum dried at 60 ° C for 24 h to obtain polydopamine@hexagonal boron nitride.
[0055] (2) Dissolve 10 g of polydopamine@hexagonal boron nitride described in step (1) in 100 mL of 98% ethanol solution, add 3-aminopropyltriethoxysilane coupling agent APTES, and add 0.6 g of 3-aminopropyltriethoxysilane coupling agent APTES. Assemble APTES on polydopamine@hexagonal boron nitride by electrostatic action. Polydopamine has excellent adhesion and can improve the corrosion resistance of hexagonal boron nitride. APTES acts as an intermediate medium to improve the dispersibility and interfacial affinity of hexagonal boron nitride in the epoxy resin matrix. Ultrasonic treatment is performed for 20 min, and the mixture is stirred at 80° C. and 500 rpm for 6 h. Centrifuge at a centrifugal speed of 6000 rpm for 10 min. Wash the precipitate with anhydrous ethanol solution 5 times, and then vacuum dry at 60° C. for 24 h to obtain polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES.
[0056] The preparation method of the composite pigment and filler specifically comprises the following steps:
[0057] a. Dissolve 8.5g of alumina powder in 25mL of deionized water, add 0.5g of alumina dispersant and perform ultrasonic treatment for 50min, then mix with 25mL of 2.0% sodium alginate aqueous solution. Sodium alginate has good antibacterial effect and can effectively control microbial contamination, thereby preventing corrosion caused by microorganisms. Sodium alginate also has good ion exchange and adsorption capacity, and can adsorb a large amount of heavy metal ions, thereby reducing their corrosion to pigments, fillers and substrates. Then add sucrose powder, the amount of sucrose added is 4.5g. Sucrose acts as a pore-forming agent and volatilizes during the sintering process, thereby forming micron-level channels between alumina particles, increasing the number of pores inside the material, reducing the density, and reducing the mechanical properties. Stir evenly to obtain a ceramic slurry with an alumina solid content of 17%, and then inject the ceramic slurry into the slurry. A 20 mL syringe was placed in the slurry, and 50 mL of a 1.0% calcium chloride solution was dripped in at a drip height of 5 cm. The ceramic slurry was then immersed in the calcium chloride solution for 12 hours to solidify and form a spherical blank. After being washed with deionized water, the slurry was immersed in anhydrous ethanol for 24 hours, dried, and then transferred to a pressureless sintering furnace. The temperature was increased to 600°C at a rate of 3°C / min, and then increased to 1350°C at a rate of 5°C / min, and kept warm for 1 hour. The alumina porous ceramic microbeads prepared by this method are a lightweight non-metallic functional pigment filler with good thermal conductivity and heat resistance. The hollow structure can isolate heat, reduce temperature fluctuations on the surface of an object, reduce material aging or damage caused by temperature changes, and achieve an anti-corrosion effect. The alumina porous ceramic microbeads can also reduce the density of the coating, maintain the strength and durability of the coating, and enhance the protective effect of the coating.
[0058] b. Mix the alumina porous ceramic microbeads described in step a with polyethylene powder once. During the first mixing process, the mixing speed is 80 rpm and the mixing time is 10 min. Polyethylene, as a plastic, has good wear resistance, corrosion resistance and certain mechanical strength, and can protect the pipeline from corrosion by chemical substances. The alumina porous ceramic microbeads, due to their high hardness, high thermal stability and good thermal conductivity, play a role in enhancing wear resistance, high temperature resistance and heat insulation in the coating. The combination of the two materials can significantly improve the performance of the pipeline coating, so that it can adapt to more complex and harsh working environments. Then, mix it with talcum powder for a second time. During the second mixing process, the mixing speed is 200 rpm and the mixing time is 15 min to obtain a composite color filler. The addition of talcum powder can cooperate with the alumina porous ceramic microbeads to significantly improve the hardness, wear resistance, chemical corrosion resistance and other properties of the coating, thereby enhancing the protective effect of the pipeline coating, and reducing the high cost of using ceramic microbeads while ensuring performance.
[0059] This embodiment provides a method for preparing a corrosion-resistant pipeline coating material, which specifically includes the following steps:
[0060] S1. Add 1.0g polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES to 160mL deionized water, ultrasonicate for 30min, and set the obtained dispersion aside. Weigh L-glutamic acid and dissolve it in 50mL 4mg / mL sodium hydroxide solution. The amount of L-glutamic acid added is 2.5g. L-glutamic acid is a green corrosion inhibitor. The amino and carboxyl groups in it can form complexes with iron ions, reduce the activity of iron ions, and inhibit the corrosion of metals, thereby improving the corrosion resistance. Mechanically stir for 20min to obtain a uniform solution. Add dropwise to the dispersion, ultrasonicate for 20 minutes, stir for 24 hours at room temperature under nitrogen protection, centrifuge, wash the precipitate with anhydrous ethanol and deionized water in turn until neutral, dry, and attach L-glutamic acid to the surface of the structure of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES to obtain L-glutamic acid modified product. L-glutamic acid increases the interlayer spacing of the structure of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, effectively reduces the aggregation of nanoparticles, and also expands the diffusion path of the corrosive medium, thereby improving the barrier performance.
[0061] S2. The L-glutamic acid modifier described in step S1 is uniformly mixed with epoxy resin, compound pigments and fillers, curing agent, leveling agent and defoaming agent. The amino group and polar group of the L-glutamic acid modifier form covalent bonds with the epoxy group in the epoxy resin, which has better interfacial compatibility and is beneficial to improving the dispersibility of the L-glutamic acid modifier in the epoxy resin, thereby filling the tiny pores and depressions on the surface of the coating, making the coating surface more complete, improving the corrosion resistance and impact resistance, and making the connection between the coating and the substrate more firm, increasing the adhesion of the coating, and the compound pigments and fillers further enhance the barrier effect of the coating, making it difficult for the corrosive medium to penetrate into the interior of the coating, effectively blocking the corrosion ions from invading the coating substrate, and greatly improving the corrosion resistance of the coating. The mixture is extruded into sheets in a twin-screw extruder, the temperature of zone I of the extruder is 85° C., and the temperature of zone II is 100° C. Then the sheet material is ground in a desktop knife grinder with a screen aperture of 160 mesh to obtain a corrosion-resistant pipeline coating material.
[0062] In this embodiment, the prepared L-glutamic acid modified product and the corrosion-resistant pipeline coating material are subjected to scanning electron microscopy to observe the microscopic morphology of the brittle fracture section of the coating after curing. Figure 1 This is a 2000-fold magnified SEM image of the modified L-glutamic acid prepared in Example 1. Figure 2 This is a SEM image of the brittle fracture cross section of the corrosion-resistant pipeline coating material prepared in Example 1 after curing, magnified 1000 times. Figure 1 The modified L-glutamic acid prepared in this embodiment is a thick block structure with multilayer spacing, such as Figure 2 After the corrosion-resistant pipeline coating material prepared in this embodiment is cured, the brittle fracture cross-section of the coating is smooth and has good compatibility.
[0063] Example 2
[0064] This embodiment proposes a corrosion-resistant pipeline coating material, and the raw materials for preparation include the following components in parts by weight: 8 parts of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, 15 parts of L-glutamic acid, 80 parts of epoxy resin, 15 parts of compound color filler, 20 parts of curing agent, 3 parts of leveling agent, and 1 part of defoaming agent.
[0065] Polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, the preparation raw materials include the following components in parts by weight: 10 parts of dopamine hydrochloride, 25 parts of hexagonal boron nitride, and 2 parts of 3-aminopropyltriethoxysilane coupling agent APTES.
[0066] The compound pigment and filler comprises the following components in parts by weight: 10 parts of alumina porous ceramic microbeads, 10 parts of polyethylene powder and 10 parts of talc powder.
[0067] The preparation method of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES specifically comprises the following steps:
[0068] (1) Add 12.0 g of tris(hydroxymethyl)aminomethane) to 900 mL of deionized water, adjust the pH to 8.0 with 0.1 mol / L hydrochloric acid solution, and continue to add 2.0 g of dopamine hydrochloride and 5.0 g of hexagonal boron nitride solid powder. Hexagonal boron nitride has high permeability resistance, high hardness, insulation, excellent chemical inertness and thermal stability, and is an ideal filler candidate material in the field of corrosion protection. Ultrasonic treatment for 20 min and stirring at room temperature for 24 h. Dopamine hydrochloride can self-polymerize to form polydopamine. Through the π-π interaction between dopamine hydrochloride and hexagonal boron nitride, a uniform and stable protective layer is formed around the hexagonal boron nitride, which not only improves the dispersibility of hexagonal boron nitride and reduces agglomeration, but also enhances the impact resistance and corrosion resistance. Vacuum filtration, the precipitate is washed with deionized water until the filtrate is colorless, and the product is vacuum dried at 60 ° C for 24 h to obtain polydopamine@hexagonal boron nitride.
[0069] (2) Dissolve 10 g of polydopamine@hexagonal boron nitride described in step (1) in 100 mL of ethanol solution with a mass fraction of 98%, and then add 3-aminopropyltriethoxysilane coupling agent APTES, the amount of 3-aminopropyltriethoxysilane coupling agent APTES added is 0.4 g, and assemble APTES on polydopamine@hexagonal boron nitride through electrostatic action. Polydopamine has excellent adhesion and can improve the corrosion resistance of hexagonal boron nitride. APTES acts as an intermediate medium to improve the dispersibility and interfacial affinity of hexagonal boron nitride in the epoxy resin matrix. Ultrasonic treatment is performed for 10 min, and the mixture is stirred at 60° C. and 400 rpm for 5 h. Centrifugation is performed at a centrifugal speed of 5000 rpm for 5 min. The precipitate is washed three times with anhydrous ethanol solution, and then vacuum dried at 60° C. for 24 h to obtain polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES.
[0070] The preparation method of the composite pigment and filler specifically comprises the following steps:
[0071] a. Dissolve 7.5g of alumina powder in 25mL of deionized water, add 0.5g of alumina dispersant and perform ultrasonic treatment for 30min, then mix with 25mL of 1.5% sodium alginate aqueous solution. Sodium alginate has good antibacterial effect and can effectively control microbial contamination, thereby preventing corrosion caused by microorganisms. Sodium alginate also has good ion exchange and adsorption capacity, and can adsorb a large amount of heavy metal ions, thereby reducing their corrosion to pigments, fillers and substrates. Then add sucrose powder, the amount of sucrose added is 2.5g. Sucrose acts as a pore-forming agent and volatilizes during the sintering process, thereby forming micron-level channels between alumina particles, increasing the number of pores inside the material, reducing the density, and reducing the mechanical properties. Stir evenly to obtain a ceramic slurry with an alumina solid content of 15%, and then inject the ceramic slurry into the slurry. A 20 mL syringe was placed in the slurry, and 50 mL of a 0.5% calcium chloride solution was dripped in when the dripping height was 1 cm. The ceramic slurry was then immersed in the calcium chloride solution for 12 hours to solidify and form a spherical blank. After being washed with deionized water, the slurry was immersed in anhydrous ethanol for 24 hours, dried, and then transferred to a pressureless sintering furnace. The temperature was increased to 500°C at a rate of 3°C / min, and then increased to 1250°C at a rate of 5°C / min, and kept warm for 1 hour. The alumina porous ceramic microbeads prepared by this method are a lightweight non-metallic functional pigment filler with good thermal conductivity and heat resistance. The hollow structure can isolate heat, reduce temperature fluctuations on the surface of an object, reduce material aging or damage caused by temperature changes, and achieve an anti-corrosion effect. The alumina porous ceramic microbeads can also reduce the density of the coating, maintain the strength and durability of the coating, and enhance the protective effect of the coating.
[0072] b. Mix the alumina porous ceramic microbeads described in step a with polyethylene powder once. During the first mixing process, the mixing speed is 60 rpm and the mixing time is 5 min. Polyethylene, as a plastic, has good wear resistance, corrosion resistance and certain mechanical strength, and can protect the pipeline from corrosion by chemical substances. The alumina porous ceramic microbeads, due to their high hardness, high thermal stability and good thermal conductivity, play a role in enhancing wear resistance, high temperature resistance and heat insulation in the coating. The combination of the two materials can significantly improve the performance of the pipeline coating, so that it can adapt to more complex and harsh working environments. Then, mix it with talcum powder for a second time. During the second mixing process, the mixing speed is 100 rpm and the mixing time is 10 min to obtain a composite color filler. The addition of talcum powder can cooperate with the alumina porous ceramic microbeads to significantly improve the hardness, wear resistance, chemical corrosion resistance and other properties of the coating, thereby enhancing the protective effect of the pipeline coating, and reducing the high cost of using ceramic microbeads while ensuring performance.
[0073] This embodiment provides a method for preparing a corrosion-resistant pipeline coating material, which specifically includes the following steps:
[0074] S1. Add 0.8g polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES to 160mL deionized water, ultrasonicate for 10min, and set the obtained dispersion aside. Weigh L-glutamic acid and dissolve it in 50mL 4mg / mL sodium hydroxide solution. The amount of L-glutamic acid added is 1.5g. L-glutamic acid is a green corrosion inhibitor. The amino and carboxyl groups in it can form complexes with iron ions, reduce the activity of iron ions, and inhibit the corrosion of metals, thereby improving the corrosion resistance. Mechanically stir for 10min to obtain a uniform solution. Add dropwise to the dispersion, ultrasonicate for 10 minutes, stir for 24 hours at room temperature under nitrogen protection, centrifuge, wash the precipitate with anhydrous ethanol and deionized water in turn until neutral, dry, and attach L-glutamic acid to the surface of the structure of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES to obtain L-glutamic acid modified product. L-glutamic acid increases the interlayer spacing of the structure of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, effectively reduces the aggregation of nanoparticles, and also expands the diffusion path of the corrosive medium, thereby improving the barrier performance.
[0075] S2, the L-glutamic acid modifier described in step S1 is mixed evenly with epoxy resin, compound pigments and fillers, curing agent, leveling agent and defoaming agent. The amino group and polar group of the L-glutamic acid modifier form covalent bonds with the epoxy group in the epoxy resin, which has better interfacial compatibility and is beneficial to improving the dispersibility of the L-glutamic acid modifier in the epoxy resin, thereby filling the tiny pores and depressions on the surface of the coating, making the coating surface more complete, which not only improves the corrosion resistance and impact resistance, but also makes the connection between the coating and the substrate more firm, and increases the adhesion of the coating. The compound pigments and fillers further enhance the barrier effect of the coating, making it difficult for the corrosive medium to penetrate into the interior of the coating, effectively blocking the corrosion ions from invading the coating substrate, and greatly improving the corrosion resistance of the coating. The mixture is extruded into sheets in a twin-screw extruder. The temperature of zone I of the extruder is 65°C and the temperature of zone II is 80°C. Then the sheet material is ground in a desktop knife grinder with a screen aperture of 100 mesh to obtain a corrosion-resistant pipeline coating material.
[0076] Example 3
[0077] This embodiment proposes a corrosion-resistant pipeline coating material, and the raw materials for preparation include the following components in parts by weight: 9 parts of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, 20 parts of L-glutamic acid, 90 parts of epoxy resin, 20 parts of compound color filler, 25 parts of curing agent, 4 parts of leveling agent, and 2 parts of defoaming agent.
[0078] Polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, the preparation raw materials include the following components in parts by weight: 11 parts of dopamine hydrochloride, 27.5 parts of hexagonal boron nitride, and 2.5 parts of 3-aminopropyltriethoxysilane coupling agent APTES.
[0079] The compound pigment and filler comprises the following components in parts by weight: 15 parts of porous alumina ceramic microbeads, 15 parts of polyethylene powder and 15 parts of talc powder.
[0080] The preparation method of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES specifically comprises the following steps:
[0081] (1) Add 12.0 g of tris(hydroxymethyl)aminomethane) to 900 mL of deionized water, adjust the pH to 8.3 with 0.1 mol / L hydrochloric acid solution, and continue to add 2.2 g of dopamine hydrochloride and 5.5 g of hexagonal boron nitride solid powder. Hexagonal boron nitride has high permeability resistance, high hardness, insulation, excellent chemical inertness and thermal stability, and is an ideal filler candidate material in the field of corrosion protection. Ultrasonic treatment for 25 min and stirring at room temperature for 24 h. Dopamine hydrochloride can self-polymerize to form polydopamine. Through the π-π interaction between dopamine hydrochloride and hexagonal boron nitride, a uniform and stable protective layer is formed around the hexagonal boron nitride, which not only improves the dispersibility of hexagonal boron nitride and reduces agglomeration, but also enhances the impact resistance and corrosion resistance. Vacuum filtration, the precipitate is washed with deionized water until the filtrate is colorless, and the product is vacuum dried at 60 ° C for 24 h to obtain polydopamine@hexagonal boron nitride.
[0082] (2) Dissolve 10 g of polydopamine@hexagonal boron nitride described in step (1) in 100 mL of 98% ethanol solution, add 3-aminopropyltriethoxysilane coupling agent APTES, and add 0.5 g of 3-aminopropyltriethoxysilane coupling agent APTES. Assemble APTES on polydopamine@hexagonal boron nitride by electrostatic action. Polydopamine has excellent adhesion and can improve the corrosion resistance of hexagonal boron nitride. APTES acts as an intermediate medium to improve the dispersibility and interfacial affinity of hexagonal boron nitride in the epoxy resin matrix. Ultrasonic treatment is performed for 15 min, and the mixture is stirred at 70°C and 450 rpm for 5.5 h. Centrifuge at a centrifugal speed of 5500 rpm for 7.5 min. Wash the precipitate with anhydrous ethanol solution for 4 times, and then vacuum dry at 60°C for 24 h to obtain polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES.
[0083] The preparation method of the composite pigment and filler specifically comprises the following steps:
[0084] a. Dissolve 8.0g of alumina powder in 25mL of deionized water, add 0.5g of alumina dispersant and perform ultrasonic treatment for 40min, then mix with 25mL of 1.8% sodium alginate aqueous solution. Sodium alginate has good antibacterial effect and can effectively control microbial contamination, thereby preventing corrosion caused by microorganisms. Sodium alginate also has good ion exchange and adsorption capacity, and can adsorb a large amount of heavy metal ions, thereby reducing their corrosion to pigments, fillers and substrates. Then add sucrose powder, the amount of sucrose added is 3.5g. Sucrose acts as a pore-forming agent and volatilizes during the sintering process, thereby forming micron-level channels between alumina particles, increasing the number of pores inside the material, reducing the density, and reducing the mechanical properties. Stir evenly to obtain a ceramic slurry with an alumina solid content of 16%, and then inject the ceramic slurry into the slurry. A 20 mL syringe was placed in the well, and 50 mL of a 0.8% calcium chloride solution was dripped in when the dripping height was 3 cm. The ceramic slurry was then immersed in the calcium chloride solution for 12 hours to solidify and form a spherical blank. After being washed with deionized water, the spherical blank was immersed in anhydrous ethanol for 24 hours, dried, and then transferred to a pressureless sintering furnace. The temperature was increased to 550°C at a rate of 3°C / min, and then increased to 1300°C at a rate of 5°C / min, and kept warm for 1 hour. The alumina porous ceramic microbeads prepared by this method are a lightweight non-metallic functional pigment filler with good thermal conductivity and heat resistance. The hollow structure can isolate heat, reduce temperature fluctuations on the surface of an object, reduce material aging or damage caused by temperature changes, and achieve an anti-corrosion effect. The alumina porous ceramic microbeads can also reduce the density of the coating, maintain the strength and durability of the coating, and enhance the protective effect of the coating.
[0085] b. Mix the alumina porous ceramic microbeads described in step a with polyethylene powder once. During the first mixing process, the mixing speed is 70 rpm and the mixing time is 7.5 min. Polyethylene, as a plastic, has good wear resistance, corrosion resistance and certain mechanical strength, and can protect the pipeline from the erosion of chemical substances. The alumina porous ceramic microbeads, due to their high hardness, high thermal stability and good thermal conductivity, play a role in enhancing wear resistance, high temperature resistance and heat insulation in the coating. The combination of the two materials can significantly improve the performance of the pipeline coating, so that it can adapt to more complex and harsh working environments. Then, mix it with talcum powder for a second time. During the second mixing process, the mixing speed is 150 rpm and the mixing time is 12.5 min to obtain a composite color filler. The addition of talcum powder can cooperate with the alumina porous ceramic microbeads to significantly improve the hardness, wear resistance, chemical corrosion resistance and other properties of the coating, thereby enhancing the protective effect of the pipeline coating, and reducing the high cost of using ceramic microbeads while ensuring performance.
[0086] This embodiment provides a method for preparing a corrosion-resistant pipeline coating material, which specifically includes the following steps:
[0087] S1. Add 0.9g polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES to 160mL deionized water, ultrasonicate for 20min, and set the obtained dispersion aside. Weigh L-glutamic acid and dissolve it in 50mL 4mg / mL sodium hydroxide solution. The amount of L-glutamic acid added is 2.0g. L-glutamic acid is a green corrosion inhibitor. The amino and carboxyl groups in it can form complexes with iron ions, reduce the activity of iron ions, and inhibit the corrosion of metals, thereby improving the corrosion resistance. Mechanically stir for 15min to obtain a uniform solution. Add dropwise to the dispersion, ultrasonicate for 15 minutes, stir for 24 hours at room temperature under nitrogen protection, centrifuge, wash the precipitate with anhydrous ethanol and deionized water in turn until neutral, dry, and attach L-glutamic acid to the surface of the structure of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES to obtain L-glutamic acid modified product. L-glutamic acid increases the interlayer spacing of the structure of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, effectively reduces the aggregation of nanoparticles, and also expands the diffusion path of the corrosive medium, thereby improving the barrier performance.
[0088] S2, the L-glutamic acid modifier described in step S1 is mixed evenly with epoxy resin, compound pigments and fillers, curing agent, leveling agent and defoaming agent. The amino group and polar group of the L-glutamic acid modifier form covalent bonds with the epoxy group in the epoxy resin, which has better interfacial compatibility and is beneficial to improving the dispersibility of the L-glutamic acid modifier in the epoxy resin, thereby filling the tiny pores and depressions on the surface of the coating, making the coating surface more complete, improving the corrosion resistance and impact resistance, and making the connection between the coating and the substrate more firm, increasing the adhesion of the coating, and the compound pigments and fillers further enhance the barrier effect of the coating, making it difficult for the corrosive medium to penetrate into the interior of the coating, effectively blocking the corrosion ions from invading the coating substrate, and greatly improving the corrosion resistance of the coating. The mixture is extruded into sheets in a twin-screw extruder, the temperature of zone I of the extruder is 75°C, and the temperature of zone II is 90°C, and then the sheet material is ground in a desktop knife grinder with a screen aperture of 130 mesh to obtain a corrosion-resistant pipeline coating material.
[0089] Example 4
[0090] This embodiment proposes a corrosion-resistant pipeline coating material, and the raw materials for preparing the material include the following components in parts by weight: 10 parts of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, 15 parts of L-glutamic acid, 100 parts of epoxy resin, 15 parts of compound color filler, 30 parts of curing agent, 5 parts of leveling agent, and 3 parts of defoaming agent.
[0091] Polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, the preparation raw materials include the following components in parts by weight: 12 parts of dopamine hydrochloride, 30 parts of hexagonal boron nitride, and 2 parts of 3-aminopropyltriethoxysilane coupling agent APTES.
[0092] The compound pigment and filler comprises the following components in parts by weight: 20 parts of porous alumina ceramic microbeads, 20 parts of polyethylene powder and 20 parts of talc powder.
[0093] The preparation method of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES specifically comprises the following steps:
[0094] (1) Add 12.0 g of tris(hydroxymethyl)aminomethane) to 900 mL of deionized water, adjust the pH to 8.5 with 0.1 mol / L hydrochloric acid solution, and continue to add 2.4 g of dopamine hydrochloride and 6.0 g of hexagonal boron nitride solid powder. Hexagonal boron nitride has high permeability resistance, high hardness, insulation, excellent chemical inertness and thermal stability, and is an ideal filler candidate material in the field of corrosion protection. Ultrasonic treatment for 20 min and stirring at room temperature for 24 h. Dopamine hydrochloride can self-polymerize to form polydopamine. Through the π-π interaction between dopamine hydrochloride and hexagonal boron nitride, a uniform and stable protective layer is formed around the hexagonal boron nitride, which not only improves the dispersibility of hexagonal boron nitride and reduces agglomeration, but also enhances the impact resistance and corrosion resistance. Vacuum filtration, the precipitate is washed with deionized water until the filtrate is colorless, and the product is vacuum dried at 60 ° C for 24 h to obtain polydopamine@hexagonal boron nitride.
[0095] (2) Dissolve 10 g of polydopamine@hexagonal boron nitride described in step (1) in 100 mL of 98% ethanol solution, add 3-aminopropyltriethoxysilane coupling agent APTES, and add 0.4 g of 3-aminopropyltriethoxysilane coupling agent APTES. Assemble APTES on polydopamine@hexagonal boron nitride by electrostatic action. Polydopamine has excellent adhesion and can improve the corrosion resistance of hexagonal boron nitride. APTES acts as an intermediate medium to improve the dispersibility and interfacial affinity of hexagonal boron nitride in the epoxy resin matrix. Ultrasonic treatment is performed for 10 min, and the mixture is stirred at 80° C. and 500 rpm for 5 h. Centrifuge at a centrifugal speed of 6000 rpm for 5 min. Wash the precipitate with anhydrous ethanol solution 5 times, and then vacuum dry at 60° C. for 24 h to obtain polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES.
[0096] The preparation method of the composite pigment and filler specifically comprises the following steps:
[0097] a. Dissolve 8.5g of alumina powder in 25mL of deionized water, add 0.5g of alumina dispersant and perform ultrasonic treatment for 30-50min, then mix with 25mL of 2.0% sodium alginate aqueous solution. Sodium alginate has good antibacterial effect and can effectively control microbial contamination, thereby preventing corrosion caused by microorganisms. Sodium alginate also has good ion exchange and adsorption capacity, and can adsorb a large amount of heavy metal ions, thereby reducing their corrosion to pigments, fillers and substrates. Then add sucrose powder, the amount of sucrose added is 2.5g. Sucrose acts as a pore-forming agent and volatilizes during the sintering process, thereby forming micron-level channels between alumina particles, increasing the number of pores inside the material, reducing the density, and reducing the mechanical properties. Stir evenly to obtain a ceramic slurry with an alumina solid content of 17%, and then the ceramic slurry is added. A 20 mL syringe was injected, and 50 mL of a 1.0% calcium chloride solution was dripped in when the dripping height was 5 cm. Then the ceramic slurry was immersed in the calcium chloride solution for 12 hours, solidified to form a spherical blank, washed with deionized water, immersed in anhydrous ethanol for 24 hours, dried, and then transferred to a pressureless sintering furnace, heated to 600°C at a rate of 3°C / min, and then heated to 1350°C at a rate of 5°C / min, and kept warm for 1 hour. The alumina porous ceramic microbeads prepared by this method are a lightweight non-metallic functional pigment filler with good thermal conductivity and heat resistance. The hollow structure can isolate heat, reduce temperature fluctuations on the surface of an object, reduce material aging or damage caused by temperature changes, and achieve an anti-corrosion effect. The alumina porous ceramic microbeads can also reduce the density of the coating, maintain the strength and durability of the coating, and enhance the protective effect of the coating.
[0098] b. Mix the alumina porous ceramic microbeads described in step a with polyethylene powder once. During the first mixing process, the mixing speed is 80 rpm and the mixing time is 5 min. Polyethylene, as a plastic, has good wear resistance, corrosion resistance and certain mechanical strength, and can protect the pipeline from corrosion by chemical substances. The alumina porous ceramic microbeads, due to their high hardness, high thermal stability and good thermal conductivity, play a role in enhancing wear resistance, high temperature resistance and heat insulation in the coating. The combination of the two materials can significantly improve the performance of the pipeline coating, so that it can adapt to more complex and harsh working environments. Then, mix it with talcum powder for a second time. During the second mixing process, the mixing speed is 200 rpm and the mixing time is 10 min to obtain a composite color filler. The addition of talcum powder can cooperate with the alumina porous ceramic microbeads to significantly improve the hardness, wear resistance, chemical corrosion resistance and other properties of the coating, thereby enhancing the protective effect of the pipeline coating, and reducing the high cost of using ceramic microbeads completely while ensuring performance.
[0099] This embodiment provides a method for preparing a corrosion-resistant pipeline coating material, which specifically includes the following steps:
[0100] S1. Add 0.8g polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES to 160mL deionized water, ultrasonicate for 10min, and set the obtained dispersion aside. Weigh L-glutamic acid and dissolve it in 50mL 4mg / mL sodium hydroxide solution. The amount of L-glutamic acid added is 1.5g. L-glutamic acid is a green corrosion inhibitor. The amino and carboxyl groups in it can form complexes with iron ions, reduce the activity of iron ions, and inhibit the corrosion of metals, thereby improving the corrosion resistance. Mechanically stir for 10min to obtain a uniform solution. Add dropwise to the dispersion, ultrasonicate for 10 minutes, stir for 24 hours at room temperature under nitrogen protection, centrifuge, wash the precipitate with anhydrous ethanol and deionized water in turn until neutral, dry, and attach L-glutamic acid to the surface of the structure of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES to obtain L-glutamic acid modified product. L-glutamic acid increases the interlayer spacing of the structure of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, effectively reduces the aggregation of nanoparticles, and also expands the diffusion path of the corrosive medium, thereby improving the barrier performance.
[0101] S2. The L-glutamic acid modifier described in step S1 is uniformly mixed with epoxy resin, compound pigments and fillers, curing agent, leveling agent and defoaming agent. The amino group and polar group of the L-glutamic acid modifier form covalent bonds with the epoxy group in the epoxy resin, which has better interfacial compatibility and is beneficial to improving the dispersibility of the L-glutamic acid modifier in the epoxy resin, thereby filling the tiny pores and depressions on the surface of the coating, making the coating surface more complete, improving the corrosion resistance and impact resistance, and making the connection between the coating and the substrate more firm, increasing the adhesion of the coating, and the compound pigments and fillers further enhance the barrier effect of the coating, making it difficult for the corrosive medium to penetrate into the interior of the coating, effectively blocking the corrosion ions from invading the coating substrate, and greatly improving the corrosion resistance of the coating. The mixture is extruded into sheets in a twin-screw extruder, the temperature of zone I of the extruder is 85° C., and the temperature of zone II is 100° C. Then the sheet material is ground in a desktop knife grinder with a screen aperture of 160 mesh to obtain a corrosion-resistant pipeline coating material.
[0102] Comparative Example 1
[0103] This comparative example provides a corrosion-resistant pipeline coating material, which is different from Example 1 in that the corrosion-resistant pipeline coating material does not contain polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES; the preparation method of the composite pigment and filler is the same as that of Example 1; the preparation method of the corrosion-resistant pipeline coating material does not contain a dispersion of polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES in step S1, and only contains a uniform solution of L-glutamic acid, and in step S2, the L-glutamic acid described in step S1 is uniformly mixed with the epoxy resin, the composite pigment and filler, the curing agent, the leveling agent and the defoaming agent, and the other contents are the same as those in Example 1.
[0104] Comparative Example 2
[0105] The present comparative example provides a corrosion-resistant pipeline coating material, which is different from Example 1 in that the corrosion-resistant pipeline coating material does not contain L-glutamic acid; the preparation method of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES is the same as that of Example 1; the preparation method of the compound pigment and filler is the same as that of Example 1; in the preparation method of the corrosion-resistant pipeline coating material, step S1 does not contain a uniform solution of L-glutamic acid, but only contains a dispersion of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, and in step S2, the polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES described in step S1 is uniformly mixed with epoxy resin, compound pigment and filler, curing agent, leveling agent and defoaming agent, and the other contents are the same as those in Example 1.
[0106] Comparative Example 3
[0107] This comparative example provides a corrosion-resistant pipeline coating material, which differs from Example 1 in that the composite pigment and filler does not contain alumina porous ceramic microbeads; the preparation method of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES is the same as that in Example 1; the preparation method of the composite pigment and filler does not include step a; the preparation method of the corrosion-resistant pipeline coating material is the same as that in Example 1.
[0108] Experimental Example 1
[0109] Corrosion resistance test
[0110] Test samples: corrosion-resistant pipeline coating materials prepared in Examples 1-4 and Comparative Examples 1-3.
[0111] Test method: According to the national standard GB / T1771-2007, the test sample is scratched with an X to the substrate, and a 3.5% by mass NaCl solution is sprayed (pH value is 6.5-7.2). The salt spray resistance test is carried out by continuous spraying for 500 hours. After the test, the rust is peeled off along the X scratch, and the length of the maximum corrosion of the substrate is measured, which is recorded as the maximum corrosion length (mm). The smaller the maximum corrosion length, the stronger the corrosion resistance.
[0112] Figure 3 The maximum corrosion length results of Examples 1-4 and Comparative Examples 1-3 are shown in FIG. Figure 3 , the maximum corrosion length of Examples 1-4 is 0.23-0.28 mm, indicating that the corrosion resistance is strong; the maximum corrosion length of Comparative Examples 1-3 is 0.34-0.45 mm, indicating that the corrosion resistance is weak; the corrosion-resistant pipeline coating material of Comparative Example 1 does not contain polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES, which cannot synergize with the compound pigment filler to play the filler role, weakening the filling effect of the pores generated by the curing of the epoxy resin, and also weakening the diffusion path of the corrosive medium, reducing the barrier performance to the corrosive medium, resulting in weak corrosion resistance; the corrosion-resistant pipeline coating material of Comparative Example 2 does not contain polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES, which cannot synergize with the compound pigment filler to play the filler role, weakening the filling effect of the pores generated by the curing of the epoxy resin, and also weakening the diffusion path of the corrosive medium, reducing the barrier performance to the corrosive medium, resulting in weak corrosion resistance; Containing L-glutamic acid, it is impossible to modify the polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, which is not conducive to increasing the interlayer spacing of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES and reducing its aggregation phenomenon, and it is also unable to produce a strong interface effect with the epoxy resin, which is not conducive to the integrity of the coating, resulting in weak corrosion resistance; the composite color filler of Comparative Example 3 does not contain alumina porous ceramic microbeads, and cannot effectively reduce the density of the filler, which is not conducive to maintaining the strength and durability of the coating, thereby adversely affecting the protective effect of the coating, resulting in weak corrosion resistance.
[0113] Experimental Example 2
[0114] Impact test
[0115] Test samples: corrosion-resistant pipeline coating materials prepared in Examples 1-4 and Comparative Examples 1-3.
[0116] Test method: According to GB / T1732-2020 Determination of impact resistance of paint film, use a paint film impactor to test the impact resistance of the coating. The greater the impact strength (cm), the better the impact resistance.
[0117] Figure 4 The impact strength results of Examples 1-4 and Comparative Examples 1-3 are shown in FIG. Figure 4The impact strength of Examples 1-4 is 65-70cm, all ≥ 65cm, indicating good impact resistance; the impact strength of Comparative Examples 1-3 is 45-55cm, all ≤ 55cm, indicating poor impact resistance; the corrosion-resistant pipeline coating material of Comparative Example 1 does not contain polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES, and cannot form a thick block of coating film, which is not conducive to filling cracks during coating curing and enhancing the protective effect on the substrate, resulting in poor impact resistance. Poor; the corrosion-resistant pipeline coating material of Comparative Example 2 does not contain L-glutamic acid, and cannot improve the dispersibility of polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES in epoxy resin, which is not conducive to the integrity of the coating surface, thereby weakening the ability to resist collision and impact, resulting in poor impact resistance; the composite color filler of Comparative Example 3 does not contain alumina porous ceramic microbeads, and cannot be matched with L-glutamic acid modifiers as fillers, which is not conducive to enhancing the barrier effect of the coating material, resulting in poor impact resistance.
[0118] Experimental Example 3
[0119] Adhesion test
[0120] Test samples: corrosion-resistant pipeline coating materials prepared in Examples 1-4 and Comparative Examples 1-3.
[0121] Test method: The test sample is measured by a pull-off adhesion tester in accordance with ASTM D4514. The pressure system is calibrated by NIST with an accuracy of ±1% (full scale) and a value accurate to 0.01.
[0122] Figure 5 1-4 and comparative examples 1-3. Figure 5 The adhesion of Examples 1-4 is 11.6-12.5MPa, indicating that the adhesion is good; the adhesion of Comparative Examples 1-3 is 9.2-10.8MPa, indicating that the adhesion is poor; the corrosion-resistant pipeline coating material of Comparative Example 1 does not contain polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES, and cannot form an adhesive thick block material, which is not conducive to enhancing the adhesion to the substrate, resulting in poor adhesion; the corrosion-resistant pipeline coating material of Comparative Example 2 does not contain L-glutamic acid, It is impossible to improve the dispersibility of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES in epoxy resin, and it is also impossible to form a dense cross-linked coating with the epoxy resin, which is not conducive to better adhesion to the substrate, resulting in poor adhesion; the composite pigment filler of comparative example 3 does not contain alumina porous ceramic microbeads, and cannot synergistically play the role of filler with the L-glutamic acid modifier, which is not conducive to improving the density of the coating, thereby not being conducive to strengthening the firm connection between the coating material and the substrate, resulting in poor adhesion.
[0123] The above experimental results show that the corrosion resistance, impact resistance and adhesion of Examples 1-4 of the present invention are significantly better than those of Comparative Examples 1-3. Among them, Example 1 using L-glutamic acid modified polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES and compounded pigments and fillers has stronger corrosion resistance, better impact resistance and better adhesion. The modification of polydopamine @ hexagonal boron nitride @ 3-aminopropyltriethoxysilane coupling agent APTES by L-glutamic acid increases the interlayer spacing of the structure and effectively reduces the aggregation and agglomeration phenomenon. At the same time, the amino group of L-glutamic acid undergoes a ring-opening reaction with the epoxy group of the epoxy resin, thereby improving the adhesion of polydopamine. @Hexagonal boron nitride@The dispersibility of 3-aminopropyltriethoxysilane coupling agent APTES in epoxy resin enables it to better fill the pores and cracks during coating curing, improve the integrity of the coating surface, and enhance the corrosion resistance and impact resistance. L-glutamic acid expands or blocks the diffusion path of the corrosive medium through dense cross-linking with the epoxy resin, making it difficult for the corrosive medium to pass through the coating and directly react with the substrate, thereby helping to enhance the corrosion resistance; the combination of compound pigments and fillers with L-glutamic acid modifiers enhances the barrier effect of the coating material, improves the corrosion resistance and impact resistance of the coating material, and also makes the connection between the coating material and the substrate more firmly.
[0124] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.
[0125] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A corrosion-resistant pipeline coating material, characterized in that: The raw materials for preparing the corrosion-resistant pipeline coating material include the following components in parts by weight: 8-10 parts of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES, 15-25 parts of L-glutamic acid, 80-100 parts of epoxy resin, 15-25 parts of compound pigments and fillers, 20-30 parts of curing agent, 3-5 parts of leveling agent, and 1-3 parts of defoaming agent; the raw materials for preparing the polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES include the following components in parts by weight: 10-12 parts of dopamine hydrochloride, 25-30 parts of hexagonal boron nitride, and 2-3 parts of 3-aminopropyltriethoxysilane coupling agent APTES; the compound pigments and fillers include the following components in parts by weight: 10-20 parts of alumina porous ceramic microbeads, 10-20 parts of polyethylene powder, and 10-20 parts of talc; The preparation method of the polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES specifically comprises the following steps: (1) Add 12.0 g of tris(hydroxymethyl)aminomethane to 900 mL of deionized water, adjust the pH to 8.0-8.5 with 0.1 mol / L hydrochloric acid solution, continue to add 2.0-2.4 g of dopamine hydrochloride and 5.0-6.0 g of hexagonal boron nitride solid powder, ultrasonically treat for 20-30 min, stir at room temperature for 24 h, vacuum filter, wash the precipitate with deionized water until the filtrate is colorless, and vacuum dry the product at 60 ° C for 24 h to obtain polydopamine@hexagonal boron nitride; (2) dissolving the polydopamine@hexagonal boron nitride described in step (1) in 100 mL of 98% ethanol solution, adding 3-aminopropyltriethoxysilane coupling agent APTES, ultrasonically treating for 10-20 min, stirring for 5-6 h at 60-80° C. and 400-500 rpm, centrifuging at a centrifugal speed of 5000-6000 rpm for 5-10 min, washing the precipitate with anhydrous ethanol solution for 3-5 times, and then vacuum drying at 60° C. for 24 h to obtain polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES; The preparation method of the porous alumina ceramic microbeads specifically comprises the following steps: dissolving 7.5-8.5 g of alumina powder in 25 mL of deionized water, adding 0.5 g of an alumina dispersant and performing ultrasonic treatment for 30-50 min, mixing with 25 mL of a sodium alginate aqueous solution with a mass fraction of 1.5-2.0%, then adding sucrose powder, stirring evenly, obtaining a ceramic slurry with an alumina solid phase content of 15-17%, and then injecting the ceramic slurry into a 20 mL syringe. When the dripping height is 1-5 cm, 50 mL of a calcium chloride solution with a mass fraction of 0.5-1.0% is dripped in, and then the ceramic slurry is immersed in the calcium chloride solution for 12 hours to solidify to form a spherical blank, which is then washed with deionized water and immersed in anhydrous ethanol for 24 hours, dried, and then transferred to a pressureless sintering furnace, heated to 500-600° C. at a rate of 3° C. / min, and then heated to 1250-1350° C. at a rate of 5° C. / min, and kept warm for 1 hour to obtain alumina porous ceramic microbeads; Specifically, the method comprises the following steps: adding 0.8-1.0g of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES into 160mL of deionized water, ultrasonicating for 10-30min, and setting aside the obtained dispersion; weighing L-glutamic acid and dissolving it in 50mL of 4mg / mL sodium hydroxide solution; mechanically stirring for 10-20min; adding the obtained uniform solution dropwise into the dispersion; ultrasonicating for 10-20min; stirring for 24h at room temperature under nitrogen protection; centrifuging; washing the precipitate with anhydrous ethanol and deionized water in turn until it is neutral; and drying to obtain L-glutamic acid modified product.
2. A method for preparing the corrosion-resistant pipeline coating material according to claim 1, characterized in that: The specific steps include: S1. Add 0.8-1.0g of polydopamine@hexagonal boron nitride@3-aminopropyltriethoxysilane coupling agent APTES to 160mL of deionized water, and ultrasonicate for 10-30min. The obtained dispersion is set aside. L-glutamic acid is weighed and dissolved in 50mL of 4mg / mL sodium hydroxide solution. Mechanical stirring is performed for 10-20min. The obtained uniform solution is added dropwise to the dispersion. Ultrasonication is performed for 10-20min. Stirring is performed at room temperature under nitrogen protection for 24h, and centrifugation is performed. The precipitate is washed with anhydrous ethanol and deionized water in turn until it is neutral, and dried to obtain L-glutamic acid modified product. S2. The modified L-glutamic acid described in step S1 is mixed evenly with epoxy resin, compound pigment and filler, curing agent, leveling agent and defoaming agent. The mixture is extruded into sheets in a twin-screw extruder. The temperature of zone I of the extruder is 65-85° C., and the temperature of zone II is 80-100° C. Then the sheet material is ground in a desktop knife grinder with a sieve aperture of 100-160 mesh to obtain a corrosion-resistant pipeline coating material.
3. The method for preparing the corrosion-resistant pipeline coating material according to claim 2, characterized in that: The preparation method of the composite pigment and filler specifically comprises the following steps: a. Dissolve 7.5-8.5g of alumina powder in 25mL of deionized water, add 0.5g of alumina dispersant and perform ultrasonic treatment for 30-50min, then mix with 25mL of sodium alginate aqueous solution with a mass fraction of 1.5-2.0%, then add sucrose powder and stir evenly to obtain a ceramic slurry with an alumina solid content of 15-17%, then inject the ceramic slurry into a 20mL syringe, and drip 50mL of a 0.5-1.0% calcium chloride solution at a drip height of 1-5cm, then soak the ceramic slurry in the calcium chloride solution for 12h, solidify to form a spherical blank, wash with deionized water, soak in anhydrous ethanol for 24h, dry, and then transfer to a pressureless sintering furnace, heat to 500-600℃ at a rate of 3℃ / min, and then heat to 1250-1350℃ at a rate of 5℃ / min, keep warm for 1h, and obtain alumina porous ceramic microbeads; b. Mix the alumina porous ceramic microbeads described in step a with polyethylene powder once, at a mixing speed of 60-80 rpm and a mixing time of 5-10 min, and then mix with talcum powder for a second time, at a mixing speed of 100-200 rpm and a mixing time of 10-15 min, to obtain a composite pigment and filler.
4. The method for preparing the corrosion-resistant pipeline coating material according to claim 3, characterized in that: In step a, the amount of sucrose added is 2.5-4.5 g.
Citation Information
Patent Citations
Nanometer composite ocean anticorrosion coating and preparation method thereof
CN109943169A
Composite material modified wear-resistant and corrosion-resistant coating as well as preparation method thereof
CN110527404A