Environment-friendly recycling treatment method of aluminum slag

By mixing aluminum slag with water or acid solution at a specific temperature, performing a hydrolysis reaction, grinding and drying, the problem of high energy consumption and pollution in the existing aluminum slag treatment methods is solved, and economical and environmentally friendly reuse of aluminum slag is achieved. Thermal conductive powder with high thermal conductivity.

CN118853101APending Publication Date: 2024-10-29DONGGUAN ZIITEK ELECTRONICAL MATERIAL & TECHNOLOGY LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410835311.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing aluminum slag treatment methods have problems such as high energy consumption, not environmentally friendly and may contaminate the manufacturing of high-purity aluminum. Traditional hydrolysis inhibition solutions consume a lot of energy, are difficult to control the thickness of the protective layer, and often produce toxic gases.

Method used

By mixing the screened aluminum slag with water or acid solution at a specific temperature, performing a hydrolysis reaction and then grinding, washing and drying, a thermally conductive powder with a high thermal conductivity coefficient is obtained. An aqueous solution of 5 to 80°C is used to control the reaction speed. Avoid high temperature heat and ammonia gas escape.

Benefits of technology

Economical and environmentally friendly aluminum slag reuse has been achieved. The thermally conductive powder obtained has high thermal conductivity and is easy to operate. It avoids the generation of toxic gases such as ammonia and reduces energy consumption and safety hazards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118853101A_ABST
    Figure CN118853101A_ABST
Patent Text Reader

Abstract

The invention provides an environment-friendly recycling treatment method of aluminum slag, which comprises the following steps: (1) screening the aluminum slag to obtain treated aluminum slag; (2) mixing the treated aluminum slag with an aqueous solution for reaction, and sequentially grinding, washing and drying to obtain heat-conducting powder; the aqueous solution comprises water or an acid solution; the temperature of the aqueous solution is 5-80 DEG C. The environment-friendly recycling treatment method for the aluminum slag is economical, environment-friendly, safe, efficient, capable of recycling heat conduction powder and suitable for large-scale application and popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of solid waste treatment, and in particular to an environmentally friendly recycling treatment method for aluminum slag. Background Art

[0002] The high-temperature smelting process of aluminum metal produces aluminum slag with complex components, mainly composed of aluminum oxides, nitrides, silicon oxides and their salts. Because it easily reacts with moisture to produce gases such as ammonia and a small amount of hydrogen, the common treatment method in the early days was to abandon or bury it, but this method releases toxic ammonia, so it is very environmentally unfriendly. Currently, the commercial bulk recycling plan is to recycle it in aluminum smelters and enter the aluminum smelting industry to be remade into metal aluminum for use, but it requires more complicated pre-treatment.

[0003] The main hydrolysis reaction of aluminum nitride is as follows:

[0004] AlN+3H2O→Al(OH)3+NH3

[0005] Traditional hydrolysis inhibition methods are to treat the aluminum nitride surface with hydrophobicity, such as coupling agents or surfactants, or directly perform high-temperature oxidation to form an Al2O3 film for protection, but this method is very energy-consuming. The oxidation of aluminum nitride can only occur at 1370°C, and it is difficult to control the thickness of the protective layer because the oxidation speed is very fast at this temperature.

[0006] Aluminum oxide and hydroxide are also common industrial raw materials. They can be used as thermal conductors, flame retardants, fillers, etc. The traditional method is to treat and purify bauxite through a strong alkali reaction such as sodium hydroxide, water washing, and then grind and bake it into suitable inorganic powder particles.

[0007] CN114933858A discloses an aluminum slag coating, which, based on the total weight, comprises 40% to 60% of an aluminum slag composition, 3% to 10% of a coupling agent, 30% to 50% of a resin, and the remainder of additives; wherein the aluminum slag composition is a powder formed by anhydrous grinding of an aluminum slag and a grinding aid, and the grinding aid is selected from at least one of alcohol amine polar molecules, polyols, unsaturated fatty acids, sodium stearate, minerals, styrene copolymers, and maleic anhydride derivatives.

[0008] CN212712780U discloses a kinetic energy dryer capable of treating aluminum slag ash, comprising a furnace body, which is an upright hollow body with a height of more than 12 meters, a closed top and a feeding port formed at the bottom; a heating device, whose heating pipe is connected to the outer periphery of the upper section of the furnace body and heats the interior of the furnace body with a heating nozzle; an aluminum slag ash feeding device, whose feeding nozzle sprays the aluminum slag ash into the furnace body at an upward tilt angle, swirling it to the top in a cyclone-like airflow, and the interior of the furnace body presents a decreasing distribution of 1400° C. to 600° C. from top to bottom, and the different airflow densities at the top and bottom cause a vortex kinetic energy effect, so that the aluminum slag ash moves downward in a natural falling manner, and then in the furnace body of more than 12 meters, by virtue of the full interaction of kinetic energy and thermal energy, an aluminum oxide powder product is formed, which is recovered from the feeding port at the bottom, achieving a high-value resource recycling effect.

[0009] TW202246533 discloses a recycled aluminum grinding aid, which uses polyethylene glycol as a main component and is used to contact and mix with the recycled aluminum through heating and spraying before the recycled aluminum is ball-milled, thereby forming a barrier layer on the surface of the recycled aluminum.

[0010] However, the above methods all use high energy or finished chemical products to treat aluminum slag, which is considered waste, which is not economically cost-effective or environmentally friendly. If the aluminum slag is directly sent to an aluminum smelter to reduce aluminum metal, the energy consumption is higher, which is not cost-effective from an economic perspective, and it often contains other metal impurities, which will pollute the production of high-purity aluminum. Summary of the invention

[0011] In view of the problems existing in the prior art, the present invention provides an environmentally friendly recycling treatment method for aluminum slag, which is obtained by mixing the screened aluminum slag with an aqueous solution at a specific temperature, performing a hydrolysis reaction, and then grinding, washing and drying to obtain a recyclable thermal conductive powder. The environmentally friendly recycling treatment method of the present invention is economical, environmentally friendly and has no safety hazards, and is suitable for large-scale promotion and application.

[0012] To achieve this object, the present invention adopts the following technical solutions:

[0013] The present invention provides an environmentally friendly recycling treatment method for aluminum slag, and the environmentally friendly recycling treatment method comprises the following steps:

[0014] (1) The aluminum slag is subjected to screening treatment to obtain treated aluminum slag;

[0015] (2) the treated aluminum slag is mixed with an aqueous solution for reaction, and then ground, washed with water and dried in sequence to obtain a thermally conductive powder;

[0016] The aqueous solution includes water or an acid solution; the temperature of the aqueous solution is 5-80°C.

[0017] The environmentally friendly recycling treatment method of aluminum slag described in the present invention first screens the aluminum slag to remove large wastes generated in the aluminum melting process and the environment, such as sand and gravel, unoxidized aluminum blocks and other impurities; then mixes with an aqueous solution to hydrolyze various components in the aluminum slag; after the reaction is completed, grinds, washes and dries to recover thermal conductive powder with a high thermal conductivity coefficient, which has certain economic value. Among them, the temperature of the aqueous solution is 5-80°C, which has economic and safety advantages. When the temperature of the aqueous solution is low, the hydrolysis reaction rate of aluminum nitride will be too slow, which will extend the time of the process and increase the cost; when the temperature of the aqueous solution is high, the hydrolysis reaction rate of aluminum nitride will be too fast, releasing a large amount of heat and ammonia, causing harm. In the present invention, the aluminum slag is mixed with an acid solution after treatment, and can be directly ground without the phenomenon of continuous heating after grinding. In this way, the time of pre-treatment can be saved, the amount of acid required is small, the occurrence of hydrolysis reaction can be suppressed, and no additional organic solvent is needed as a grinding medium. Moreover, because the solution is weakly acidic, if there is a trace of ammonia generated by hydrolysis, it will not escape. Since the hydrolysis reaction is suppressed, a considerable amount of aluminum nitride can still be retained, which helps to improve the thermal conductivity coefficient. The obtained thermal conductive powder includes aluminum oxide and aluminum nitride.

[0018] The environmentally friendly recycling treatment method of the present invention is simple to operate, economical and environmentally friendly, does not generate toxic and harmful gases such as ammonia during the treatment process, and the temperature during the grinding process is relatively low, so there is no safety hazard.

[0019] In the mixed reaction of the treated aluminum slag and the aqueous solution in step (2) of the present invention, when the aqueous solution is water, water at a relatively low temperature of 5 to 50° C. can be used to react with the treated aluminum slag first, and then water at a relatively high temperature of 60 to 80° C. can be used to continue the reaction, and grinding can be performed after no bubbles are generated.

[0020] The temperature of the aqueous solution of the present invention is 5 to 80°C, for example, it can be 5°C, 8°C, 10°C, 15°C, 20°C, 30°C, 50°C, 60°C, 70°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] Preferably, the composition of the aluminum slag in step (1) includes 20 to 90 wt% of aluminum oxide, for example, 20 wt%, 50 wt%, 60 wt%, 70 wt%, 75 wt%, 80 wt% or 90 wt%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0022] 5-50wt% aluminum nitride, for example, 5wt%, 10wt%, 20wt%, 25wt%, 30wt%, 40wt% or 50wt%, etc., but not limited to the listed values, other values ​​not listed within the numerical range are also applicable;

[0023] 0-30wt% silicon aluminum oxide, for example, can be 0wt%, 5wt%, 10wt%, 15wt%, 20wt%, 25wt% or 30wt%, etc., but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable;

[0024] and 0-60% aluminum hydroxide, for example, it can be 0wt%, 10wt%, 20wt%, 30wt%, 40wt%, 50wt% or 60wt%, etc., but it is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, the sieving process in step (1) uses a sieve of 60 to 100 mesh, for example, it can be 60 mesh, 65 mesh, 70 mesh, 80 mesh, 90 mesh, 95 mesh or 100 mesh, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the mass ratio of the treated aluminum slag and the aqueous solution in the mixed reaction in step (2) is 1:3 to 1:9, for example, it can be 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:8 or 1:9, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] The present invention preferably has a mass ratio of 1:3 to 1:9 for the mixed reaction of the treated aluminum slag and the aqueous solution, which has the advantages of being economical, environmentally friendly and having a fast reaction. When the mass of the mixed reaction of the treated aluminum slag and the aqueous solution is relatively small, the reaction will be slow and water resources will be consumed; when the mass of the mixed reaction of the treated aluminum slag and the aqueous solution is relatively large, excessive water consumption will result in increased product viscosity, which will increase the difficulty of recycling and treatment.

[0028] Preferably, the time for the mixed reaction of the treated aluminum slag and water in step (2) is 0.5 to 48 hours, for example, it can be 0.5 hours, 1 hour, 5 hours, 10 hours, 15 hours, 20 hours, 30 hours, 40 hours, 45 hours or 48 hours, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0029] In the present invention, the higher the temperature of the water, the shorter the mixing reaction time.

[0030] Preferably, the acid solution in step (2) comprises any one of citric acid solution, tartaric acid solution, oxalic acid solution, succinic acid solution or adipic acid solution, or a combination of at least two of them, wherein typical but non-limiting combinations include a combination of citric acid solution and tartaric acid solution, a combination of oxalic acid solution and succinic acid solution, a combination of adipic acid solution and citric acid solution, or a combination of tartaric acid solution and succinic acid solution.

[0031] Preferably, the mass concentration of the acid solution in step (2) is 0.5% to 5%, for example, it can be 0.5%, 0.8%, 1%, 1.2%, 2%, 3%, 4% or 5%, etc., but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; preferably 1.2%.

[0032] Preferably, when the treated aluminum slag is mixed with water for reaction, the obtained thermally conductive powder includes aluminum oxide and aluminum hydroxide.

[0033] Preferably, when the treated aluminum slag is mixed and reacted with an acid solution, the obtained thermally conductive powder includes aluminum oxide and aluminum nitride.

[0034] As a preferred technical solution of the present invention, the environmentally friendly recycling treatment method comprises the following steps:

[0035] (1) Aluminum slag is sieved through a 60-100 mesh screen to obtain treated aluminum slag; the aluminum slag comprises 20-90 wt% aluminum oxide, 5-50 wt% aluminum nitride, 0-30 wt% silicon aluminum oxide and 0-60% aluminum hydroxide;

[0036] (2) the treated aluminum slag is mixed with an aqueous solution for reaction, and then ground, washed with water and dried in sequence to obtain a thermally conductive powder;

[0037] The aqueous solution includes water or an acid solution; the temperature of the aqueous solution is 5 to 80° C.;

[0038] The mass ratio of the treated aluminum slag to the aqueous solution in the mixed reaction is 1:3 to 1:9;

[0039] The time for the treated aluminum slag to mix and react with water is 0.5 to 48 hours;

[0040] The acid solution comprises any one of citric acid solution, oxalic acid solution, malonic acid solution, tartaric acid solution or succinic acid solution, or a combination of at least two thereof; the mass concentration of the acid solution is 0.5% to 5%;

[0041] When the treated aluminum slag is mixed with water for reaction, the obtained thermal conductive powder includes aluminum oxide and aluminum hydroxide; when the treated aluminum slag is mixed with acid solution for reaction, the obtained thermal conductive powder includes aluminum oxide and aluminum nitride.

[0042] Compared with the prior art, the present invention has at least the following beneficial effects:

[0043] (1) The environmentally friendly recycling method of aluminum slag provided by the present invention is economical, environmentally friendly, safe and efficient, and can be recycled to obtain thermal conductive powder;

[0044] (2) The present invention provides an environmentally friendly recycling method for aluminum slag. The screened aluminum slag is mixed with an acid solution for reaction and can be directly ground without generating continuous heat after grinding, thus saving pre-treatment time and preventing ammonia gas from escaping and causing health hazards. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is a temperature change diagram of the entire water-containing product after grinding in Example 1 of the present invention.

[0046] Figure 2 It is a temperature change diagram of the entire water-containing product after grinding in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0047] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0048] The present invention is further described in detail below. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0049] Example 1

[0050] This embodiment provides an environmentally friendly recycling treatment method for aluminum slag, and the environmentally friendly recycling treatment method comprises the following steps:

[0051] (1) Aluminum slag is sieved through a 80-mesh sieve to obtain treated aluminum slag; the aluminum slag comprises 60 wt% aluminum oxide, 20 wt% aluminum nitride, 10 wt% silicon aluminum oxide and 10% aluminum hydroxide;

[0052] (2) The treated aluminum slag is mixed with water at 20° C. in a mass ratio of 1:9 for reaction for 5 hours, and then warm water at 40° C. is used to continue the reaction. After no bubbles are generated, the mixture is ground, washed with water, and dried in sequence to obtain a thermal conductive powder composed of aluminum oxide and aluminum hydroxide.

[0053] The aluminum nitride in the aluminum slag of this embodiment has been completely reacted during the hydrolysis process, so there is no problem of releasing ammonia. The subsequent grinding process is no longer reactive, so the general grinding procedure can be carried out without worrying about heating again and causing safety hazards.

[0054] Example 2

[0055] This embodiment provides an environmentally friendly recycling treatment method for aluminum slag, and the environmentally friendly recycling treatment method comprises the following steps:

[0056] (1) Aluminum slag is sieved through a 100-mesh sieve to obtain treated aluminum slag; the aluminum slag comprises 50 wt% aluminum oxide, 10 wt% aluminum nitride, 10 wt% silicon aluminum oxide and 30% aluminum hydroxide;

[0057] (2) The treated aluminum slag is mixed with a citric acid solution having a temperature of 10° C. and a mass concentration of 1.2% at a mass ratio of 1:5 for reaction for 4 hours, and then ground, washed with water and dried in sequence to obtain a thermal conductive powder composed of aluminum oxide and aluminum nitride.

[0058] The temperature change diagram of the whole water-containing product after grinding in this embodiment is as follows Figure 1 As shown, from Figure 1 It can be seen that the temperature of the mixed reaction of aluminum slag and citric acid solution is relatively low, not exceeding 40° C. Moreover, the reaction using citric acid solution is an acidic environment, which can inhibit the hydrolysis of aluminum nitride.

[0059] Example 3

[0060] This embodiment provides an environmentally friendly recycling treatment method for aluminum slag, and the environmentally friendly recycling treatment method comprises the following steps:

[0061] (1) Aluminum slag is sieved through a 60-mesh sieve to obtain treated aluminum slag; the aluminum slag comprises 70 wt% aluminum oxide, 5 wt% aluminum nitride, 5 wt% silicon aluminum oxide and 20% aluminum hydroxide;

[0062] (2) The treated aluminum slag is mixed with water at a temperature of 50° C. in a mass ratio of 1:3 for reaction for 48 hours, and then ground, washed with water and dried in sequence to obtain a thermal conductive powder composed of aluminum oxide and aluminum hydroxide.

[0063] Example 4

[0064] This embodiment provides an environmentally friendly recycling treatment method for aluminum slag, and the environmentally friendly recycling treatment method comprises the following steps:

[0065] (1) Aluminum slag is sieved through a 70-mesh sieve to obtain treated aluminum slag; the aluminum slag comprises 80 wt% aluminum oxide, 10 wt% aluminum nitride, 7 wt% silicon aluminum oxide and 3% aluminum hydroxide;

[0066] (2) The treated aluminum slag is mixed with an oxalic acid solution having a temperature of 30° C. and a mass concentration of 3% at a mass ratio of 1:6 for reaction for 12 hours, and then ground, washed with water and dried in sequence to obtain a thermal conductive powder composed of aluminum oxide and aluminum nitride.

[0067] Example 5

[0068] This embodiment provides an environmentally friendly recycling treatment method for aluminum slag, which is the same as Example 2 except that the mass concentration of the citric acid solution in step (2) is 0.1%.

[0069] Example 6

[0070] This embodiment provides an environmentally friendly recycling treatment method for aluminum slag, which is the same as Example 2 except that the mass concentration of the citric acid solution is 6%.

[0071] It can be seen from Example 1 and Examples 5 to 6 that the mass concentration of the citric acid solution in Example 5 is relatively low, which will result in the inability to effectively inhibit the hydrolysis reaction of aluminum nitride; and the mass concentration of the citric acid solution in Example 6 is relatively high, which will cause aluminum oxide to react with citric acid to produce salts or compounds.

[0072] Comparative Example 1

[0073] This comparative example provides a method for treating aluminum slag, wherein the aluminum slag and water are directly fed into a grinder at a mass ratio of 1:9 for grinding.

[0074] The temperature change diagram of the whole water-containing product after grinding in this comparative example is as follows Figure 2 As shown, it can be seen that the mixture of aluminum slag and water can reach a high temperature of about 90°C, almost boiling; in addition to the strong smell of ammonia, the gas methylhydrazine (CAS.No.60-34-4) can be detected through GC-MS.

[0075] Comparative Example 2

[0076] This comparative example provides an environmentally friendly recycling method for aluminum slag, which is the same as Example 2 except that the temperature of the citric acid solution in step (2) is 0°C.

[0077] Comparative Example 3

[0078] This comparative example provides an environmentally friendly recycling method for aluminum slag, which is the same as Example 2 except that the temperature of the citric acid solution in step (2) is 60°C.

[0079] It can be seen from Example 1 and Comparative Examples 2 to 3 that the temperature of the citric acid solution in Comparative Example 2 is relatively low, which will lead to the precipitation of citrate and silicate; and the temperature of the citric acid solution in Comparative Example 3 is relatively high, which will lead to excessive hydrolysis of aluminum nitride and release of excessive ammonia.

[0080] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A method for environmentally friendly recycling of aluminum slag, characterized in that: The environmentally friendly recycling treatment method comprises the following steps: (1) The aluminum slag is subjected to screening treatment to obtain treated aluminum slag; (2) the treated aluminum slag is mixed with an aqueous solution for reaction, and then ground, washed with water and dried in sequence to obtain a thermally conductive powder; The aqueous solution includes water or an acid solution; the temperature of the aqueous solution is 5 to 80° C.; The acid solution includes any one of citric acid solution, oxalic acid solution, malonic acid solution, tartaric acid solution or succinic acid solution, or a combination of at least two thereof.

2. The environmentally friendly recycling method according to claim 1, characterized in that: The aluminum slag in step (1) comprises 20-90 wt% aluminum oxide, 5-50 wt% aluminum nitride, 0-30 wt% silicon aluminum oxide and 0-60 wt% aluminum hydroxide.

3. The environmentally friendly recycling method according to claim 1 or 2, characterized in that: The screening process in step (1) uses a sieve of 60 to 100 meshes.

4. The environmentally friendly recycling method according to any one of claims 1 to 3, characterized in that: The mass ratio of the treated aluminum slag and the aqueous solution in the mixed reaction in step (2) is 1:3 to 1:

9.

5. The environmentally friendly recycling method according to any one of claims 1 to 4, characterized in that: The time for the reaction of the treated aluminum slag and water is 0.5 to 48 hours.

6. The environmentally friendly recycling method according to any one of claims 1 to 5, characterized in that: The mass concentration of the acid solution in step (2) is 0.5% to 5%.

7. The environmentally friendly recycling method according to claim 6, characterized in that: The mass concentration of the acid solution in step (2) is 1.2%.

8. The environmentally friendly recycling method according to any one of claims 1 to 7, characterized in that: When the treated aluminum slag is mixed with water for reaction, the resulting thermally conductive powder includes aluminum oxide and aluminum hydroxide.

9. The environmentally friendly recycling method according to any one of claims 1 to 8, characterized in that: When the treated aluminum slag is mixed with an acid solution for reaction, the resulting thermally conductive powder includes aluminum oxide and aluminum nitride.

10. The environmentally friendly recycling method according to any one of claims 1 to 9, characterized in that: The environmentally friendly recycling treatment method comprises the following steps: (1) Aluminum slag is sieved through a 60-100 mesh screen to obtain treated aluminum slag; the aluminum slag comprises 20-90 wt% aluminum oxide, 5-50 wt% aluminum nitride, 0-30 wt% silicon aluminum oxide and 0-60% aluminum hydroxide; (2) the treated aluminum slag is mixed with an aqueous solution for reaction, and then ground, washed with water and dried in sequence to obtain a thermally conductive powder; The aqueous solution includes water or an acid solution; the temperature of the aqueous solution is 5 to 80° C.; The mass ratio of the treated aluminum slag to the aqueous solution in the mixed reaction is 1:3 to 1:9; The time for the treated aluminum slag to mix with water is 0.5 to 48 hours; The acid solution comprises any one of citric acid solution, oxalic acid solution, malonic acid solution, tartaric acid solution or succinic acid solution, or a combination of at least two thereof; the mass concentration of the acid solution is 0.5% to 5%; When the treated aluminum slag is mixed with water for reaction, the obtained thermal conductive powder includes aluminum oxide and aluminum hydroxide; when the treated aluminum slag is mixed with acid solution for reaction, the obtained thermal conductive powder includes aluminum oxide and aluminum nitride.

Citation Information

Patent Citations

  • Aluminum slag coating

    CN114933858A

  • Kinetic energy dryer capable of treating aluminum slag ash