A thermal treatment process for bamboo and its application in biofuel

Through impregnation treatment, saturated steam heat treatment and low-temperature pyrolysis in bamboo, catalytic sites are constructed and high-temperature cracking is performed, the problem of low quality of pyrolysis bio-oil in bamboo is solved, and the yield and quality of bio-oil is improved, making it suitable for Preparation of biofuel.

CN118853219BActive Publication Date: 2024-12-06HUNAN INSTITUTE OF ENGINEERING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411356423.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-12-06
Estimated Expiration
2044-09-27

AI Technical Summary

Technical Problem

The bio-oil obtained by pyrolysis of bamboo has complex composition and low quality, making it difficult to effectively utilize.

Method used

Using a bamboo heat treatment processing process, including impregnation treatment, saturated steam heat treatment and low-temperature pyrolysis, catalytic active metal and maleic anhydride are distributed in the internal pores of bamboo, internal pores and in-situ catalytic sites are constructed, and finally, rapid through high temperature Cracking to prepare bamboo-derived bio-oil.

Benefits of technology

It improves the yield of bamboo-derived bio-oil, reduces moisture content and ingredient complexity, and improves quality, making it suitable for the preparation of biofuel oil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the field of fuel technology, and in particular to a heat treatment process for bamboo and its application in biofuel. The heat treatment process for bamboo includes (1) preparing a treatment liquid, (2) an immersion treatment, (3) a saturated steam heat treatment, (4) low-temperature pyrolysis, and (5) high-temperature pyrolysis; the treatment liquid is prepared from zinc nitrate hexahydrate, copper nitrate trihydrate, maleic anhydride and deionized water. The present invention effectively improves the calorific value of bamboo-derived bio-oil through immersion treatment, saturated steam heat treatment and low-temperature pyrolysis treatment, reduces the complexity of bamboo-derived bio-oil components, greatly improves the quality, and can be used for the preparation of biofuel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fuel, and in particular to a heat treatment process of bamboo and its application in biofuel. Background Art

[0002] With the increasing awareness of environmental protection and the demand for renewable energy, biofuels, as a renewable and clean energy form, have gradually attracted the attention of researchers. Among the many biomass resources, bamboo has become an ideal biofuel raw material due to its fast growth rate, abundant resources, and rich cellulose and lignin. However, the traditional bamboo pyrolysis process has some challenges in the extraction and utilization of bio-oil.

[0003] Pyrolysis of bamboo refers to the process of bamboo decomposing at high temperature to form solid, liquid and gas products under anaerobic or anoxic conditions. Studies have shown that bamboo pyrolysis can effectively produce bio-oil, charcoal and gaseous fuel. Bio-oil is an important liquid product in the pyrolysis process of bamboo, containing a variety of organic compounds such as phenols, aldehydes, acids and ketones. However, the bio-oil currently obtained from bamboo pyrolysis is often difficult to use directly as fuel due to its complex composition and low quality.

[0004] In the face of the above challenges, researchers have developed some improved pyrolysis technologies, such as catalytic pyrolysis, ultrasound-assisted pyrolysis, etc. Although these technologies have improved the yield and quality of bio-oil to a certain extent, the pyrolysis conditions still need to be further optimized to improve the availability of bio-oil. Summary of the invention

[0005] In view of this, the purpose of the present invention is to propose a heat treatment process for bamboo and its application in biofuel, so as to solve the problem that the bio-oil obtained by rapid pyrolysis of bamboo has complex components, low quality and is difficult to effectively utilize.

[0006] Based on the above purpose, the present invention provides a bamboo heat treatment process, comprising the following steps:

[0007] (1) preparing a treatment solution: adding zinc nitrate hexahydrate, copper nitrate trihydrate and maleic anhydride to deionized water and stirring for 25-35 minutes to obtain a treatment solution;

[0008] (2) Impregnation treatment: the bamboo powder is immersed in a treatment liquid for impregnation treatment to obtain wet bamboo powder;

[0009] (3) Saturated steam heat treatment: subjecting the wet bamboo powder to saturated steam heat treatment to obtain saturated steam heat treated bamboo powder;

[0010] (4) Low-temperature pyrolysis: The saturated steam heat-treated bamboo powder is subjected to low-temperature pyrolysis in a mixed atmosphere of nitrogen and hydrogen at a pyrolysis temperature of 240-260°C and a heat preservation time of 50-70 minutes to obtain low-temperature pyrolysis bamboo powder;

[0011] (5) High-temperature pyrolysis: The low-temperature pyrolysis bamboo powder was subjected to high-temperature pyrolysis. The pyrolysis heating rate was 10°C / ms, the pyrolysis temperature was 650°C, and the pyrolysis time was 15 s. The solid product, liquid product and gas product were collected separately. The liquid product was the bamboo-derived bio-oil.

[0012] Furthermore, in step (1), the molar ratio of zinc nitrate hexahydrate, copper nitrate trihydrate and maleic anhydride is 1:0.3-0.7:1.5-2.5.

[0013] Preferably, the amount of deionized water added in step (1) is twice the total weight of zinc nitrate hexahydrate, copper nitrate trihydrate and maleic anhydride.

[0014] Preferably, the impregnation step in step (2) is: pre-impregnation for 3 h in a vacuum drying oven at a vacuum degree of 0.01 MPa, followed by pressurized impregnation for 3 h in a pressure tank at 0.7 MPa.

[0015] Preferably, in step (3), the pressure of the saturated steam is 5 MPa, the temperature is 150° C., and the treatment time is 120 min.

[0016] Preferably, in step (4), the volume ratio of nitrogen to hydrogen in the mixed gas is 10:1, and the flow rate of the mixed gas is 200 ml / min.

[0017] Preferably, the heating rate of the low-temperature pyrolysis in step (4) is 10°C / min.

[0018] Preferably, the high-temperature pyrolysis in step (5) is carried out in a pyrolysis apparatus.

[0019] Furthermore, the present invention also provides an application of bamboo-derived bio-oil, which can be used for the preparation of bio-fuel.

[0020] Beneficial effects of the present invention:

[0021] The invention provides a heat treatment process for bamboo, wherein catalytically active metals and maleic anhydride are distributed in the internal pores of the bamboo by impregnation treatment, and the internal pores are constructed by saturated steam treatment and the action of maleic anhydride, while the catalytically active metals are evenly distributed in the internal pores, and then acidic catalytic sites are constructed in situ by low-temperature reduction, and finally bamboo-derived bio-oil is prepared by high-temperature rapid cracking.

[0022] The heat treatment process adopted by the present invention effectively improves the yield of bamboo-derived bio-oil through impregnation treatment, saturated steam heat treatment and low-temperature pyrolysis treatment. The prepared bamboo-derived bio-oil has low water content and high calorific value. In addition, through the construction of in-situ catalytic sites, the complexity of the bamboo-derived bio-oil components is effectively reduced, the quality is greatly improved, and it can be used for the preparation of biofuel. DETAILED DESCRIPTION

[0023] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.

[0024] Embodiment 1:

[0025] (1) Preparation of treatment solution: Add 29.75 g of zinc nitrate hexahydrate, 12.08 g of copper nitrate trihydrate and 15.58 g of maleic anhydride to 114.82 g of deionized water and stir for 30 min to obtain a treatment solution;

[0026] (2) Impregnation treatment: The bamboo is crushed, passed through a 40-mesh sieve, and then immersed in the treatment liquid. The pre-impregnation treatment is carried out in a vacuum drying oven with a vacuum degree of 0.01 MPa for 3 h, and then pressurized in a pressure tank at 0.7 MPa for 3 h to obtain wet bamboo powder.

[0027] (3) Saturated steam heat treatment: The wet bamboo powder was placed in a saturated steam pressure tank for saturated steam heat treatment. The saturated steam pressure was set to 5 MPa, the temperature was 150 °C, and the treatment time was 120 min. After the treatment, it was dried at 80 °C for 12 h and ground through a 100-mesh sieve to obtain saturated steam heat-treated bamboo powder.

[0028] (4) Low-temperature pyrolysis: The saturated steam heat-treated bamboo powder was placed on a ceramic dish, and heated to 250°C at a rate of 10°C / min in a mixed atmosphere of nitrogen and hydrogen (volume ratio of 10:1) at a flow rate of 200 ml / min, and kept at that temperature for 60 min, and cooled to room temperature to obtain low-temperature pyrolysis bamboo powder;

[0029] (5) High-temperature pyrolysis: The low-temperature pyrolysis bamboo powder is placed between two layers of quartz wool in a quartz tube and placed in a pyrolysis instrument for high-temperature pyrolysis. The pyrolysis heating rate is 10°C / ms, the pyrolysis temperature is 650°C, and the pyrolysis time is 15 s. The solid product, liquid product, and gas product are collected separately. The liquid product is the bamboo-derived bio-oil.

[0030] Embodiment 2:

[0031] (1) Preparation of treatment solution: Add 29.75 g of zinc nitrate hexahydrate, 7.25 g of copper nitrate trihydrate and 11.69 g of maleic anhydride to 97.38 g of deionized water and stir for 30 min to obtain a treatment solution;

[0032] (2) Impregnation treatment: The bamboo is crushed, passed through a 40-mesh sieve, and then immersed in the treatment liquid. The pre-impregnation treatment is carried out in a vacuum drying oven with a vacuum degree of 0.01 MPa for 3 h, and then pressurized in a pressure tank at 0.7 MPa for 3 h to obtain wet bamboo powder.

[0033] (3) Saturated steam heat treatment: The wet bamboo powder was placed in a saturated steam pressure tank for saturated steam heat treatment. The saturated steam pressure was set to 5 MPa, the temperature was 150 °C, and the treatment time was 120 min. After the treatment, it was dried at 80 °C for 12 h and ground through a 100-mesh sieve to obtain saturated steam heat-treated bamboo powder.

[0034] (4) Low-temperature pyrolysis: The saturated steam heat-treated bamboo powder was placed on a ceramic dish, and heated to 240°C at a rate of 10°C / min in a mixed atmosphere of nitrogen and hydrogen (volume ratio of 10:1) at a flow rate of 200 ml / min, and kept at that temperature for 50 min, and cooled to room temperature to obtain low-temperature pyrolysis bamboo powder;

[0035] (5) High-temperature pyrolysis: The low-temperature pyrolysis bamboo powder is placed between two layers of quartz wool in a quartz tube and placed in a pyrolysis instrument for high-temperature pyrolysis. The pyrolysis heating rate is 10°C / ms, the pyrolysis temperature is 650°C, and the pyrolysis time is 15 s. The solid product, liquid product, and gas product are collected separately. The liquid product is the bamboo-derived bio-oil.

[0036] Embodiment 3:

[0037] (1) Preparation of treatment solution: Add 29.75 g of zinc nitrate hexahydrate, 16.91 g of copper nitrate trihydrate and 19.48 g of maleic anhydride to 132.28 g of deionized water and stir for 30 min to obtain a treatment solution;

[0038] (2) Impregnation treatment: The bamboo is crushed, passed through a 40-mesh sieve, and then immersed in the treatment liquid. The pre-impregnation treatment is carried out in a vacuum drying oven with a vacuum degree of 0.01 MPa for 3 h, and then pressurized in a pressure tank at 0.7 MPa for 3 h to obtain wet bamboo powder.

[0039] (3) Saturated steam heat treatment: The wet bamboo powder was placed in a saturated steam pressure tank for saturated steam heat treatment. The saturated steam pressure was set to 5 MPa, the temperature was 150 °C, and the treatment time was 120 min. After the treatment, it was dried at 80 °C for 12 h and ground through a 100-mesh sieve to obtain saturated steam heat-treated bamboo powder.

[0040] (4) Low-temperature pyrolysis: The saturated steam heat-treated bamboo powder was placed on a ceramic dish, and heated to 260°C at a rate of 10°C / min in a mixed atmosphere of nitrogen and hydrogen (volume ratio of 10:1) at a flow rate of 200 ml / min, and kept at that temperature for 70 min, and cooled to room temperature to obtain low-temperature pyrolysis bamboo powder;

[0041] (5) High-temperature pyrolysis: The low-temperature pyrolysis bamboo powder is placed between two layers of quartz wool in a quartz tube and placed in a pyrolysis instrument for high-temperature pyrolysis. The pyrolysis heating rate is 10°C / ms, the pyrolysis temperature is 650°C, and the pyrolysis time is 15 s. The solid product, liquid product, and gas product are collected separately. The liquid product is the bamboo-derived bio-oil.

[0042] Comparative Example 1:

[0043] The difference between Comparative Example 1 and Example 1 is that: in Comparative Example 1, no impregnation treatment is performed, and the dry bamboo powder that has been crushed and passed through a 40-mesh sieve is directly subjected to saturated steam heat treatment;

[0044] The specific preparation steps are as follows:

[0045] (1) Saturated steam heat treatment: The bamboo is crushed, passed through a 40-mesh sieve, and then placed in a saturated steam pressure tank for saturated steam heat treatment. The saturated steam pressure is set to 5 MPa, the temperature is 150°C, and the treatment time is 120 min. After the treatment, it is dried at 80°C for 12 h and ground to pass through a 100-mesh sieve to obtain saturated steam heat-treated bamboo powder.

[0046] (2) Low-temperature pyrolysis: The saturated steam heat-treated bamboo powder was placed on a ceramic dish, and heated to 250°C at a rate of 10°C / min in a mixed atmosphere of nitrogen and hydrogen (volume ratio of 10:1) at a flow rate of 200 ml / min, and kept at that temperature for 60 min, and cooled to room temperature to obtain low-temperature pyrolysis bamboo powder;

[0047] (3) High-temperature pyrolysis: The low-temperature pyrolysis bamboo powder is placed between two layers of quartz wool in a quartz tube and placed in a pyrolysis instrument for high-temperature pyrolysis. The pyrolysis heating rate is 10°C / ms, the pyrolysis temperature is 650°C, and the pyrolysis time is 15s. The solid product, liquid product, and gas product are collected separately. The liquid product is the bamboo-derived bio-oil.

[0048] Comparative Example 2:

[0049] The difference between Comparative Example 2 and Example 1 is that zinc nitrate hexahydrate is not added to the treatment solution;

[0050] The specific preparation steps are as follows:

[0051] (1) Preparation of treatment solution: Add 12.08 g of copper nitrate trihydrate and 15.58 g of maleic anhydride to 114.82 g of deionized water and stir for 30 min to obtain a treatment solution;

[0052] (2) Impregnation treatment: The bamboo is crushed, passed through a 40-mesh sieve, and then immersed in the treatment liquid. The pre-impregnation treatment is carried out in a vacuum drying oven with a vacuum degree of 0.01 MPa for 3 h, and then pressurized in a pressure tank at 0.7 MPa for 3 h to obtain wet bamboo powder.

[0053] (3) Saturated steam heat treatment: The wet bamboo powder was placed in a saturated steam pressure tank for saturated steam heat treatment. The saturated steam pressure was set to 5 MPa, the temperature was 150 °C, and the treatment time was 120 min. After the treatment, it was dried at 80 °C for 12 h and ground through a 100-mesh sieve to obtain saturated steam heat-treated bamboo powder.

[0054] (4) Low-temperature pyrolysis: The saturated steam heat-treated bamboo powder was placed on a ceramic dish, and heated to 250°C at a rate of 10°C / min in a mixed atmosphere of nitrogen and hydrogen (volume ratio of 10:1) at a flow rate of 200 ml / min, and kept at that temperature for 60 min, and cooled to room temperature to obtain low-temperature pyrolysis bamboo powder;

[0055] (5) High-temperature pyrolysis: The low-temperature pyrolysis bamboo powder is placed between two layers of quartz wool in a quartz tube and placed in a pyrolysis instrument for high-temperature pyrolysis. The pyrolysis heating rate is 10°C / ms, the pyrolysis temperature is 650°C, and the pyrolysis time is 15 s. The solid product, liquid product, and gas product are collected separately. The liquid product is the bamboo-derived bio-oil.

[0056] Comparative Example 3:

[0057] The difference between Comparative Example 3 and Example 1 is that no copper nitrate trihydrate is added to the treatment solution;

[0058] The specific preparation steps are as follows:

[0059] (1) Preparation of treatment solution: Add 29.75 g of zinc nitrate hexahydrate and 15.58 g of maleic anhydride to 114.82 g of deionized water and stir for 30 min to obtain a treatment solution;

[0060] (2) Impregnation treatment: The bamboo is crushed, passed through a 40-mesh sieve, and then immersed in the treatment liquid. The pre-impregnation treatment is carried out in a vacuum drying oven with a vacuum degree of 0.01 MPa for 3 h, and then pressurized in a pressure tank at 0.7 MPa for 3 h to obtain wet bamboo powder.

[0061] (3) Saturated steam heat treatment: The wet bamboo powder was placed in a saturated steam pressure tank for saturated steam heat treatment. The saturated steam pressure was set to 5 MPa, the temperature was 150 °C, and the treatment time was 120 min. After the treatment, it was dried at 80 °C for 12 h and ground through a 100-mesh sieve to obtain saturated steam heat-treated bamboo powder.

[0062] (4) Low-temperature pyrolysis: The saturated steam heat-treated bamboo powder was placed on a ceramic dish, and heated to 250°C at a rate of 10°C / min in a mixed atmosphere of nitrogen and hydrogen (volume ratio of 10:1) at a flow rate of 200 ml / min, and kept at that temperature for 60 min, and cooled to room temperature to obtain low-temperature pyrolysis bamboo powder;

[0063] (5) High-temperature pyrolysis: The low-temperature pyrolysis bamboo powder is placed between two layers of quartz wool in a quartz tube and placed in a pyrolysis instrument for high-temperature pyrolysis. The pyrolysis heating rate is 10°C / ms, the pyrolysis temperature is 650°C, and the pyrolysis time is 15 s. The solid product, liquid product, and gas product are collected separately. The liquid product is the bamboo-derived bio-oil.

[0064] Comparative Example 4:

[0065] The difference between Comparative Example 4 and Example 1 is that no maleic anhydride is added to the treatment liquid;

[0066] The specific steps are as follows:

[0067] (1) Preparation of treatment solution: Add 29.75 g of zinc nitrate hexahydrate and 12.08 g of copper nitrate trihydrate into 114.82 g of deionized water and stir for 30 min to obtain a treatment solution;

[0068] (2) Impregnation treatment: The bamboo is crushed, passed through a 40-mesh sieve, and then immersed in the treatment liquid. The pre-impregnation treatment is carried out in a vacuum drying oven with a vacuum degree of 0.01 MPa for 3 h, and then pressurized in a pressure tank at 0.7 MPa for 3 h to obtain wet bamboo powder.

[0069] (3) Saturated steam heat treatment: The wet bamboo powder was placed in a saturated steam pressure tank for saturated steam heat treatment. The saturated steam pressure was set to 5 MPa, the temperature was 150 °C, and the treatment time was 120 min. After the treatment, it was dried at 80 °C for 12 h and ground through a 100-mesh sieve to obtain saturated steam heat-treated bamboo powder.

[0070] (4) Low-temperature pyrolysis: The saturated steam heat-treated bamboo powder was placed on a ceramic dish, and heated to 250°C at a rate of 10°C / min in a mixed atmosphere of nitrogen and hydrogen (volume ratio of 10:1) at a flow rate of 200 ml / min, and kept at that temperature for 60 min, and cooled to room temperature to obtain low-temperature pyrolysis bamboo powder;

[0071] (5) High-temperature pyrolysis: The low-temperature pyrolysis bamboo powder is placed between two layers of quartz wool in a quartz tube and placed in a pyrolysis instrument for high-temperature pyrolysis. The pyrolysis heating rate is 10°C / ms, the pyrolysis temperature is 650°C, and the pyrolysis time is 15 s. The solid product, liquid product, and gas product are collected separately. The liquid product is the bamboo-derived bio-oil.

[0072] Comparative Example 5:

[0073] The difference between Comparative Example 5 and Example 1 is that the bamboo powder is directly subjected to high temperature cracking by heat treatment with saturated steam;

[0074] The specific steps are as follows:

[0075] (1) Preparation of treatment solution: Add 29.75 g of zinc nitrate hexahydrate, 12.08 g of copper nitrate trihydrate and 15.58 g of maleic anhydride to 114.82 g of deionized water and stir for 30 min to obtain a treatment solution;

[0076] (2) Impregnation treatment: The bamboo is crushed, passed through a 40-mesh sieve, and then immersed in the treatment liquid. The pre-impregnation treatment is carried out in a vacuum drying oven with a vacuum degree of 0.01 MPa for 3 h, and then pressurized in a pressure tank at 0.7 MPa for 3 h to obtain wet bamboo powder.

[0077] (3) Saturated steam heat treatment: The wet bamboo powder was placed in a saturated steam pressure tank for saturated steam heat treatment. The saturated steam pressure was set to 5 MPa, the temperature was 150 °C, and the treatment time was 120 min. After the treatment, it was dried at 80 °C for 12 h and ground through a 100-mesh sieve to obtain saturated steam heat-treated bamboo powder.

[0078] (4) High-temperature pyrolysis: The saturated steam heat-treated bamboo powder was placed between two layers of quartz wool in a quartz tube and placed in a pyrolysis instrument for high-temperature pyrolysis. The pyrolysis heating rate was 10°C / ms, the pyrolysis temperature was 650°C, and the pyrolysis time was 15 s. The solid product, liquid product, and gas product were collected separately. The liquid product was the bamboo-derived bio-oil.

[0079] Comparative Example 6:

[0080] The difference between Comparative Example 6 and Example 1 is that the atmosphere of low-temperature pyrolysis is a nitrogen atmosphere.

[0081] (1) Preparation of treatment solution: Add 29.75 g of zinc nitrate hexahydrate, 12.08 g of copper nitrate trihydrate and 15.58 g of maleic anhydride to 114.82 g of deionized water and stir for 30 min to obtain a treatment solution;

[0082] (2) Impregnation treatment: The bamboo is crushed, passed through a 40-mesh sieve, and then immersed in the treatment liquid. The pre-impregnation treatment is carried out in a vacuum drying oven with a vacuum degree of 0.01 MPa for 3 h, and then pressurized in a pressure tank at 0.7 MPa for 3 h to obtain wet bamboo powder.

[0083] (3) Saturated steam heat treatment: The wet bamboo powder was placed in a saturated steam pressure tank for saturated steam heat treatment. The saturated steam pressure was set to 5 MPa, the temperature was 150 °C, and the treatment time was 120 min. After the treatment, it was dried at 80 °C for 12 h and ground through a 100-mesh sieve to obtain saturated steam heat-treated bamboo powder.

[0084] (4) Low-temperature pyrolysis: The saturated steam heat-treated bamboo powder was placed on a ceramic dish, and the temperature was raised to 250°C at a rate of 10°C / min under a nitrogen atmosphere with a nitrogen flow rate of 200 ml / min. The temperature was kept at this temperature for 60 min and cooled to room temperature to obtain low-temperature pyrolysis bamboo powder.

[0085] (5) High-temperature pyrolysis: The low-temperature pyrolysis bamboo powder is placed between two layers of quartz wool in a quartz tube and placed in a pyrolysis instrument for high-temperature pyrolysis. The pyrolysis heating rate is 10°C / ms, the pyrolysis temperature is 650°C, and the pyrolysis time is 15 s. The solid product, liquid product, and gas product are collected separately. The liquid product is the bamboo-derived bio-oil.

[0086] Performance Test:

[0087] Distribution of pyrolysis products: The yields of solid products and liquid products are calculated by weighing, and the gas yield is estimated, which is calculated by deducting the weight of carbon products and oil products from the total material. However, the actual loss in the logistics pipeline is not taken into account, and a mass balance state is assumed. The results are shown in Table 1.

[0088] Physical properties of bio-oil: The water content of bio-oil was determined by Karl Fischer titration method, and the calorific value of bio-oil was determined by oxygen bomb calorimeter method. The results are shown in Table 2.

[0089] Bio-oil product analysis: The analysis was performed using gas chromatography-mass spectrometry. The results are shown in Table 3.

[0090] Table 1 Distribution of pyrolysis products

[0091]

[0092] It can be seen from the data of Examples 1-3 in Table 1 that the liquid product accounts for more than 40% of the products obtained by the bamboo heat treatment process of the present invention. It can be seen from the data of Example 1 and Comparative Examples 1-6 that the impregnation treatment, saturated steam heat treatment and low-temperature pyrolysis treatment adopted by the present invention are all helpful to increase the proportion of liquid products.

[0093] Table 2 Physical properties of bio-oil

[0094]

[0095] It can be seen from the data of Examples 1-3 in Table 2 that the bamboo-derived bio-oil prepared by the present invention has a lower water content and a higher calorific value. It can be seen from the data of Example 1 and Comparative Examples 1-6 that the impregnation treatment of the present invention does not increase the water content of the bio-oil, but greatly improves the calorific value. In addition, low-temperature pyrolysis helps to reduce the water content. This may be because low-temperature pyrolysis causes cellulose degradation and construction of internal pores, which further releases the internal bound water.

[0096] Table 3 Analysis of bio-oil products

[0097]

[0098] From the data of Examples 1-3 in Table 3, it can be seen that the bamboo-derived bio-oil prepared by the present invention contains a high content of aromatic hydrocarbons, and the content of phenol is as low as less than 1%, which indicates that a large amount of phenols are converted into aromatic hydrocarbons, reducing the complexity of the bio-oil components and improving the quality.

[0099] It can be seen from the data of Example 1 and Comparative Examples 1-4 in Table 3 that the impregnation treatment helps to increase the content of aromatic hydrocarbons and reduce the content of phenol in the bio-oil, and improve the conversion rate of phenol to aromatic hydrocarbons. This is mainly due to the introduction of catalytically active zinc and copper. Under the action of maleic anhydride, zinc and copper are uniformly distributed inside the bamboo through impregnation, thereby constructing in-situ catalytic sites.

[0100] It can be seen from the data of Example 1 and Comparative Examples 5-6 in Table 3 that low-temperature pyrolysis has a significant effect on the enrichment of aromatic hydrocarbons. This is mainly because low-temperature pyrolysis, on the one hand, promotes the degradation of cellulose and removes some oxygen-containing functional groups, and on the other hand, activates zinc and copper, constructs in situ strong acid sites, which is beneficial to the conversion of phenols to aromatic hydrocarbons.

[0101] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

Claims

1. A heat treatment process for bamboo materials. It is characterized in that The following steps are involved: (1) preparing a treatment solution: adding zinc nitrate hexahydrate, copper nitrate trihydrate and maleic anhydride to deionized water and stirring for 25-35 minutes to obtain a treatment solution; (2) Impregnation treatment: the bamboo powder is immersed in a treatment liquid for impregnation treatment to obtain wet bamboo powder; (3) Saturated steam heat treatment: subjecting the wet bamboo powder to saturated steam heat treatment to obtain saturated steam heat treated bamboo powder; (4) Low-temperature pyrolysis: The saturated steam heat-treated bamboo powder is subjected to low-temperature pyrolysis in a mixed atmosphere of nitrogen and hydrogen at a pyrolysis temperature of 240-260°C and a heat preservation time of 50-70 minutes to obtain low-temperature pyrolysis bamboo powder; (5) High-temperature pyrolysis: The low-temperature pyrolysis bamboo powder was subjected to high-temperature pyrolysis, with a pyrolysis heating rate of 10°C / ms, a pyrolysis temperature of 650°C, and a pyrolysis time of 15 s. Solid products, liquid products, and gas products were collected separately, of which the liquid product was bamboo-derived bio-oil. In the step (1), the molar ratio of zinc nitrate hexahydrate, copper nitrate trihydrate and maleic anhydride is 1:0.3-0.7:1.5-2.

5.

2. The heat treatment process of bamboo material according to claim 1, It is characterized in that The amount of deionized water added in step (1) is twice the total weight of zinc nitrate hexahydrate, copper nitrate trihydrate and maleic anhydride.

3. The heat treatment process of bamboo material according to claim 1, It is characterized in that The impregnation process in step (2) is as follows: pre-impregnation in a vacuum drying oven at a vacuum degree of 0.01 MPa for 3 h, followed by pressurized impregnation in a pressure tank at 0.7 MPa for 3 h.

4. The heat treatment process of bamboo material according to claim 1, It is characterized in that In step (3), the pressure of saturated steam is 5 MPa, the temperature is 150° C., and the treatment time is 120 min.

5. The heat treatment process of bamboo material according to claim 1, It is characterized in that In step (4), the volume ratio of nitrogen to hydrogen in the mixed gas is 10:1, and the flow rate of the mixed gas is 200 ml / min.

6. The heat treatment process of bamboo material according to claim 1, It is characterized in that The heating rate of the low-temperature pyrolysis in step (4) is 10°C / min.

7. The heat treatment process of bamboo material according to claim 1, It is characterized in that The high temperature pyrolysis in step (5) is carried out in a pyrolysis apparatus.

8. Application of bamboo-derived bio-oil, It is characterized in that The bamboo-derived bio-oil obtained by the heat treatment process of bamboo as described in any one of claims 1 to 7 can be used for the preparation of biofuel.