Preparation method and application of nano-copper particle surface modifier
The surface modifier is prepared by mixing nano-copper particles with PAO oil and performing ultrasonic treatment. After treating the friction interface, it fills the wear marks and forms a friction film, which solves the problem of high friction coefficient under high load and achieves a significant reduction in friction coefficient. and improved lubrication effect.
Patent Information
- Application Number
- CN202410885854.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-10-29
AI Technical Summary
When the existing technology simply uses poly-alpha olefin oil (PAO oil) under high load, the friction coefficient is still high, and the wear of the friction pair is large and the wear spot size of the small ball is also relatively large, making it difficult to effectively reduce the friction coefficient of the friction interface. .
By mixing nano-copper particles with pure PAO oil and performing ultrasonic treatment, a nano-copper particle surface modifier is prepared and used to treat the friction interface, fill the wear marks and gullies, form a friction film, and reduce the friction coefficient.
It significantly reduces the friction coefficient and friction pair wear, improves the lubrication effect, and reduces energy consumption and equipment losses.
Smart Images

Figure CN118853258A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of running-in lubrication, and specifically relates to a preparation method and application of a nano copper particle surface modifier.
[0002] Friction is the main cause of energy loss associated with human activities. Reducing friction will help achieve carbon neutrality in global energy audits. Friction converts valuable kinetic energy into heat energy, causing wear on moving parts. One-fifth of all energy generated globally is used to overcome friction (about 100 million TJ). Industry (29%) and transportation (27%) are the largest energy users. In global road transportation alone, 200 billion liters of gasoline are consumed each year to overcome friction. Reasonable lubrication optimization schemes can effectively reduce friction and wear. The current mainstream friction reduction and anti-wear methods are mainly divided into two categories. One is the common use of lubricating media, such as lubricating oil, between two friction surfaces to reduce friction and wear, and the other is surface modification of the friction interface. Adding lubricating oil to the friction interface is the most common method, which can play an excellent role in friction performance during the friction process, such as polyalphaolefin oil (PAO oil). However, under high loads, the friction coefficient of PAO oil alone is still high, and the wear of the friction pair is also large and the wear spot size of the ball is also relatively large. Therefore, a method for effectively reducing the friction coefficient of the friction interface is still in urgent need in this field. Summary of the invention
[0003] Based on the above purpose, the purpose of the present application is to provide a preparation method and application of a nano copper particle surface modifier, so that the friction coefficient of the friction interface treated with the surface modifier can be effectively and stably reduced, thereby reducing energy consumption.
[0004] To this end, the first technical solution of the present application provides a method for preparing a nano-copper particle surface modifier, comprising mixing and stirring nano-copper particles with pure PAO and then subjecting the mixture to ultrasonic treatment.
[0005] Furthermore, the mass ratio of the nano copper particles to PAO is 1:(90-99).
[0006] Furthermore, the ultrasonic treatment time is 20 to 30 minutes.
[0007] And, the nano copper particle surface modifier prepared according to the above preparation method.
[0008] The second technical solution of the present application provides the application of the above-mentioned nano-copper particle surface modifier in reducing the friction coefficient of the friction interface, including using the nano-copper particle surface modifier as a surface treatment liquid to first perform surface modification treatment on the friction interface; and then using conventional lubricating oil for running-in treatment.
[0009] In this application, when the nano-copper particle surface modifier is used as a surface treatment liquid to treat the friction interface, the nano-copper particles will fill in the newly generated wear scars and gullies, playing a repairing role. When a large number of nano-copper particles accumulate, they will be squeezed and deformed into a friction film attached to the surface of the friction pair, thereby playing a role in surface modification. Therefore, compared with the substrate without surface treatment, a better lubrication effect can be achieved when conventional lubricants are used for running-in treatment later.
[0010] Preferably, the running-in treatment is performed using a friction running-in testing machine, with a set load of 20 to 35 N, a speed of 10 to 30 mm / s, and a time of 20 to 45 min.
[0011] The beneficial effects of the present application are as follows: the present application obtains a nano-copper particle surface modifier by mixing nano-copper particles with pure PAO and subjecting the mixture to ultrasonic treatment, and the surface modifier has good lubrication and surface modification properties. When the surface modifier is used to treat the friction interface, the nano-copper particles therein will perform a certain extrusion friction movement when contacting the friction interface surface, and the friction surface thus obtained will have a significantly lower friction coefficient than the prior art, and at the same time, the wear spot wear of the friction pair (small ball) is also significantly reduced, thereby reducing the energy consumption of the friction interface and also helping to reduce equipment loss. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Attached Figure 1 This is a graph showing the change of the friction coefficient over time in Example 1;
[0013] Attached Figure 2 This is a graph showing the change of the friction coefficient over time in Example 2;
[0014] Attached Figure 3 This is a graph showing the variation of the friction coefficient over time in Comparative Example 1;
[0015] Attached Figure 4 This is a graph showing the variation of the friction coefficient over time in Comparative Example 2;
[0016] Attached Figure 5 The surface wear spots of the small balls used as friction pairs in Example 1-2 and Comparative Example 1-2 are shown. DETAILED DESCRIPTION
[0017] The present invention is further described in detail below in conjunction with specific examples. This implementation case is implemented based on the technology of the present invention, and a detailed implementation method and specific operation process are now given to illustrate that the present invention is creative, but the protection scope of the present invention is not limited to the following examples.
[0018] The "conventional lubricating oil" mentioned in this application refers to a lubricating oil that is different from the nano-copper particle surface modifier used as the surface treatment liquid in this application, which is commonly known to those skilled in the art and plays a lubricating role at the friction interface, such as pure PAO.
[0019] Example 1 Application of Nano-Copper Particle Surface Modifier
[0020] 1. Weigh 0.05g of nano copper particles and 0.45g of PAO oil (PAO+1wt% Cu) in a container, mix them, stir for 5min, and then put them into an ultrasonic cleaner for ultrasonic treatment for 20min to obtain a nano copper particle surface modifier.
[0021] 2. The surface modifier is used to treat the friction interface. Specifically, a ball-to-disk reciprocating friction test is performed using a UMT-2 friction and wear tester. After the device is built, a load of 35 N, a speed of 20 mm / s, and a time of 25 min are set. The configured nano-copper particle surface modifier is dripped onto the substrate surface. The ball is used as a friction pair to ensure that the area that rubs against the ball is completely covered. A friction test is performed to obtain a graph showing the change in friction coefficient over time (e.g. Figure 1 .PAO+1wt%Cu friction stage): After a period of running-in, the friction coefficient decreases and remains stable (the friction coefficient decreases to about 0.114 after running-in); and a treated friction interface is obtained.
[0022] 3. Continue the experiment on the friction interface treated in step 2, keep the equipment unchanged, replace a new ball (friction pair) in place, and remove the PAO + 1wt% Cu remaining on the substrate surface, then set the load and speed again, add PAO oil to the substrate surface to ensure that the area rubbed by the ball is completely covered, and conduct the friction experiment; set the load to 30N, the speed to 20mm / s, and the time to 10min, and finally obtain the change of friction coefficient over time (as shown in Figure 1 .PAO stage): At the friction interface after being treated with a surface modifier containing nano-copper particles, the friction coefficient in subsequent work remained at around 0.114.
[0023] Example 2 Application of Nano-Copper Particle Surface Modifier
[0024] 1. Weigh 0.05g of nano copper particles and 0.45g of PAO oil (PAO+1wt% Cu) in a container, mix them, stir for 5min, and then put them into an ultrasonic cleaner for ultrasonic treatment for 20min to obtain a nano copper particle surface modifier.
[0025] 2. The surface modifier is used to treat the friction interface. Specifically, a ball-to-disk reciprocating friction test is performed using a UMT-2 friction and wear tester. After the device is built, a load of 30 N, a speed of 20 mm / s, and a time of 25 min are set. The configured nano-copper particle surface modifier is dripped onto the substrate surface. The ball is used as a friction pair to ensure that the area that rubs against the ball is completely covered. A friction test is performed to obtain a graph showing the change in friction coefficient over time (e.g. Figure 2 .PAO+1wt%Cu friction stage): After a period of running-in, the friction coefficient decreases and remains stable (the friction coefficient decreases to about 0.117 after running-in); and the treated friction interface is obtained
[0026] 3. Continue the experiment on the friction interface treated in step 2, keep the equipment unchanged, replace a new ball (friction pair) in place, and remove the PAO + 1wt% Cu remaining on the substrate surface, then set the load and speed again, add PAO oil to the substrate surface to ensure that the area rubbed by the ball is completely covered, and conduct the friction experiment; set the load to 25N, the speed to 20mm / s, and the time to 10min, and finally obtain the change of friction coefficient over time (as shown in Figure 2 .PAO stage): At the friction interface after being treated with a surface modifier containing nano-copper particles, the friction coefficient in subsequent work remained at around 0.115.
[0027] Comparative Example 1
[0028] The experimental method is the same as that of Example 1, except that step 1 is omitted in Comparative Example 1, and PAO 4 oil is used in step 2 instead of the surface modifier of the nano copper particles to obtain a graph showing the change of the friction coefficient over time. Figure 3 As shown: It can be seen that in step 2, there is no running-in, and the friction coefficient is consistently maintained in the range of 0.4-0.45, but it is very unstable. After entering step 3, the friction coefficient is still very high, rising from 0.35 to 0.38, and the friction coefficient is not stable.
[0029] Comparative Example 2
[0030] The experimental method is the same as that of Example 2, except that step 1 is omitted in Comparative Example 1, and PAO oil is used in step 2 instead of the surface modifier of the nano copper particles to obtain a graph showing the change of the friction coefficient over time. Figure 4 As shown: It can be seen that in step 2, there is no running-in, and the friction coefficient is consistently maintained in the range of 0.4-0.45, but it is very unstable. After entering step 3, the friction coefficient is still very high, dropping from 0.47 to 0.41, and the friction coefficient is not stable.
[0031] Figure 5The wear spot morphology of the small ball used as the friction pair in step 2 of Examples 1 and 2 and Comparative Examples 1 and 2 after the reciprocating friction test. It can be clearly seen that the wear degree of the wear spot of the small ball in Examples 1 and 2 is less than that in Comparative Examples 1 and 2.
[0032] Finally, it should be noted that the above implementation cases are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred implementation cases, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a surface modifier for nano copper particles, characterized in that: The method comprises mixing and stirring nano copper particles and PAO and then performing ultrasonic treatment to obtain the nano copper particles.
2. The preparation method according to claim 1, characterized in that: The mass ratio of the nano copper particles to PAO is 1: (90-99)。 3. The preparation method according to claim 1, characterized in that: The ultrasonic treatment time is 20 to 30 minutes.
4. A surface modifier for nano copper particles prepared according to any one of the preparation methods of claims 1-3.
5. A use of the nano copper particle surface modifier as claimed in claim 4 in reducing the friction coefficient of a friction interface, characterized in that: Using the nano copper particle surface modifier as a surface treatment liquid, firstly performing surface modification treatment on the friction interface; Then use conventional lubricating oil for running-in.
6. The use according to claim 4, characterized in that: The running-in treatment is carried out using a friction running-in testing machine, with a set load of 20 to 35 N, a speed of 10 to 30 mm / s, and a time of 20 to 45 min.