High-strength aluminum alloy rivet and preparation method thereof

By using alloys of magnesium, zinc, copper and rare earth elements in rivets and a multi-stage cold heading forming process, combined with rapid solution treatment and surface treatment, the problem of insufficient performance of traditional rivets under high loads and harsh environments has been solved and achieved High strength, corrosion resistance and efficient production.

CN118854130AInactive Publication Date: 2024-10-29WUXI ANSHIDA HARDWARE
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410853455.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional aluminum alloy rivets are difficult to meet the requirements of high-performance fields such as aerospace and aerospace under high loads and harsh environments. They suffer from insufficient mechanical properties, inconsistent processing accuracy, low heat treatment efficiency and poor surface treatment.

Method used

An alloy of specific proportions of magnesium, zinc, copper and rare earth elements is used to optimize the mechanical properties and surface quality of the rivets through multi-stage cold heading forming and rapid solid solution treatment, combined with processes such as age hardening and mechanical polishing.

Benefits of technology

Significantly improves the strength, toughness, corrosion resistance and production efficiency of rivets, ensuring product consistency and high-performance applications, suitable for high loads and complex environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854130A_ABST
    Figure CN118854130A_ABST
Patent Text Reader

Abstract

The invention relates to the field of rivet production and processing, and discloses a high-strength aluminum alloy rivet which comprises the following alloys in percentage by weight: 1.0%-2.0% of magnesium, 2.0%-3.0% of zinc, 1.5%-2.5% of copper, 0.1%-0.5% of rare earth elements and the balance of aluminum and inevitable impurities. By mixing aluminum, magnesium, zinc, copper and rare earth elements in a specific proportion, the mechanical property of the rivet is improved, and the technical purpose of being suitable for a high-load environment is achieved. The alloy configuration enables the rivet to have higher strength and toughness, the rivet is suitable for being used in the industrial fields with strict requirements such as aerospace, by introducing the multi-stage cold heading forming process, accurate control over the shape and size of the rivet is achieved, and the technical purposes of improving product consistency and reducing manufacturing defects are achieved. The multi-stage cold heading not only optimizes the microstructure of the rivet, but also improves the production efficiency, and ensures that each rivet reaches a strict industrial standard.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rivet production and processing, and in particular to a high-strength aluminum alloy rivet and a preparation method thereof. Background Art

[0002] In high-performance industrial fields, especially the aerospace industry, the performance requirements for structural connectors such as rivets are extremely stringent. As a key structural connection element, rivets not only need to meet basic mechanical load requirements, but also need to withstand complex environmental factors such as extreme temperature changes, high-intensity vibrations and corrosive environments. Although traditional aluminum alloy rivets are widely used due to their light weight and easy processing characteristics, their performance in strength, corrosion resistance and fatigue life often cannot meet the demanding requirements of modern high-tech fields such as aerospace. Under high loads and harsh working conditions, conventional aluminum alloy rivets may not guarantee long-term reliability and safety.

[0003] Deficiencies of existing technology:

[0004] Mechanical performance limitations: Traditional aluminum alloy rivets are limited by their alloy composition and are prone to deformation or breakage under high load conditions. Especially when subjected to extreme temperature fluctuations or continuous high vibration environments, their structural stability and fatigue resistance often fail to meet the standards required for high-performance applications.

[0005] Processing accuracy issues: In the production process of rivets, especially in the critical cold heading stage, existing technologies often make it difficult to ensure the precise consistency of size and shape of each rivet. This inconsistency in accuracy will lead to fluctuations in product quality, thus affecting the assembly quality and reliability of the entire structure.

[0006] Low heat treatment efficiency: Traditional heat treatment processes, such as solution treatment and age hardening, can be complex and time-consuming to operate, especially when large quantities of high-quality rivets need to be produced quickly. The existing batch processing methods are usually not efficient, becoming a bottleneck in the production process.

[0007] Insufficient surface treatment: In terms of surface treatment of rivets, traditional technology often ignores the importance of optimizing the surface quality of rivets and improving their corrosion resistance. This neglect may cause rivets to be easily corroded by environmental factors during use, affecting their performance and life.

[0008] Therefore, the present invention provides a high-strength aluminum alloy rivet and a preparation method thereof to solve the deficiencies of the prior art. Summary of the invention

[0009] In view of the deficiencies in the prior art, the present invention provides a high-strength aluminum alloy rivet and a preparation method thereof, which not only optimizes the mechanical properties and corrosion resistance of the rivet, but also significantly improves the production efficiency and consistency of the rivet.

[0010] To achieve the above objectives, the present invention is implemented through the following technical solutions: a high-strength aluminum alloy rivet, the rivet is composed of the following alloys in weight percentage: 1.0%-2.0% magnesium, 2.0%-3.0% zinc, 1.5%-2.5% copper, 0.1%-0.5% rare earth elements, and the balance is aluminum and inevitable impurities.

[0011] Preferably, the rare earth element is selected from cerium, lanthanum or a combination thereof.

[0012] Preferably, the diameter of the rivet ranges from 3 mm to 10 mm, and the length ranges from 5 mm to 50 mm.

[0013] Preferably, a method for preparing a high-strength aluminum alloy rivet comprises the following steps:

[0014] a) Alloy smelting: magnesium, zinc, copper and rare earth elements are mixed and melted with aluminum in a furnace, and the smelting temperature is controlled at 750°C to 850°C;

[0015] b) Casting: The molten alloy is cast into a billet in a mold preheated to 250°C;

[0016] c) Cold heading: The blank is formed into a rivet through a multi-pass cold heading process at room temperature;

[0017] d) Heat treatment: including rapid solution treatment and aging hardening, wherein the rapid solution treatment is carried out at 560°C for no more than 30 seconds, followed by rapid cooling; and the aging hardening is carried out at 200°C for 4 hours.

[0018] Preferably, the cold heading forming process includes at least three cold heading stages, specifically including:

[0019] The first stage: preforming, the cast blank is initially pressed into a predetermined rough shape. This stage mainly eliminates burrs and irregular surfaces of the casting and prepares the blank for precision cold heading;

[0020] The second stage: precision forming, using precisely designed dies to further shape the detailed features of the rivet, including the head and tail;

[0021] The third stage: refinement and finishing, fine-tuning and smoothing the final shape of the rivet, including removing any minor imperfections.

[0022] Preferably, the rapid solution treatment adopts a continuous furnace line, specifically comprising:

[0023] The rivets are evenly arranged on a conveyor belt, which slowly passes through the furnace to ensure that each rivet is evenly heated to 560°C.

[0024] The heating time is controlled within 30 seconds to avoid excessive oxidation of the alloy components or grain coarsening.

[0025] Preferably, the quenching medium is selected to be water or a polymer mixed solution, wherein the polymer mixed solution includes polyvinyl alcohol and polyvinyl pyrrolidone in a ratio of 1:1, and is mixed with deionized water at a ratio of 5% to 10% of the total volume.

[0026] Preferably, the aging hardening further includes the steps of mechanically polishing and cleaning the rivet surface, specifically including:

[0027] Mechanical polishing: Use fine sandpaper and polishing paste to polish the rivet surface to eliminate tiny scratches and unevenness on the surface;

[0028] Cleaning steps: Use an ultrasonic cleaner and appropriate deionized water to thoroughly clean the rivets to remove impurities and residues generated during the polishing process to ensure that the rivet surface is clean and free of contamination.

[0029] The present invention provides a high-strength aluminum alloy rivet and a preparation method thereof, which has the following beneficial effects:

[0030] 1. The present invention improves the mechanical properties of rivets by using a mixture of aluminum, magnesium, zinc, copper and rare earth elements in a specific ratio, achieving the technical purpose of being suitable for high-load environments. This alloy configuration makes the rivets have higher strength and toughness, and is suitable for use in demanding industrial fields such as aerospace.

[0031] 2. The present invention achieves precise control of the shape and size of the rivets by introducing a multi-stage cold heading process, achieving the technical purpose of improving product consistency and reducing manufacturing defects. Multi-stage cold heading not only optimizes the microstructure of the rivets, but also improves production efficiency, ensuring that each rivet meets strict industrial standards.

[0032] 3. The present invention uses a continuous furnace line for rapid solution treatment to achieve uniform heating and rapid cooling of rivets, thereby achieving the technical purpose of enhancing material properties and reducing production time. This treatment method effectively avoids excessive oxidation of alloy elements and grain coarsening, and maintains the optimal performance of the alloy.

[0033] 4. The present invention uses a polymer mixed solution of polyvinyl alcohol and polyvinyl pyrrolidone in a specific ratio as a quenching medium to achieve precise control of the cooling rate of the rivet and achieve the technical purpose of optimizing the microstructure and mechanical properties of the rivet. The application of this quenching medium reduces the stress concentration and microcracks that may be generated in the material during the cooling process, thereby extending the service life of the product.

[0034] 5. The present invention improves the surface finish and cleanliness of the rivet by mechanically polishing and ultrasonic cleaning the rivet after aging hardening, thereby achieving the technical purpose of improving the surface quality of the rivet. This surface treatment not only improves the appearance quality of the rivet, but also reduces the friction coefficient of the rivet in practical applications and enhances its corrosion resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The present invention is a flow chart of the preparation method of high-strength aluminum alloy rivets. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the specification of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Please see attached Figure 1 :

[0038] Example:

[0039] Example 1: High-strength aluminum alloy rivets for the aerospace industry

[0040] Specific steps:

[0041] Alloy melting:

[0042] Ingredients: Accurately weigh 1.5% magnesium, 2.5% zinc, 2.0% copper, 0.3% cerium and the remainder aluminum.

[0043] Melting: Heating to 800℃ in a medium frequency induction furnace to ensure that the alloy components are completely melted and evenly mixed. Stirring is performed during the process to prevent stratification.

[0044] Degassing and slag removal: Nitrogen is used for degassing during the smelting process to reduce porosity defects, and refining agents are used to remove inclusions in the melt.

[0045] Casting:

[0046] Mold preheating: Preheat the mold in an oven at 250°C for 1 hour to ensure uniform cooling of the casting and reduce stress.

[0047] Casting: Pour the molten alloy into a mold preheated to 250°C and cast slowly to avoid inclusions and bubble formation.

[0048] Cooling and demoulding: After naturally cooling to room temperature, demoulding is performed to obtain a blank with a diameter of 5 mm and a length of 20 mm.

[0049] Cold heading:

[0050] The first stage is pre-forming: the blank is pre-pressed on a 200-ton cold heading machine to perform preliminary forming to eliminate burrs and irregular surfaces.

[0051] Second stage precision forming: further shaping using precision dies to form the detailed features of the rivet, including the head and tail, to ensure accurate dimensions.

[0052] The third stage is refinement and finishing: high-precision tools are used for final refinement and finishing to ensure that the rivet shape and size are exactly as designed.

[0053] Heat Treatment:

[0054] Rapid solution treatment: The rivets are placed in a continuous furnace line at 560°C, uniformly heated for 20 seconds, then rapidly cooled to room temperature and quenched using water or a polymer mixed solution.

[0055] Age hardening: 4 hours of age hardening in a heat treatment furnace at 200°C ensures that the mechanical properties of the rivets reach the best state.

[0056] Surface treatment:

[0057] Mechanical polishing: Use 400 to 1200 grit sandpaper to polish gradually, and use polishing paste for final treatment to make the surface finish reach mirror effect.

[0058] Ultrasonic cleaning: In an ultrasonic cleaner, use deionized water to thoroughly clean the surface of the rivet to remove residual impurities and polishing paste.

[0059] Summary: The rivets produced in this embodiment have excellent strength and toughness, are suitable for use in high-load and high-temperature environments, and meet the stringent requirements of the aerospace industry. Through fine cold heading and strict heat treatment processes, the performance of the rivets is greatly improved.

[0060] Example 2: High-strength aluminum alloy rivets for the automotive industry

[0061] Specific steps:

[0062] Alloy melting:

[0063] Ingredients: Accurately weigh 1.0% magnesium, 2.0% zinc, 1.5% copper, 0.2% lanthanum and the remainder aluminum.

[0064] Melting: Heating to 750℃ in a medium frequency induction furnace to ensure uniform melting of the alloy. Refining agents are added during the process to remove impurities.

[0065] Degassing: Use nitrogen for degassing to reduce porosity defects and ensure the purity of the alloy.

[0066] Casting:

[0067] Mold preheating: Preheat the mold in an oven at 250°C for 1 hour.

[0068] Casting: Slowly pour the molten alloy into a mold preheated to 250°C, ensuring there are no inclusions and bubbles.

[0069] Cooling: After cooling naturally to room temperature, demoulding is performed to obtain a blank with a diameter of 8 mm and a length of 30 mm.

[0070] Cold heading:

[0071] The first stage is pre-forming: using a 200-ton cold heading machine to initially shape the blank.

[0072] The second stage of precision forming: the head and tail of the rivet are further formed through precision molds.

[0073] Stage 3 Refinement and finishing: Final refinement is performed using high-precision tools to ensure that the shape and size of the rivet meet the design requirements.

[0074] Heat Treatment:

[0075] Rapid solution treatment: The rivets are heated in a continuous furnace at 560°C for 25 seconds and then rapidly cooled to room temperature.

[0076] Age Hardening: Age hardening was carried out in a furnace at 200°C for 4 hours.

[0077] Surface treatment:

[0078] Mechanical polishing: Polish the rivets gradually using 400 to 1200 grit sandpaper and use polishing paste for a final finish.

[0079] Ultrasonic cleaning: Clean the rivets in an ultrasonic cleaner using deionized water to remove any residue.

[0080] Summary: The rivets produced in this embodiment have excellent corrosion resistance and durability, and are suitable for use in high-stress connection parts in the automotive industry. Through the optimized cold heading and heat treatment processes, the mechanical properties of the rivets are significantly improved.

[0081] Example 3: High-strength aluminum alloy rivets for construction engineering

[0082] Specific steps:

[0083] Alloy melting:

[0084] Ingredients: Weigh 1.2% magnesium, 2.8% zinc, 2.3% copper, 0.4% cerium and the remainder aluminum.

[0085] Melting: Heating to 850°C in a medium frequency induction furnace to ensure uniform melting of the components, stirring and refining during the process.

[0086] Degassing and deslagging: Nitrogen is used for degassing, and refining agents are added to remove impurities in the melt.

[0087] Casting:

[0088] Mold preheating: Preheat the mold in an oven at 250°C.

[0089] Casting: Pour the molten alloy into a mold preheated to 250°C and cast slowly to avoid inclusions and bubbles.

[0090] Cooling and demoulding: After naturally cooling to room temperature, demoulding is performed to obtain a blank with a diameter of 10 mm and a length of 50 mm.

[0091] Cold heading:

[0092] The first stage is preforming: the blank is initially formed on a 300-ton cold heading machine.

[0093] Second stage precision forming: Use precision dies to further form the detailed features of the rivet.

[0094] Stage 3 Refinement and finishing: Final refinement and finishing using high-precision tools.

[0095] Heat Treatment:

[0096] Rapid solution treatment: The rivets are heated on a continuous furnace line at 560°C for 30 seconds and then rapidly cooled.

[0097] Age hardening: Age hardening is carried out in a heat treatment furnace at 200°C for 4 hours.

[0098] Surface treatment:

[0099] Mechanical polishing: Polishing step by step using sandpaper and polishing paste.

[0100] Ultrasonic Cleaning: Clean the rivets using deionized water in an ultrasonic cleaner.

[0101] Summary: The rivets produced in this embodiment have high strength and durability and are suitable for use in high-load bearing structures in construction projects. The performance of the rivets is significantly improved through multi-stage cold heading and strict heat treatment processes.

[0102] Example 4: High-strength aluminum alloy rivets for shipbuilding industry

[0103] Specific steps:

[0104] Alloy melting:

[0105] Ingredients: Weigh 2.0% magnesium, 3.0% zinc, 2.5% copper, 0.5% lanthanum and the remainder aluminum.

[0106] Melting: Heat to 850℃ in a medium frequency induction furnace to ensure that the alloy components are evenly melted and stirred.

[0107] Degassing and deslagging: Nitrogen is used for degassing and refining agents are added to remove impurities.

[0108] Casting:

[0109] Mold preheating: Preheat the mold in an oven at 250°C.

[0110] Casting: Slowly pour the molten alloy into a mold preheated to 250°C, ensuring there are no inclusions and bubbles.

[0111] Cooling and demoulding: After naturally cooling to room temperature, demoulding is performed to obtain a blank with a diameter of 6 mm and a length of 25 mm.

[0112] Cold heading:

[0113] The first stage is pre-forming: using a 200-ton cold heading machine to initially shape the blank.

[0114] The second stage of precision forming: the detailed features of the rivet are further formed through precision molds.

[0115] Stage 3 Refinement and finishing: Final refinement and finishing using high-precision tools.

[0116] Heat Treatment:

[0117] Rapid solution treatment: The rivets are heated in a continuous furnace at 560°C for 28 seconds and then rapidly cooled.

[0118] Age hardening: Age hardening is carried out in a heat treatment furnace at 200°C for 4 hours.

[0119] Surface treatment:

[0120] Mechanical polishing: Polishing is done step by step using sandpaper and polishing paste.

[0121] Ultrasonic Cleaning: Clean the rivets in an ultrasonic cleaner using deionized water.

[0122] Summary: The rivets produced in this embodiment have excellent corrosion resistance and are suitable for use in the marine environment of the shipbuilding industry. The durability and strength of the rivets are improved through optimized alloy composition and strict heat treatment process.

[0123] Example 5: High-strength aluminum alloy rivets for electronic equipment

[0124] Specific steps:

[0125] Alloy melting:

[0126] Ingredients: Weigh 1.8% magnesium, 2.7% zinc, 2.0% copper, 0.2% cerium and the remainder aluminum.

[0127] Melting: Heating to 800°C in a medium frequency induction furnace to ensure uniform melting of the components and stirring.

[0128] Degassing and deslagging: Nitrogen is used for degassing and refining agents are added to remove impurities.

[0129] Casting:

[0130] Mold preheating: Preheat the mold in an oven at 250°C.

[0131] Casting: Slowly pour the molten alloy into a mold preheated to 250°C, ensuring there are no inclusions and bubbles.

[0132] Cooling and demoulding: After naturally cooling to room temperature, demoulding is performed to obtain a blank with a diameter of 3 mm and a length of 10 mm.

[0133] Cold heading:

[0134] The first stage is pre-forming: using a 200-ton cold heading machine to initially shape the blank.

[0135] The second stage of precision forming: the detailed features of the rivet are further formed through precision molds.

[0136] Stage 3 Refinement and finishing: Final refinement and finishing using high-precision tools.

[0137] Heat Treatment:

[0138] Rapid solution treatment: The rivets are heated on a continuous furnace line at 560°C for 15 seconds and then rapidly cooled.

[0139] Age hardening: Age hardening is carried out in a heat treatment furnace at 200°C for 4 hours.

[0140] Surface treatment:

[0141] Mechanical polishing: Polishing is done step by step using sandpaper and polishing paste.

[0142] Ultrasonic Cleaning: Clean the rivets in an ultrasonic cleaner using deionized water.

[0143] Summary: The rivet produced in this embodiment has good electrical conductivity and thermal stability, and is suitable for internal structural connection of electronic equipment. The performance of the rivet is significantly improved through optimized cold heading and heat treatment processes.

[0144] Summary:

[0145] Through the above five different embodiments, high-strength aluminum alloy rivets have demonstrated their potential for application in multiple industrial fields. Each embodiment has detailed process design and processing steps according to specific usage scenarios and requirements to ensure that the rivets achieve optimal performance in terms of strength, corrosion resistance, conductivity, etc. These embodiments not only demonstrate the superior performance of rivets in high-load, high-temperature, and highly corrosive environments, but also demonstrate their wide applicability under precision manufacturing and high-performance requirements. Each embodiment ensures the reliability and performance of rivets in different applications through detailed alloy smelting, cold heading, heat treatment, and surface treatment processes.

[0146] Comparative experiment 1: Mechanical properties comparison experiment

[0147] Experimental purpose: To compare the differences between conventional aluminum alloy rivets and the rivets of the present invention in terms of tensile strength, yield strength and elongation.

[0148] Experimental Materials:

[0149] Conventional aluminum alloy rivets (control group): made of aluminum alloy 6061-T6, which contains magnesium (0.8%-1.2%), silicon (0.4%-0.8%), copper (0.15%-0.4%), chromium (0.04%-0.35%), and the remainder is aluminum and unavoidable impurities.

[0150] The rivet of the present invention (experimental group) is made of a high-strength aluminum alloy containing 1.5% magnesium, 2.5% zinc, 2.0% copper, rare earth elements (0.2% cerium, 0.1% lanthanum) and the remainder aluminum.

[0151] Experimental methods:

[0152] Sample preparation: 50 rivet samples with a diameter of 5 mm and a length of 20 mm were prepared.

[0153] Tensile Test: Tensile tests are performed on a universal materials testing machine to measure tensile strength, yield strength and elongation.

[0154] Experimental parameters:

[0155] Stretching rate: 2mm / min

[0156] Ambient temperature: room temperature (25°C)

[0157] Testing equipment: Instron 5967 universal material testing machine

[0158] Experimental data:

[0159] Sample type Tensile strength(MPa) Yield strength (MPa) Elongation(%) Traditional aluminum alloy rivets 310 270 12 Rivet of the present invention 370 330 15

[0160] Experimental results: The rivets of the present invention are significantly superior to traditional aluminum alloy rivets in terms of tensile strength, yield strength and elongation, which reflects the mechanical performance advantages of the rivets of the present invention.

[0161] Comparative experiment 2: Corrosion resistance comparison experiment

[0162] Experimental purpose: To compare the corrosion resistance of traditional aluminum alloy rivets and the rivets of the present invention in salt spray tests.

[0163] Experimental Materials:

[0164] Traditional aluminum alloy rivets (control group): made of aluminum alloy 6061-T6.

[0165] The rivet of the present invention (experimental group) is made of a high-strength aluminum alloy containing 1.5% magnesium, 2.5% zinc, 2.0% copper, rare earth elements (0.2% cerium, 0.1% lanthanum) and the remainder aluminum.

[0166] Experimental methods:

[0167] Sample preparation: 50 rivet samples with a diameter of 5 mm and a length of 20 mm were prepared.

[0168] Salt spray test: Carry out a 72-hour salt spray test in a salt spray test chamber to observe the surface corrosion of the sample and measure the corrosion rate.

[0169] Experimental parameters:

[0170] Salt spray solution: 5% NaCl solution

[0171] Temperature: 35℃

[0172] Humidity: 95%

[0173] Experimental data:

[0174] Sample type <![CDATA[Corrosion rate (mg / cm 2 / day)]]> Traditional aluminum alloy rivets 0.25 Rivet of the present invention 0.1

[0175] Experimental results: The corrosion resistance of the rivet of the present invention in the salt spray test is significantly better than that of the traditional aluminum alloy rivet, showing better corrosion resistance.

[0176] Comparative experiment 3: Fatigue life comparison experiment

[0177] Experimental purpose: To compare the difference in fatigue life between traditional aluminum alloy rivets and the rivets of the present invention.

[0178] Experimental Materials:

[0179] Traditional aluminum alloy rivets (control group): made of aluminum alloy 6061-T6.

[0180] The rivet of the present invention (experimental group) is made of a high-strength aluminum alloy containing 1.5% magnesium, 2.5% zinc, 2.0% copper, rare earth elements (0.2% cerium, 0.1% lanthanum) and the remainder aluminum.

[0181] Experimental methods:

[0182] Sample preparation: 50 rivet samples with a diameter of 5 mm and a length of 20 mm were prepared.

[0183] Rotating bending fatigue test: measures the fatigue life of samples at different stress levels.

[0184] Experimental parameters:

[0185] Frequency: 10Hz

[0186] Stress ratio: 0.1

[0187] Ambient temperature: room temperature (25°C)

[0188] Experimental data:

[0189]

[0190]

[0191] Experimental results: The rivets of the present invention are significantly superior to traditional aluminum alloy rivets in terms of fatigue life, indicating that they have higher reliability and durability in high stress and high vibration environments.

[0192] Comparative experiment 4: Heat treatment efficiency comparison experiment

[0193] Experimental purpose: To compare the efficiency and performance of the heat treatment process between the conventional aluminum alloy rivets and the rivets of the present invention.

[0194] Experimental Materials:

[0195] Conventional aluminum alloy rivets (control group): made of aluminum alloy 6061-T6, using conventional batch heat treatment process.

[0196] The rivet of the present invention (experimental group) is made of a high-strength aluminum alloy containing 1.5% magnesium, 2.5% zinc, 2.0% copper, rare earth elements (0.2% cerium, 0.1% lanthanum) and the remainder of aluminum, and is rapidly solution treated by a continuous furnace line.

[0197] Experimental methods:

[0198] Sample preparation: 50 rivet samples with a diameter of 5 mm and a length of 20 mm were prepared.

[0199] Heat treatment: Rapid solution treatment (30 seconds) and aging hardening (4 hours) were performed, and the hardness after treatment and the treatment time were measured.

[0200] Experimental parameters:

[0201] Solution treatment temperature: 560℃

[0202] Solution treatment time: 30 seconds (invention), 2 hours (conventional process)

[0203] Aging hardening temperature: 200℃

[0204] Aging time: 4 hours

[0205] Experimental data:

[0206]

[0207]

[0208] Experimental results: The hardness of the rivet of the present invention after heat treatment is significantly higher than that of the traditional aluminum alloy rivet, and the heat treatment time is reduced by half, showing higher production efficiency and performance improvement.

[0209] Summary:

[0210] Through four comparative experiments, the significant advantages of the high-strength aluminum alloy rivet of the present invention in mechanical properties, corrosion resistance, fatigue life and heat treatment efficiency are fully demonstrated. These experimental data not only verify the superiority of the rivet of the present invention in multiple key performance indicators, but also further prove its application potential in harsh environments such as high load, high corrosion and high vibration. The present invention successfully solves the shortcomings of the existing technology in rivet performance and production efficiency by optimizing alloy composition, fine cold heading forming and efficient heat treatment process, and has broad industrial application prospects.

[0211] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high-strength aluminum alloy rivet, It is characterized in that The rivet is composed of the following alloys in weight percentage: 1.0%-2.0% magnesium, 2.0%-3.0% zinc, 1.5%-2.5% copper, 0.1%-0.5% rare earth elements, and the balance being aluminum and inevitable impurities.

2. A high-strength aluminum alloy rivet according to claim 1, It is characterized in that The rare earth element is selected from cerium, lanthanum or a combination thereof.

3. A high-strength aluminum alloy rivet according to claim 1, It is characterized in that The diameter of the rivet ranges from 3 mm to 10 mm, and the length ranges from 5 mm to 50 mm.

4. A method for preparing a high-strength aluminum alloy rivet according to any one of claims 1 to 3, It is characterized in that The following steps are involved: a) Alloy smelting: magnesium, zinc, copper and rare earth elements are mixed and melted with aluminum in a furnace, and the smelting temperature is controlled at 750°C to 850°C; b) Casting: The molten alloy is cast into a billet in a mold preheated to 250°C; c) Cold heading: The blank is formed into a rivet through a multi-pass cold heading process at room temperature; d) Heat treatment: including rapid solution treatment and aging hardening, wherein the rapid solution treatment is carried out at 560°C for no more than 30 seconds, followed by rapid cooling; and the aging hardening is carried out at 200°C for 4 hours.

5. A method for preparing a high-strength aluminum alloy rivet according to claim 4, It is characterized in that The cold heading forming process includes at least three cold heading stages, specifically including: The first stage: preforming, the cast blank is initially pressed into a predetermined rough shape. This stage mainly eliminates burrs and irregular surfaces of the casting and prepares the blank for precision cold heading; The second stage: precision forming, using precisely designed dies to further shape the detailed features of the rivet, including the head and tail; The third stage: refinement and finishing, fine-tuning and smoothing the final shape of the rivet, including removing any minor imperfections.

6. A method for preparing a high-strength aluminum alloy rivet according to claim 4, It is characterized in that The rapid solution treatment adopts a continuous furnace line, which specifically includes: The rivets are evenly arranged on a conveyor belt, which slowly passes through the furnace to ensure that each rivet is evenly heated to 560°C. The heating time is controlled within 30 seconds to avoid excessive oxidation of the alloy components or grain coarsening.

7. A method for preparing a high-strength aluminum alloy rivet according to claim 4, It is characterized in that The quenching medium is selected to be water or a polymer mixed solution, wherein the polymer mixed solution includes polyvinyl alcohol and polyvinyl pyrrolidone in a ratio of 1:1, and is mixed with deionized water in a ratio of 5% to 10% of the total volume.

8. A method for preparing a high-strength aluminum alloy rivet according to claim 4, It is characterized in that The aging hardening further includes the steps of mechanically polishing and cleaning the rivet surface, specifically including: Mechanical polishing: Use fine sandpaper and polishing paste to polish the rivet surface to eliminate tiny scratches and unevenness on the surface; Cleaning steps: Use an ultrasonic cleaner and appropriate deionized water to thoroughly clean the rivets to remove impurities and residues generated during the polishing process to ensure that the rivet surface is clean and free of contamination.

Citation Information

Patent Citations

  • Ultra-fast solid solution treatment method for 6-series and 7-series aluminum alloys

    CN107502842A

  • Metal-Me gravity casting aluminum alloy material and preparation method thereof

    CN108467979A

  • Sand mold gravity casting aluminum alloy material and preparation method thereof

    CN108486441A

  • Aluminum-copper-magnesium alloy and processing technology thereof

    CN111286652A