Preparation method and application of transition metal doped nickel-sulfur / phosphorus compound and support composite material catalytic electrode

By preparing a transition metal-doped nickel sulfur/phosphorus compound and a support composite catalytic electrode, the problem of high cost of precious metal catalysts is solved, and low-cost, high catalytic activity electrolysis of water for oxygen and hydrogen production is achieved, which has industrial applications. potential.

CN118854352APending Publication Date: 2024-10-29NINGBO HIDROTEK CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410959186.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The precious metal catalysts used in the current electrolysis of water for hydrogen production and oxygen production are expensive and scarce, which limits the industrial application of water electrolysis for hydrogen production technology.

Method used

A composite catalytic electrode of transition metal-doped nickel sulfur/phosphorus compound and support is used to prepare FeS-Ni3S2 or Fe2P nanoarray catalytic electrode through hydrothermal method and in-situ sulfur/phosphating method, combining one-dimensional and two-dimensional nanometer The morphological structure of the material improves the catalytic activity.

Benefits of technology

A catalytic electrode with low cost, high catalytic activity and long life is realized, which exhibits excellent redox reaction performance, is suitable for electrolyzing water to produce oxygen and hydrogen, and has good industrial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854352A_ABST
    Figure CN118854352A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a transition metal doped nickel sulfur / phosphorus compound and support composite material catalytic electrode. The preparation method is characterized by comprising the following steps: (1) preparing a transition metal doped nickel hydroxide precursor on a flaky support by a hydrothermal method; and (2) the transition metal doped nickel oxide precursor is subjected to in-situ sulfuration / phosphorization, the transition metal doped nickel sulfur / phosphorus compound and support composite material catalytic electrode is obtained, the transition metal doped nickel sulfur / phosphorus compound is a FeS-Ni3S2 catalytic electrode or a Fe2P-Ni2P catalytic electrode, the catalytic electrode can be used for water electrolysis hydrogen / oxygen production, and the transition metal doped nickel sulfur / phosphorus compound and support composite material catalytic electrode can be applied to water electrolysis hydrogen / oxygen production. The catalyst has the advantages of high catalytic activity and long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of water electrolysis catalysts, and specifically relates to a preparation method and application of a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support. Background Art

[0002] Hydrogen energy is considered a key clean energy that can effectively replace fossil fuels. Water electrolysis can produce high-calorie hydrogen without carbon emissions, and can simultaneously store unstable renewable wind energy, solar energy, tidal energy, etc., and is considered one of the most environmentally friendly methods of producing hydrogen.

[0003] Among the existing energy conversion technologies, electrochemical water splitting to produce hydrogen has become the most effective method for producing high-purity hydrogen due to its advantages such as simplicity, economy, high energy conversion efficiency and good environmental compatibility. When electrolyzing water, protons or hydronium ions gain electrons at the cathode, undergo a reduction reaction, and generate hydrogen gas. This process is referred to as the hydrogen reduction reaction (HER). The oxygen evolution reaction (Oxygen Evolution Reaction, OER) refers to the process in which hydroxide ions or water lose electrons and generate oxygen, which occurs at the cathode of the electrolyzer. However, the occurrence of HER and OER requires overcoming a large reaction energy barrier, and the use of catalysts is necessary. The hydrogen evolution reaction currently mainly uses Pt-based precious metal catalysts, while the oxygen evolution reaction mainly uses precious metal oxide catalysts such as IrO2 and RuO2. Precious metals with high catalytic activity are limited by their high prices and scarce reserves, and cannot be used on a large scale in industrial production. Based on this, the development of low-cost non-precious metal catalytic electrodes with excellent catalytic performance is of extremely important practical significance for the development of water electrolysis oxygen evolution technology and its industrial application. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a preparation method and application of a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support body with high catalytic activity and long service life, and the catalytic electrode can be used for electrolyzing water to produce oxygen.

[0005] The technical solution adopted by the present invention to solve the above technical problems is: a method for preparing a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support, comprising the following steps: (1) preparing a transition metal-doped nickel hydroxide precursor on a sheet support by a hydrothermal method; (2) The transition metal-doped nickel hydroxide precursor obtained in step (1) is subjected to in-situ sulfurization / phosphating to obtain a transition metal-doped nickel sulfur / phosphorus compound and a support composite material catalytic electrode, wherein the transition metal-doped nickel sulfur / phosphorus compound is a FeS-Ni3S2 catalytic electrode or a Fe2P-Ni2P catalytic electrode.

[0006] Furthermore, step (1) is specifically as follows: adding the pretreated and dried nickel foam to a mixed solution consisting of a nickel source, an iron source and an ammonium source, and then reacting in a high-pressure reactor at 100-200° C. for 4-24 h, cooling, washing and drying to obtain a nickel foam having a layer of needle-shaped FeNi double transition metal hydroxide precursor loaded on the surface, recorded as FeNi-LDH / NF.

[0007] Further, step (2) is specifically as follows: the nickel foam obtained in step (1) is placed in 20-40 mL of a mixed solution of polysulfide and N,N-dimethylformamide (DMF) in a volume ratio of 1:2, and then reacted in a high-pressure reactor at 100-200° C. for 5-24 h, cooled, washed and dried to obtain a nickel foam catalytic electrode loaded with a rod-shaped hydrotalcite structure FeS-Ni3S2 nanoarray, recorded as a needle-shaped FeS-Ni3S2 / NF catalytic electrode, wherein the polysulfide is polysulfide poly(S-DIB) with 1,3-diisopropenylbenzene as a cross-linking agent; Furthermore, step (2) is specifically as follows: the nickel foam obtained in step (1) is placed in 20 mL of deionized water containing 0.18 mmol trisodium citrate, 0.06 mmol Ni(NO3)2·6H2O and 0.08 mmol K3[Fe(CN)6], reacted in a high pressure reactor at 10-50°C for 10-30 h, washed and dried to obtain a nickel foam loaded with a hydrotalcite structure FeNi-LDH / NF, recorded as FeNi PBAs-FeNi-LDH / NF; the nickel foam FeNi PBAs-FeNi-LDH / NF is mixed with a phosphorus source in a mass ratio of 3:1 and calcined in a tube furnace at a calcination temperature of 300-500°C for 2-4 h, washed and dried after cooling to obtain a nickel foam catalytic electrode loaded with a nanosheet array structure Fe2P-Ni2P, recorded as Fe2P-Ni2P / NF.

[0008] Furthermore, the phosphorus source is selected from red phosphorus or sodium hypophosphite powder.

[0009] Furthermore, the molar ratio of the nickel foam area to the nickel source is (2.7-3.3) cm 2 :1mmol, the concentration of nickel source in the mixed solution is 0.5-2mol / L; the molar ratio of nickel source to iron source is (1-5):1; the molar ratio of ammonium source to nickel source is (1-10):1.

[0010] Furthermore, the nickel source is selected from any one of nickel nitrate, nickel chloride or nickel sulfate; the iron source is one of ferric nitrate, ferrous sulfate or ferric chloride; the ammonium source is selected from any one or any two of urea, ammonium fluoride, ammonium chloride or ammonium nitrate; and the solvent is any one of water, ethanol or methanol.

[0011] The present invention also provides the use of a composite material catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support prepared by the above preparation method in the electrolysis of water to produce oxygen or hydrogen.

[0012] Compared with the prior art, the advantages of the present invention are: 1) A method for preparing a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support and its application, the method has low raw material cost, simple preparation process and low energy consumption in the preparation process; 2) The OER electrocatalytic activity of the present invention is good at both low current density and high current density; 3) The present invention has a unique morphological structure, combining one-dimensional and two-dimensional nanomaterials, and combining two sizes of nanomaterials. These morphological engineerings make the material have a larger catalytic active area and more abundant catalytic active sites; 4) The unique electronic structure and excellent physical properties of the material of the present invention also have good application prospects in energy storage and conversion, sensors and photocatalysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 XRD diffraction spectrum of FeS-Ni3S2 / NF prepared in Example 1; Figure 2 The SEM image of FeS-Ni3S2 / NF prepared in Example 1; Figure 3 LSV curves of FeS-Ni3S2 / NF prepared in Example 1 before and after long-term oxygen evolution test under alkaline conditions; Figure 4 The chronopotentiometry curves of FeS-Ni3S2 / NF prepared in Example 1 before and after a long-term oxygen evolution test under alkaline conditions; Figure 5 The XRD diffraction spectrum of Fe2P-Ni2P / NF prepared in Example 2; Figure 6 This is the SEM image of Fe2P-Ni2P / NF prepared in Example 2; Figure 7 LSV curves of Fe2P-Ni2P / NF prepared in Example 2 before and after long-term oxygen evolution test under alkaline conditions; Figure 8 The chronopotentiometry curves of the Fe2P-Ni2P / NF prepared in Example 2 before and after a long-term oxygen evolution test under alkaline conditions; Fig. 9 LSV performance curves of FeS-Ni3S2 / NF, Ni3S2 / NF, FeS / NF, and RuO2 / NF catalytic electrodes prepared in Example 1; Fig.10 The Tafel curves of FeS-Ni3S2 / NF, Ni3S2 / NF, FeS / NF and RuO2 / NF catalytic electrodes prepared in Example 1; Fig.11 The Energquist diagrams of the FeS-Ni3S2 / NF, Ni3S2 / NF, FeS / NF and RuO2 / NF catalytic electrodes prepared in Example 1; Fig.12 Cdl curves of FeS-Ni3S2 / NF, Ni3S2 / NF, FeS / NF and RuO2 / NF catalytic electrodes prepared in Example 1; Fig.13 LSV performance curves of Fe2P-Ni2P / NF, PBA-FeNi-LDH / NF, FeNi-P / NF, and FeNi-P / NF-p catalytic electrodes prepared in Example 2 of the present invention; Fig.14 The Tafel curves of Fe2P-Ni2P / NF, PBA-FeNi-LDH / NF, FeNi-P / NF, and FeNi-P / NF-p catalytic electrodes prepared in Example 2 of the present invention are shown in FIG. Fig.15 The Nerquist diagrams of the Fe2P-Ni2P / NF, PBA-FeNi-LDH / NF, FeNi-P / NF, and FeNi-P / NF-p catalytic electrodes prepared in Example 2 of the present invention; Fig.16 This is a Cdl curve diagram of the Fe2P-Ni2P / NF, PBA-FeNi-LDH / NF, FeNi-P / NF, and FeNi-P / NF-p catalytic electrodes prepared in Example 2 of the present invention. DETAILED DESCRIPTION

[0014] The present invention is further described in detail below with reference to the accompanying drawings.

[0015] Example 1: A method for preparing a composite catalytic electrode of a transition metal-doped nickel-sulfur compound and a support, comprising the following steps: a. Take nickel foam, cut it into 1cm×3cm, place it in a beaker, add anhydrous ethanol until it is submerged, pour out the anhydrous ethanol after ultrasonication for 15min, add 1 mol / L dilute hydrochloric acid until it is submerged, ultrasonicate for 15min, wash it with water for later use; weigh 1 mmol Ni(NO3)2·6H2O, 1 mmol Fe(NO3)3·9H2O, 8 mmol NH4F and 4 mmol urea and prepare a 40 mL solution, then transfer it to a 50 mL stainless steel autoclave lined with polytetrafluoroethylene, add the treated nickel foam, react at 120℃ for 5h, and freeze-dry for 18h to obtain a nickel foam with a layer of needle-shaped FeNi double transition metal hydroxide precursor on the surface, namely FeNi-LDH / NF, in which the molar ratio of the nickel foam area to the nickel source is 3cm 2 :1mmol.

[0016] b. The FeNi-LDH / NF obtained in step a was placed in a 30 mL mixed solution of polysulfide / DMF (V:V=1:2), and transferred to a 50 mL Teflon autoclave, and reacted at 180 °C in an oven for 10 h. After cooling, it was washed and freeze-dried for 18 h to obtain a foamed nickel catalytic electrode loaded with mixed particles of ferrous sulfide and nickel sulfide, i.e., FeS-Ni3S2 / NF catalyst.

[0017] The XRD diffraction spectrum of the prepared FeS-Ni3S2 / NF is shown in Figure 1 As shown, by observing the XRD pattern of FeS-Ni3S2 / NF, it can be found that the strong diffraction peaks at 21.75°, 31.10°, 37.78°, 44.33°, 49.79° and 55.16° are attributed to the (101), (110), (003), (202), (113) and (300) crystal planes of Ni2S3. In addition, the diffraction peaks at 31.04°, 38.27°, 44.33° and 55.16° are characteristic peaks of FeS. This indicates that after in-situ sulfidation, FeNi-LDH was successfully sulfided to prepare FeS-Ni3S2.

[0018] The scanning electron microscope image of the prepared FeS-Ni3S2 is shown in Figure 2 As shown in the figure, after the sulfurization reaction, the sheet array of FeNi-LDH is reconstructed into FeS-Ni3S2 nanorod array, which is tightly and evenly covered on the surface of nickel foam. There is a tiny nanosheet network structure on the surface of the nanorod. After the two-dimensional nanosheet array is transformed into a three-dimensional porous nanowire structure, more channels are provided for faster material transport, and a larger surface area is exposed as a catalytic reaction site.

[0019] The prepared FeS-Ni3S2 / NF will be cut into a size of 5 mm × 5 mm as a working electrode. All electrochemical tests were performed using a three-electrode system of a CHI760E electrochemical workstation, in which a carbon rod was used as an auxiliary electrode, a FeS-Ni3S2 / NF with a geometric area of ​​5 mm × 5 mm was used as a working electrode, and a Hg / HgO electrode was used as a reference electrode. All electrochemical tests were carried out in a 1M KOH solution, and before the electrochemical test, nitrogen was passed through for 30 min to eliminate oxygen in the KOH solution. The LSV curves of the prepared FeS-Ni3S2 / NF before and after a long-term oxygen evolution test under alkaline conditions are shown in Figure 2. Figure 3 As shown, the scanning rate of the electrochemical cycling stability test CV was 100 mVs -1 The number of cycles was 5000, and the potential range was -0.1 V~0.1 V versus RHE. After 5000 CV cycles, the performance of FeS-Ni3S2 / NF decreased by only 11 mV. Figure 4 As shown in the figure, after 25 h of long-term stability test, the catalytic performance of FeS-Ni3S2 / NF remained almost unchanged compared with the initial performance, indicating that FeS-Ni3S2 / NF has excellent catalytic stability.

[0020] Example 2: A method for preparing a composite catalytic electrode of a transition metal-doped nickel-phosphorus compound and a support, comprising the following steps: a. A 3 cm × 1 cm nickel foam was ultrasonically treated in 3 M HCl solution, anhydrous ethanol and deionized water for 15 min to remove possible oxides on the surface, and then washed with ultrapure water for several times and dried for use. 1 mmol Ni(NO3)2·6H2O, 1 mmol Fe(NO3)3·9H2O, 8 mmol NH4F and 4 mmol urea were weighed and prepared into a 40 mL solution, which was then transferred to a 50 ml stainless steel autoclave lined with polytetrafluoroethylene, and the treated nickel foam was added. The reaction was carried out at 120 ° C for 5 h to obtain a nickel foam with a layer of needle-shaped FeNi double transition metal hydroxide precursor on the surface, namely FeNi-LDH / NF, in which the molar ratio of the nickel foam area to the nickel source was 3 cm 2 :1mmol; b. The FeNi-LDH / NF prepared in step a was placed in 20 mL of deionized water dissolved with 0.18 mmol of trisodium citrate, 0.06 mmol of Ni(NO3)2·6H2O and 1 mmol of K3[Fe(CN)6], and the mixture was reacted at 25°C in a high-pressure reactor for 24 h to obtain a nickel foam loaded with particles of FeNi-LDH anchored with a hydrotalcite structure, namely PBAs-FeNi-LDH / NF; c. After washing and drying the PBAs-FeNi-LDH / NF obtained in step b, annealing and calcining with sodium hypophosphite at 350°C for 2 h in a nitrogen atmosphere to obtain a nickel foam catalytic electrode loaded with hydrotalcite structure Fe2P-Ni2P, namely Fe2P-Ni2P / NF.

[0021] The XRD diffraction spectrum of the prepared Fe2P-Ni2P / NF is shown in Figure 5 As shown, the peaks at 40.79°, 44.59°, 47.31°, 54.23°, 74.67°, 80.92° and 88.89° belong to the (111), (201), (210), (300), (400), (401) and (321) crystal planes of Ni2P (PDF#03-0953), respectively. The diffraction peaks at 40.27°, 44.20°, 47.28° and 54.10° in Fe2P-Ni2P / NF correspond to the (111), (201), (210) and (300) crystal planes of Fe2P (PDF#51-0943), respectively.

[0022] The scanning electron microscope image of the prepared Fe2P-Ni2P / NF is shown in Figure 6 As shown in the figure, after phosphating, Fe2P-Ni2P retains the main structure of the nanosheet array, the surface of Fe2P-Ni2P becomes rough, and the thickness of the nanosheet becomes thicker than before phosphating. Although the FeNi PBA cubes become less obvious after phosphating, only small encapsulated protrusions can be observed on the nanosheet array. These nanosheets are interconnected to form a network. The network with a porous structure will provide sufficient space for the transport / diffusion of electrolytes and hydrogen and oxygen. In addition, the nanosheets grown directly on the nickel foam will ensure the rapid transmission of electrons, which is beneficial to the reduction of the resistance of the Fe2P-Ni2P / NF electrocatalyst. The LSV diagram of the material can effectively prove this.

[0023] The LSV curve of the prepared Fe2P-Ni2P / NF after long-term oxygen evolution test under alkaline conditions is as follows: Figure 7 As shown in Figure 2, after 4000 CV cycles, the LSV curve of Fe2P-Ni2P / NF has almost no change. Figure 8 As shown in the figure, after 24 h of long-term stability test, the catalytic performance of Fe2P-Ni2P / NF remained almost unchanged compared with the initial performance, indicating that Fe2P-Ni2P / NF has excellent catalytic stability.

[0024] In addition to the above embodiments, the nickel source in step (1) can also be selected from nickel chloride or nickel sulfate; the iron source can also be selected from ferrous sulfate or ferric chloride; the ammonium source can also be selected from ammonium chloride, ammonium nitrate, urea and ammonium chloride, urea and ammonium nitrate, ammonium fluoride and ammonium chloride, ammonium fluoride and ammonium nitrate, and the solvent can also be ethanol or methanol. The molar ratio of the area of ​​the nickel foam to the nickel source can also be (2.7-3.3) cm 2 : any value within 1mmol; the concentration of the nickel source in the mixed solution is any value within 0.5-2mol / L; the molar ratio of the nickel source to the iron source is any value within (1-5):1; the molar ratio of the ammonium source to the nickel source is any value within (1-10):1.

[0025] 2. Experimental Results Analysis 1. Performance analysis of FeS-Ni3S2 / NF prepared by the method of Example 1 Control group 1: Preparation of Ni3S2 / NF catalyst a. Take the nickel foam, cut it into 1cm×3cm, place it in a beaker, add anhydrous ethanol until it is submerged, pour out the anhydrous ethanol after ultrasonication for 15min, add 1 mol / L dilute hydrochloric acid until it is submerged, and wash it with water after ultrasonication for 15min. 1 mmol Ni(NO3)2·6H2O, 8 mmol NH4F, 1 g PEG and 4 mmol urea are weighed and configured into 40 mL solution. Then, it is transferred to a 50 mL stainless steel autoclave lined with polytetrafluoroethylene, and the treated nickel foam is added. After constant temperature reaction at 120℃ for 5h, freeze-dried for 18h, nickel foam loaded with needle-shaped Ni transition metal hydroxide precursor, namely NiOOH / NF, is obtained. The molar ratio of the nickel foam area to the nickel source is 3cm 2 :1mmol; b. The NiOOH / NF obtained in step a was placed in a 30 mL mixed solution of polysulfide / DMF (V:V=1:2), and transferred to a 50 mL Teflon autoclave, and reacted at 180°C in an oven for 10 h. After cooling, it was washed and freeze-dried for 18 h to obtain a foamed nickel catalytic electrode loaded with mixed particles of ferrous sulfide and nickel sulfide, i.e., Ni3S2 / NF catalyst.

[0026] Control group 2: Preparation of FeS / NF catalyst a. Take nickel foam, cut it into 1cm×3cm, place it in a beaker, add anhydrous ethanol until it is submerged, pour out the anhydrous ethanol after ultrasonication for 15min, add 1 mol / L dilute hydrochloric acid until it is submerged, and wash it with water after ultrasonication for 15min. 1 mmol Fe(NO3)2·9H2O, 8 mmol NH4F, 1 g PEG and 4 mmol urea are weighed and prepared into 40 mL solution, which is then transferred to a 50mL stainless steel autoclave lined with polytetrafluoroethylene, and the treated nickel foam is added. After isothermal reaction at 120℃ for 5h, freeze-drying is carried out for 18h to obtain nickel foam loaded with Fe double transition metal hydroxide precursor, namely FeNi-LDH / NF, and the molar ratio of nickel foam area to nickel source is 3cm 2 :1mmol; b. The FeOOH / NF obtained in step a was placed in a 30 mL mixed solution of polysulfide / DMF (V:V=1:2), and transferred to a 50 mL Teflon autoclave, and reacted at 180°C in an oven for 10 h. After cooling, it was washed and freeze-dried for 18 h to obtain a foamed nickel catalytic electrode loaded with mixed particles of ferrous sulfide and nickel sulfide, i.e., FeS / NF catalyst.

[0027] Preparation method of RuO2 / NF: 4 mg of commercial RuO2 and 0.04 mL of Nafion solution (5%) were ultrasonically dispersed in a mixed solvent containing 0.72 mL of pure water and 0.24 mL of anhydrous ethanol. After the solution formed a uniform dispersion, 0.18 mL of the dispersion was dropwise dripped on the pretreated nickel foam and dried to obtain RuO2 / NF.

[0028] The electrochemical performance of Ni3S2 / NF prepared in control group 1, FeS prepared in control group 2 and other samples were tested. Figure 9-12 shown.

[0029] Polarization curves were obtained by linear sweep voltammetry (LSV) at a scan rate of 2 mV s -1 The test process needs to give 85% voltage drop compensation. The Tafel slope is calculated based on the LSV curve. The voltage value selected for the electrochemical impedance spectroscopy (EIS) test is the current density of the polarization curve is 20 mA cm -2 The voltage value at the time of the test was 100 KHz~0.1Hz, the step voltage was 5 mV, and the impedance data was fitted using Zsimpwin software after the test. Fig. 9 As shown, FeS-Ni3S2 / NF only needs 215 mV to reach 50 mA cm -2The current density is much lower than that of FeNi-LDH / NF (320 mV), Ni3S2 / NF (343 mV), FeS / NF (241 mV) and RuO2 / NF (367 mV). This shows the morphological advantages of the hierarchical nanorod structure of FeS-Ni3S2 / NF. This unique structural feature can not only expose more catalytic active sites, but also help release bubbles. The Tafel slope is an important indicator of catalyst reaction kinetics.

[0030] like Fig.10 As shown in Figure 2, the Tafel slope of FeS-Ni3S2 / NF is the smallest, which is 51 mV dec. -1 , lower than FeNi-LDH / NF (52 mV dec -1 ), Ni3S2 / NF (168 mV dec -1 ), FeS / NF (62 mV dec -1 ) and RuO2 (115 mV dec -1 ), indicating that FeS-Ni3S2 / NF has better OER reaction kinetics.

[0031] like Fig.11 As shown in the figure, it can be seen that FeS-Ni3S2 / NF has a charge transfer resistance (R ct ) is 5.38 Ω, which is much smaller than the charge transfer resistance of other materials. The impedance of the electrocatalyst doped with S is much smaller than that of FeNi-LDH / NF, indicating that the introduction of S changes the electronic structure of the catalyst material. On the other hand, the heterojunction interface of FeS-Ni3S2 / NF is conducive to electron transfer, thereby enhancing the conductivity and benefiting the occurrence of electrocatalytic reactions.

[0032] Fig.12 The CV curves of FeS / NF, Ni3S2 / NF, FeS-Ni3S2 / NF and FeNi-LDH / NF were measured at different scan rates in the non-Faraday range (0.76~0.86 V vs. RHE). The electrochemical double layer capacitance (C dl ), C of FeS-Ni3S2 / NF dl 86 mF / cm 2 , C of FeS / NF dl 55 mF / cm 2 , C of Ni3S2 / NF dl 27mF / cm 2 And the C of FeNi-LDH / NF dl 28 mF / cm 2 Since the electrochemical active area (ECSA) is related to C dlTherefore, FeS-Ni3S2 / NF has a larger electrochemical active area, which also confirms the influence of the catalyst surface morphology on the catalytic reaction. FeS-Ni3S2 / NF and FeS / NF with porous nano-grid structure not only expose a larger active surface area, but also the porous structure can promote the release of gas on the catalyst surface. Since the main structure of FeS-Ni3S2 / NF is a more closely arranged nanowire, and the pore size of the FeS-Ni3S2 / NF nano-network is smaller, it has more advantages in terms of morphology and structure. The catalytic electrode can provide more OER reaction active sites for H2O and reaction intermediates.

[0033] Combining the above results, it can be seen that FeS-Ni3S2 / NF has the smallest overpotential, the lowest Tafel slope, the smallest charge transfer resistance and the largest electrochemical double layer area. Therefore, it can be shown that FeS-Ni3S2 / NF has the best catalytic activity.

[0034] 2. Performance analysis of FeNi-LDH / NF prepared by the method of Example 2 Control group 3: a. A 3 cm × 1 cm nickel foam was ultrasonically treated in 3 M HCl solution, anhydrous ethanol and deionized water for 15 min to remove possible oxides on the surface, and then washed with ultrapure water for multiple times and dried for use. 1 mmol Ni(NO3)2·6H2O, 1 mmol Fe(NO3)3·9H2O, 6 mmol NH4F, 1 g PEG and 4 mmol urea were weighed and prepared into a 40 mL solution, which was then transferred to a 50 ml stainless steel autoclave lined with polytetrafluoroethylene, and the treated nickel foam was added. The reaction was carried out at 120°C for 5 h to obtain a nickel foam loaded with a needle-shaped layered FeNi double transition metal hydroxide precursor, namely FeNi-LDH / NF.

[0035] b. The FeNi-LDH / NF prepared in step a was placed in 20 mL of deionized water containing 0.18 mmol trisodium citrate, 0.06 mmol Ni(NO3)2·6H2O and 1 mmol K3[Fe(CN)6], and the mixture was reacted at 25°C in a high-pressure reactor for 24 h to obtain nickel foam loaded with FeNi-LDH particles with a hydrotalcite structure, namely PBAs-FeNi-LDH / NF.

[0036] Control group 4: a. A 3 cm × 1 cm nickel foam was ultrasonically treated in 3 M HCl solution, anhydrous ethanol and deionized water for 15 min to remove possible oxides on the surface, and then washed with ultrapure water for multiple times and dried for use. 1 mmol Ni(NO3)2·6H2O, 1 mmol Fe(NO3)3·9H2O, 6 mmol NH4F, 1 g PEG and 4 mmol urea were weighed and prepared into 40 mL solution, and then weighed and prepared into 40 ml solution according to the proportion, and then transferred to a 50 ml stainless steel autoclave lined with polytetrafluoroethylene, and the treated nickel foam was added, and the reaction was carried out at 120°C for 5 h to obtain nickel foam loaded with needle-shaped layered FeNi double transition metal hydroxide precursor, namely FeNi-LDH / NF.

[0037] b. After washing and drying the FeNi-LDH / NF obtained in step a, annealing and calcining with sodium hypophosphite at 350° C. for 2 h in a nitrogen atmosphere to obtain a nickel foam loaded with FeNi-P of hydrotalcite structure, namely FeNi-P / NF.

[0038] Preparation method of FeNi-P / NF-p: a. The pretreated NF was placed in 20 mL of deionized water containing 0.18 mmol trisodium citrate, 0.06 mmol Ni(NO3)2·6H2O and 1 mmol K3[Fe(CN)6], and reacted at 25°C in a high-pressure reactor for 24 h to obtain nickel foam loaded with particles of Prussian blue analogs, namely FeNi PBAs / NF; b. After washing and drying the FeNi PBAs / NF obtained in step a, the FeNi PBAs / NF was annealed and calcined with sodium hypophosphite at 350° C. for 2 h in a nitrogen atmosphere to obtain FeNi-P / NF-p (-p indicates that the precursor contains FeNi PBA).

[0039] The electrochemical performance of the catalytic electrode prepared in Example 2, the PBAs-FeNi-LDH / NF prepared in Control Group 3, the FeNi-P / NF and the FeNi-P / NF-p prepared in Control Group 4 were tested. Figure 13-15 shown.

[0040] Fig.13 The polarization curves of each catalytic electrode show that Fe2P-Ni2P / NF only needs an overpotential of 177 mV to reach 50 mA / cm 2 The current density of FeNi PBA / FeNi LDH / NF, FeNi-LDH / NF, FeNi-P / NF-p and FeNi-P / NF reached 50 mA / cm 2The overpotentials required for the current densities are 220 mV, 207 mV, 191 mV, and 194 mV, respectively. Moreover, at a larger current density of 200 mA / cm 2 , Fe2P-Ni2P / NF can also exhibit excellent OER performance (254 mV), which is also much lower than that of FeNi PBA / FeNi LDH / NF (316 mV), FeNi-LDH / NF (303 mV), FeNi-P / NF-p (261 mV), and FeNi-P / NF (280 mV) at the same current density, indicating that this electrocatalyst has great potential in industrial applications.

[0041] Fig.14 Figure 5 is the Tafel curve diagram of each sample calculated and fitted according to the polarization curve. It can be observed from the figure that the Tafel slope of Fe2P-Ni2P / NF is the smallest, which is 42 mV dec -1 , lower than that of FeNi PBA / FeNi LDH / NF (43 mV dec -1 ), FeNi-LDH / NF (46 mV dec -1 ), FeNi-P / NF-p (53 mV dec -1 ), and FeNi-P / NF (73 mV dec -1 ). This result indicates that Fe2P-Ni2P / NF has excellent reaction kinetics in an alkaline environment. The reaction kinetics during the OER process can also be studied through electrochemical impedance. The Nyquist curves of the fitted Fe2P-Ni2P / NF and the control samples are as Fig.15 shown. It can be seen from the figure that the solution internal resistances (R s ) of each electrode material are close. And the equivalent circuit of Fe2P-Ni2P / NF and the control samples is the Randles circuit, and Rct is reflected in the Nyquist curve as the curvature radius. After observation, the curvature radius sizes of each electrocatalyst are Fe2P-Ni2P / NF < FeNiPBA / FeNi LDH / NF < FeNi-P / NF < FeNi-LDH / NF < FeNi-P / NF-p. Therefore, the charge transfer resistance of Fe2P-Ni2P / NF is the smallest, and the fitted calculation is only 1.53 Ω, while the Rct values of FeNi PBA / FeNi LDH / NF, FeNi-LDH / NF, FeNi-P / NF-p, and FeNi-P / NF are 1.73 Ω, 1.94 Ω, 2.92 Ω, and 1.79 Ω, respectively. This shows that the Fe2P-Ni2P / NF electrocatalyst has stronger charge transfer ability and good reaction kinetics.

[0042] The electrochemical active area (ECSA) of the electrocatalyst can be obtained from the electrochemical double layer capacitance (Cdl) information, and C dl It is calculated and fitted from the CV diagrams at different scan rates. Fig.16 Fe2P-Ni2P / NF and its control sample at a scan rate of 20 mVs -1 ~100 mV s -1 CV diagram of the fitted C dl like Fig.16 As shown in Figure 2, Fe2P-Ni2P / NF has the largest Cdl, which is 20.47 mF cm -2 Greater than FeNi PBA / FeNi LDH / NF (15.16 mF cm -2 ), FeNi-LDH / NF (10.57 mF cm -2 ), FeNi-P / NF-p (14.64 mF cm -2 ) and FeNi-P / NF (18.55 mF cm -2 ), indicating that the excellent OER performance of Fe2P-Ni2P / NF is mainly attributed to its significant intrinsic catalytic activity, which also fully proves that Fe2P-Ni2P / NF nanoparticles have a larger electrochemical active area and better morphological advantages.

[0043] The above description is not intended to limit the present invention, and the present invention is not limited to the above examples. Any changes, modifications, additions or substitutions made by a person skilled in the art within the spirit and scope of the present invention shall also fall within the protection scope of the present invention.

Claims

1. A method for preparing a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support, characterized in that The following steps are involved: (1) preparing a transition metal-doped nickel hydroxide precursor on a sheet support by a hydrothermal method; (2) The transition metal-doped nickel hydroxide precursor obtained in step (1) is subjected to in-situ sulfurization / phosphating to obtain a transition metal-doped nickel sulfur / phosphorus compound and a support composite material catalytic electrode, wherein the transition metal-doped nickel sulfur / phosphorus compound is a FeS-Ni3S2 catalytic electrode or a Fe2P-Ni2P catalytic electrode.

2. The method for preparing a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support according to claim 1, characterized in that Step (1) is specifically as follows: adding the pretreated and dried nickel foam to a mixed solution consisting of a nickel source, an iron source and an ammonium source, and then reacting in a high-pressure reactor at 100-200° C. for 4-24 h, cooling, washing and drying to obtain a nickel foam with a layer of needle-shaped FeNi double transition metal hydroxide precursor loaded on the surface, recorded as FeNi-LDH / NF.

3. The method for preparing a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support according to claim 2, characterized in that Step (2) is specifically as follows: the nickel foam obtained in step (1) is placed in 20-40 mL of a mixed solution of polysulfide and N,N-dimethylformamide in a volume ratio of 1:2, and then reacted in a high-pressure reactor at 100-200° C. for 5-24 h, cooled, washed and dried to obtain a nickel foam catalytic electrode loaded with a rod-shaped hydrotalcite structure FeS-Ni3S2 nanoarray, recorded as a needle-shaped FeS-Ni3S2 / NF catalytic electrode, wherein the polysulfide is polysulfide with 1,3-diisopropenylbenzene as a cross-linking agent.

4. The method for preparing a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support according to claim 2, characterized in that Step (2) is as follows: the nickel foam obtained in step (1) is placed in 20 mL of deionized water containing 0.18 mmol of trisodium citrate, 0.06 mmol of Ni(NO3)2·6H2O and 0.08 mmol of K3[Fe(CN)6], reacted in a high pressure reactor at 10-50°C for 10-30 h, washed and dried to obtain a nickel foam loaded with a hydrotalcite structure FeNi-LDH / NF, recorded as FeNi PBAs-FeNi-LDH / NF; the nickel foam FeNi PBAs-FeNi-LDH / NF is mixed with a phosphorus source in a mass ratio of 3:1 and calcined in a tube furnace at a calcination temperature of 300-500°C for 2-4 h, washed and dried after cooling to obtain a nickel foam catalytic electrode loaded with a nanosheet array structure Fe2P-Ni2P, recorded as Fe2P-Ni2P / NF.

5. The method for preparing a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support according to claim 4, characterized in that: The phosphorus source is selected from red phosphorus or sodium hypophosphite powder.

6. A method for preparing a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support according to any one of claims 2 to 5, characterized in that: The molar ratio of the nickel foam area to the nickel source is (2.7-3.3) cm 2 :1mmol, the concentration of nickel source in the mixed solution is 0.5-2mol / L; the molar ratio of nickel source to iron source is (1-5):1; the molar ratio of ammonium source to nickel source is (1-10):

1.

7. A method for preparing a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support according to any one of claims 2 to 5, characterized in that: The nickel source is selected from any one of nickel nitrate, nickel chloride or nickel sulfate; the iron source is one of ferric nitrate, ferrous sulfate or ferric chloride; the ammonium source is selected from any one or any two of urea, ammonium fluoride, ammonium chloride or ammonium nitrate; and the solvent is any one of water, ethanol or methanol.

8. Use of a composite catalytic electrode of a transition metal-doped nickel-sulfur / phosphorus compound and a support prepared by the preparation method according to any one of claims 1 to 5 in the electrolysis of water to produce oxygen or hydrogen.