Viscose fiber with high water absorption performance for suppository carrier and preparation method of viscose fiber

By combining cotton fiber, rose fiber, bamboo fiber and modal fiber with mesoporous molecular sieve and wool keratin, viscose fiber with high water absorption and high wet state elasticity is prepared, which solves the problem of water absorption of viscose fiber in the existing technology. It solves the problems of insufficient rate and wet elasticity and improves the expansion effect and treatment efficiency of the drug.

CN118854476APending Publication Date: 2024-10-29HARBIN TIANMEI PHARM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410858954.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The viscose fiber in existing vaginal suppositories has low water absorption and low wet elasticity, which makes it difficult for the drug to effectively expand, prolongs the treatment time, and reduces the quality of treatment.

Method used

The mixed pulp of cotton fiber, rose fiber, bamboo fiber and modal fiber is soaked in alkaline solution, mesoporous molecular sieve and wool keratin yellowing reaction to form cellulose xanthate. After dissolution, it is matured and wet-processed. Spinning to prepare viscose fiber with high water absorption properties.

Benefits of technology

The water absorption rate and wet elasticity of the viscose fiber are improved, allowing the drug to expand more effectively, shortening the treatment time and improving the quality of treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854476A_ABST
    Figure CN118854476A_ABST
Patent Text Reader

Abstract

The invention provides viscose fiber with high water absorption performance for a suppository carrier and a preparation method of the viscose fiber, and relates to the technical field of medicines. The cotton fiber, the rose fiber, the bamboo fiber and the modal fiber in the preparation raw materials of the viscose fiber provided by the invention have good hygroscopicity; moreover, the wet elasticity of the modal fibers is relatively good, so that the prepared viscose fibers have relatively high hygroscopicity and wet elasticity; in addition, a mesoporous molecular sieve with a regular pore structure is introduced into the viscose fiber, so that the hygroscopicity of the viscose fiber is further improved; wool keratin is introduced into the viscose fiber, so that the hygroscopicity and the wet elasticity of the viscose fiber can be further improved. Experiments show that the viscose fiber provided by the invention has relatively high water absorption and relatively high wet elasticity at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of medical technology, in particular to a viscose fiber with high water absorption performance used as a suppository carrier and a preparation method thereof. Background Art

[0002] Viscose fiber is a kind of man-made fiber. Viscose fiber is widely used in many fields because of its smooth, cool, breathable and antistatic properties. Gynecological diseases are common and frequently-occurring diseases in women. At present, vaginal suppositories containing active ingredients for treating diseases are generally used to treat gynecological diseases. In existing vaginal suppositories, the expansion carrier is generally viscose fiber, but the viscose fiber currently used has a low water absorption rate and low wet elasticity, so that the expansion carrier cannot expand effectively, resulting in the inability of the drug to effectively reach the lesion, prolonging the treatment time, reducing the quality of treatment, and being unfavorable for the treatment of gynecological diseases. Summary of the invention

[0003] The problem solved by the invention is: how to obtain viscose fibers with both high water absorption and high wet elasticity.

[0004] In order to solve the above problems, the present invention provides a method for preparing viscose fiber with high water absorption performance for suppository carrier, comprising:

[0005] Step S1, mixing cotton fiber, rose fiber, bamboo fiber and modal fiber to obtain mixed pulp; wherein the mass ratio of the cotton fiber, the rose fiber, the bamboo fiber and the modal fiber is (15-35): (10-20): (10-30): (2-10);

[0006] Step S2, soaking the mixed pulp in a first alkaline solution to obtain an alkaline mixed pulp;

[0007] Step S3, adding mesoporous molecular sieve and wool keratin to the alkaline mixed pulp, mixing evenly, and adding carbon disulfide to carry out xanthation reaction to obtain cellulose xanthate; wherein the mass ratio of the cotton fiber, the mesoporous molecular sieve and the wool keratin is (15-35): (5-10): (5-10);

[0008] Step S4, dissolving the cellulose xanthate in a second alkaline solution to obtain a viscose solution;

[0009] Step S5, subjecting the viscose solution to a aging treatment to obtain a spinning solution;

[0010] Step S6, wet spinning the spinning solution to obtain viscose fibers.

[0011] Optionally, in step S3, the mesoporous molecular sieve includes one of a silicon-based molecular sieve and a non-silicon-based mesoporous molecular sieve.

[0012] Optionally, the silicon-based molecular sieve includes one of SBA-1 molecular sieve, SBA-2 molecular sieve, SBA-3 molecular sieve, SBA-15 molecular sieve and SBA-16 molecular sieve.

[0013] Optionally, the non-silicon-based mesoporous molecular sieve includes one of CMK-1 molecular sieve, CMK-2 molecular sieve and CMK-3 molecular sieve.

[0014] Optionally, in step S2, the first alkaline solution is a NaOH solution, the temperature of the immersion treatment is 50-60° C., and the time is 20-40 min.

[0015] Optionally, in step S3, the mass ratio of the carbon disulfide to the alkaline mixed pulp is 1:(10-12).

[0016] Optionally, in step S3, the temperature of the yellowing reaction is 20-30° C., and the time is 90-110 min.

[0017] Optionally, in step S5, the aging treatment is performed at a temperature of 20-25° C. and for a time of 20-40 min.

[0018] Optionally, in step S4, the second alkaline solution is a NaOH solution with a mass fraction of 5-10%, and the mass ratio of the second alkaline solution to the cellulose xanthate is (2-5):1.

[0019] The present invention also provides a viscose fiber with high water absorption performance for a suppository carrier, which is prepared by the preparation method of the viscose fiber with high water absorption performance for a suppository carrier as described above.

[0020] Compared with the prior art, the hygroscopicity of cotton fiber, rose fiber, bamboo fiber and modal fiber in the preparation raw materials of the viscose fiber provided by the present invention is good; moreover, the wet elasticity of modal fiber is good, so that the prepared viscose fiber has relatively high hygroscopicity and wet elasticity; in addition, the present invention also introduces a mesoporous molecular sieve with a regular pore structure into the viscose fiber, and the mesoporous molecular sieve with a regular pore structure not only provides a more convenient channel for water molecules to enter, but also makes the viscose fiber have a higher specific surface area, which is conducive to further improving the hygroscopicity of the viscose fiber; the present invention also introduces wool keratin into the viscose fiber, and the wool keratin not only has better hygroscopicity, but also has better wet elasticity, so it can further improve the hygroscopicity and wet elasticity of the viscose fiber. It is found through experiments that the viscose fiber provided by the present invention has both high water absorption and high wet elasticity. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The figure is a schematic flow chart of a method for preparing viscose fiber with high water absorption performance used as a suppository carrier in an embodiment of the present invention. DETAILED DESCRIPTION

[0022] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. Although certain embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be interpreted as being limited to the embodiments described herein. On the contrary, these embodiments are provided to provide a more thorough and complete understanding of the present invention. It should be understood that the drawings and embodiments of the present invention are only for exemplary purposes and are not intended to limit the scope of protection of the present invention.

[0023] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by those skilled in the art to which this application belongs; the terms used in the specification of this application are only for the purpose of describing specific implementation methods and are not intended to limit this application;

[0024] The term "including" and its variations used in this article are open inclusions, that is, "including but not limited to"; the term "based on" is "based at least in part on"; the term "one embodiment" means "at least one embodiment"; the term "another embodiment" means "at least one other embodiment"; the term "some embodiments" means "at least some embodiments"; the term "optionally" means "optional embodiments". The relevant definitions of other terms will be given in the following description. It should be noted that the concepts of "first" and "second" mentioned in the present invention are used to distinguish different objects, rather than to describe a specific order or a primary and secondary relationship. In addition, the terms "first" and "second" are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of this application, unless otherwise specified, the meaning of "multiple" is two or more.

[0025] like Figure 1 As shown, an embodiment of the present invention provides a method for preparing viscose fiber with high water absorption performance for suppository carrier, comprising:

[0026] Step S1, mixing cotton fiber, rose fiber, bamboo fiber and modal fiber to obtain mixed pulp; wherein the mass ratio of the cotton fiber, the rose fiber, the bamboo fiber and the modal fiber is (15-35): (10-20): (10-30): (2-10);

[0027] Step S2, soaking the mixed pulp in a first alkaline solution to obtain an alkaline mixed pulp;

[0028] Step S3, adding mesoporous molecular sieve and wool keratin to the alkaline mixed pulp, mixing evenly, and adding carbon disulfide to carry out xanthation reaction to obtain cellulose xanthate; wherein the mass ratio of the cotton fiber, the mesoporous molecular sieve and the wool keratin is (15-35): (5-10): (5-10);

[0029] Step S4, dissolving the cellulose xanthate in a second alkaline solution to obtain a viscose solution;

[0030] Step S5, subjecting the viscose solution to a aging treatment to obtain a spinning solution;

[0031] Step S6, wet spinning the spinning solution to obtain viscose fibers.

[0032] Among the raw materials for preparing the viscose fiber provided by the embodiment of the present invention, cotton fiber, rose fiber, bamboo fiber and modal fiber all have good hygroscopicity; moreover, modal fiber has good wet elasticity, so that the prepared viscose fiber has relatively high hygroscopicity and wet elasticity; in addition, in the embodiment of the present invention, a mesoporous molecular sieve with a regular pore structure is introduced into the viscose fiber. The mesoporous molecular sieve with a regular pore structure not only provides a more convenient channel for water molecules to enter, but also makes the viscose fiber have a higher specific surface area, which is conducive to further improving the hygroscopicity of the viscose fiber; in the present invention, wool keratin is introduced into the viscose fiber. The wool keratin not only has better hygroscopicity, but also has better wet elasticity, so the hygroscopicity and wet elasticity of the viscose fiber can be further improved. It is found through experiments that the viscose fiber provided by the embodiment of the present invention has both high water absorption and high wet elasticity.

[0033] Illustratively, in some embodiments of the present invention, in step S3, the method for preparing wool keratin comprises:

[0034] Add the wool into a 10% by mass NaOH solution, heat to 100° C., and react for 4-6 hours under nitrogen to obtain a reaction mixed solution;

[0035] The reaction mixture solution is filtered and centrifuged to remove insoluble matter to obtain a wool keratin solution;

[0036] The wool keratin solution is freeze-dried to obtain wool keratin; wherein the freeze-drying temperature is -55°C and the time is 8-10 hours.

[0037] In some embodiments of the present invention, in step S3, the mesoporous molecular sieve includes one of a silicon-based molecular sieve and a non-silicon-based mesoporous molecular sieve; wherein the silicon-based molecular sieve includes one of an SBA-1 molecular sieve, an SBA-2 molecular sieve, an SBA-3 molecular sieve, an SBA-15 molecular sieve and an SBA-16 molecular sieve; and the non-silicon-based mesoporous molecular sieve includes one of a CMK-1 molecular sieve, a CMK-2 molecular sieve and a CMK-3 molecular sieve.

[0038] In some embodiments of the present invention, in step S2, the first alkaline solution is a NaOH solution with a mass fraction of 10%, the temperature of the immersion treatment is 50-60° C., and the time is 20-40 min.

[0039] In some embodiments of the present invention, in step S3, the mass ratio of the carbon disulfide to the alkaline mixed pulp is 1:(10-12); the temperature of the yellowing reaction is 20-30°C, and the time is 90-110 min.

[0040] In some embodiments of the present invention, in step S4, the second alkaline solution is a NaOH solution with a mass fraction of 5-10%, and the mass ratio of the second alkaline solution to the cellulose xanthate is (2-5):1.

[0041] In some embodiments of the present invention, in step S5, the aging treatment is performed at a temperature of 20-25° C. and for a time of 20-40 min.

[0042] The embodiment of the present invention further provides a viscose fiber with high water absorption performance for a suppository carrier, which is prepared by the preparation method of the viscose fiber with high water absorption performance for a suppository carrier as described above.

[0043] The present invention is further described below in conjunction with specific embodiments.

[0044] Example 1

[0045] A1. Cotton fiber, rose fiber, bamboo fiber and modal fiber are mixed to obtain mixed pulp; wherein the mass ratio of the cotton fiber, the rose fiber, the bamboo fiber and the modal fiber is 25:15:20:6.

[0046] A2. Immersing the mixed pulp in a NaOH solution to obtain an alkaline mixed pulp; wherein the immersion temperature is 55° C. and the time is 30 min.

[0047] A3. Adding mesoporous molecular sieve and wool keratin to the alkaline mixed pulp, mixing evenly, adding carbon disulfide for xanthation reaction to obtain cellulose xanthate; wherein the mass ratio of the cotton fiber, the mesoporous molecular sieve and the wool keratin is 25:8:8, the mesoporous molecular sieve is SBA-15 molecular sieve, the mass ratio of the carbon disulfide to the alkaline mixed pulp is 1:11, the temperature of the xanthation reaction is 25°C, and the time is 100 min.

[0048] A4. Dissolving the cellulose xanthate in a NaOH solution (mass fraction of 10%) to obtain a viscose solution; wherein the mass ratio of the NaOH solution to the cellulose xanthate is 3:1.

[0049] A5. The viscose solution is subjected to a aging treatment to obtain a spinning solution; the aging treatment is performed at a temperature of 20° C. for 30 minutes.

[0050] A6. Wet spinning the spinning solution to obtain viscose fibers.

[0051] Example 2

[0052] A1. Cotton fiber, rose fiber, bamboo fiber and modal fiber are mixed to obtain mixed pulp; wherein the mass ratio of the cotton fiber, the rose fiber, the bamboo fiber and the modal fiber is 15:10:10:2.

[0053] A2. Immersing the mixed pulp in a NaOH solution to obtain an alkaline mixed pulp; wherein the immersion temperature is 55° C. and the time is 30 min.

[0054] A3. Add mesoporous molecular sieve and wool keratin to the alkaline mixed pulp, mix evenly, and then add carbon disulfide to carry out xanthation reaction to obtain cellulose xanthate; wherein the mass ratio of the cotton fiber, the mesoporous molecular sieve and the wool keratin is 3:1:1, the mesoporous molecular sieve is SBA-15 molecular sieve, the mass ratio of the carbon disulfide to the alkaline mixed pulp is 1:11, the temperature of the xanthation reaction is 25°C, and the time is 100 min.

[0055] A4. Dissolving the cellulose xanthate in a NaOH solution (mass fraction of 10%) to obtain a viscose solution; wherein the mass ratio of the NaOH solution to the cellulose xanthate is 3:1.

[0056] A5. The viscose solution is subjected to a aging treatment to obtain a spinning solution; the aging treatment is performed at a temperature of 20° C. for 30 minutes.

[0057] A6. Wet spinning the spinning solution to obtain viscose fibers.

[0058] Example 3

[0059] A1. Cotton fiber, rose fiber, bamboo fiber and modal fiber are mixed to obtain mixed pulp; wherein the mass ratio of the cotton fiber, the rose fiber, the bamboo fiber and the modal fiber is 35:20:20:10.

[0060] A2. Immersing the mixed pulp in a NaOH solution to obtain an alkaline mixed pulp; wherein the immersion temperature is 55° C. and the time is 30 min.

[0061] A3. Add mesoporous molecular sieve and wool keratin to the alkaline mixed pulp, mix them evenly, and then add carbon disulfide to carry out xanthation reaction to obtain cellulose xanthate; wherein the mass ratio of the cotton fiber, the mesoporous molecular sieve and the wool keratin is 7:2:2, the mesoporous molecular sieve is SBA-15 molecular sieve, the mass ratio of the carbon disulfide to the alkaline mixed pulp is 1:11, the temperature of the xanthation reaction is 25°C, and the time is 100 min.

[0062] A4. Dissolving the cellulose xanthate in a NaOH solution (mass fraction of 10%) to obtain a viscose solution; wherein the mass ratio of the NaOH solution to the cellulose xanthate is 3:1.

[0063] A5. The viscose solution is subjected to a aging treatment to obtain a spinning solution; the aging treatment is performed at a temperature of 20° C. for 30 minutes.

[0064] A6. Wet spinning the spinning solution to obtain viscose fibers.

[0065] Comparative Example 1

[0066] The difference from Example 1 is that step A3 is: adding wool keratin to the alkaline mixed pulp, mixing evenly, and then adding carbon disulfide to carry out xanthation reaction to obtain cellulose xanthate; wherein the mass ratio of the cotton fiber to the wool keratin is 25:8, the mesoporous molecular sieve is SBA-15 molecular sieve, the mass ratio of the carbon disulfide to the alkaline mixed pulp is 1:11, the temperature of the xanthation reaction is 25°C, and the time is 100 min.

[0067] Comparative Example 2

[0068] The difference from Example 1 is that step A3 is: adding mesoporous molecular sieve to the alkaline mixed pulp, mixing evenly, and then adding carbon disulfide to carry out xanthation reaction to obtain cellulose xanthate; wherein the mass ratio of the cotton fiber to the mesoporous molecular sieve is 25:8, the mesoporous molecular sieve is SBA-15 molecular sieve, the mass ratio of the carbon disulfide to the alkaline mixed pulp is 1:11, the temperature of the xanthation reaction is 25°C, and the time is 100 min.

[0069] Experimental example

[0070] The water absorption rate and wet elastic modulus of the viscose fibers prepared in Examples 1-3 and Comparative Examples 1-2 were tested, and the results are shown in Table 1. As can be seen from Table 1, compared with Comparative Examples 1-2, the viscose fibers prepared in Examples 1-3 have higher water absorption rate, and compared with Comparative Example 2, the viscose fibers prepared in Examples 1-3 have lower wet elastic modulus, that is, the viscose fibers in Examples 1-3 have higher wet elasticity. In summary, the viscose fibers prepared in Examples 1-3 have both higher water absorption rate and higher wet elasticity.

[0071] Table 1

[0072]

[0073] Water absorption rate detection method: weigh 10g of viscose fiber, place it in a vacuum drying oven at 40℃ for 1 hour, take it out and accurately weigh it with an analytical balance, and record the weighing result as W0. Put the weighed viscose fiber in a constant temperature and humidity box with a relative humidity of 90% and a temperature of 20℃ for 4 hours, take it out and accurately weigh it with an analytical balance, and record the weighing result as W1; calculate the water absorption rate of viscose fiber according to the following formula:

[0074] Water absorption rate = (W1-W0) / W0×100%.

[0075] Although the present invention is disclosed as above, the protection scope of the present invention is not limited thereto. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention, and these changes and modifications will fall within the protection scope of the present invention.

Claims

1. A method for preparing viscose fiber with high water absorption performance for suppository carrier, characterized in that: include: Step S1, mixing cotton fiber, rose fiber, bamboo fiber and modal fiber to obtain mixed pulp; wherein the mass ratio of the cotton fiber, the rose fiber, the bamboo fiber and the modal fiber is (15-35): (10-20): (10-30): (2-10); Step S2, soaking the mixed pulp in a first alkaline solution to obtain an alkaline mixed pulp; Step S3, adding mesoporous molecular sieve and wool keratin to the alkaline mixed pulp, mixing evenly, and adding carbon disulfide to carry out xanthation reaction to obtain cellulose xanthate; wherein the mass ratio of the cotton fiber, the mesoporous molecular sieve and the wool keratin is (15-35): (5-10): (5-10); Step S4, dissolving the cellulose xanthate in a second alkaline solution to obtain a viscose solution; Step S5, subjecting the viscose solution to a aging treatment to obtain a spinning solution; Step S6, wet spinning the spinning solution to obtain viscose fibers.

2. The method for preparing viscose fiber with high water absorption performance for suppository carrier according to claim 1, characterized in that: In the step S3, the mesoporous molecular sieve includes one of a silicon-based molecular sieve and a non-silicon-based mesoporous molecular sieve.

3. The method for preparing viscose fiber with high water absorption performance for suppository carrier according to claim 2, characterized in that: The silicon-based molecular sieve includes one of SBA-1 molecular sieve, SBA-2 molecular sieve, SBA-3 molecular sieve, SBA-15 molecular sieve and SBA-16 molecular sieve.

4. The method for preparing viscose fiber with high water absorption performance for suppository carrier according to claim 2, characterized in that: The non-silicon-based mesoporous molecular sieve includes one of CMK-1 molecular sieve, CMK-2 molecular sieve and CMK-3 molecular sieve.

5. The method for preparing viscose fiber with high water absorption performance for suppository carrier according to claim 1, characterized in that: In the step S2, the first alkaline solution is a NaOH solution, the temperature of the immersion treatment is 50-60°C, and the time is 20-40 minutes.

6. The method for preparing viscose fiber with high water absorption performance for suppository carrier according to claim 1, characterized in that: In the step S3, the mass ratio of the carbon disulfide to the alkaline mixed pulp is 1:(10-12).

7. The method for preparing viscose fiber with high water absorption performance for suppository carrier according to claim 1, characterized in that: In step S3, the temperature of the yellowing reaction is 20-30° C. and the time is 90-110 min.

8. The method for preparing viscose fiber with high water absorption performance for suppository carrier according to claim 1, characterized in that: In step S5, the aging treatment is performed at a temperature of 20-25° C. and for a time of 20-40 min.

9. The method for preparing viscose fiber with high water absorption performance for suppository carrier according to claim 1, characterized in that: In the step S4, the second alkaline solution is a NaOH solution with a mass fraction of 5-10%, and the mass ratio of the second alkaline solution to the cellulose xanthate is (2-5):

1.

10. A viscose fiber with high water absorption performance for suppository carrier, characterized in that: The method for preparing the viscose fiber with high water absorption performance for suppository carrier according to any one of claims 1 to 9 is adopted.