A method for preparing viscose-based carbon fiber material

Through the use of double impregnation and modified phenolic resin solution, the problems of low strength and high thermal conductivity of viscose-based carbon fiber materials are solved, and the preparation of high-strength and low thermal conductivity of carbon fiber materials has been achieved, which has improved its in metallurgy, photovoltaic and other fields application potential.

CN118854494BActive Publication Date: 2024-12-06ANHUI HONGCHANG NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411348881.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-26
Publication Date
2024-12-06
Estimated Expiration
2044-09-26

AI Technical Summary

Technical Problem

Viscose-based carbon fiber insulation materials have problems of low strength and high thermal conductivity, which limits their application potential in metallurgy, photovoltaic and other fields.

Method used

By using the double impregnation method, the viscose-based white felt is first impregnated, dried and pre-oxidized in the organic and inorganic impregnation liquid, and then impregnated, cured and carbide graphitized in the modified phenolic resin solution to form high-strength and low heat conduction. Carbon fiber material with coefficient.

Benefits of technology

It significantly improves the mechanical properties and thermal insulation properties of viscose-based carbon fiber materials, and enhances its thermal insulation effect in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the field of carbon fiber materials, and in particular to a method for preparing a viscose-based carbon fiber material, comprising the following steps: impregnating a viscose-based white felt in an organic impregnation liquid and an inorganic impregnation liquid, drying, and pre-oxidizing to obtain a viscose-based pre-oxidized felt; impregnating the viscose-based pre-oxidized felt in a modified phenolic resin solution, curing, and carbonizing and graphitizing to obtain a viscose-based carbon fiber material. Compared with the prior art, the present invention has the following beneficial effects: the viscose-based carbon fiber material prepared by the present invention has higher strength, lower thermal conductivity, and excellent mechanical properties and thermal insulation properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of carbon fiber materials, and in particular to a method for preparing a viscose-based carbon fiber material. Background Art

[0002] The main organic precursors for producing carbon fibers are viscose fiber, polyacrylonitrile fiber, asphalt fiber, etc. The carbon fibers prepared from different precursors have different characteristics. Among them, viscose fiber has become the earliest raw material used in the preparation of carbon fibers due to its low price and abundant resources.

[0003] Viscose-based carbon fiber is a fibrous carbon material and an excellent carbon-reinforced material for both military and civilian use. Viscose-based carbon fiber thermal insulation material is made by weaving viscose-based raw fibers and then graphitizing them. It has low density, corrosion resistance, high temperature resistance, fatigue resistance, low thermal expansion coefficient, and good softness. It can achieve thermal insulation effects through wrapping. It has great market potential for use in metallurgical, photovoltaic and other equipment. However, viscose-based carbon fiber thermal insulation materials also have disadvantages such as low strength and high thermal conductivity. Summary of the invention

[0004] In order to solve the problems mentioned in the above background technology, the present invention provides a method for preparing a viscose-based carbon fiber material.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions:

[0006] A method for preparing a viscose-based carbon fiber material comprises the following steps:

[0007] The viscose-based white felt is impregnated in an organic impregnation liquid and an inorganic impregnation liquid, dried, and pre-oxidized to obtain a viscose-based pre-oxidized felt;

[0008] The viscose-based pre-oxidized felt is impregnated in a modified phenolic resin solution, cured, carbonized and graphitized to obtain a viscose-based carbon fiber material;

[0009] The preparation method of the organic impregnation solution is as follows:

[0010] Dispersing 1-methylindole-3-carboxylic acid in thionyl chloride, heating for reaction, removing excess thionyl chloride, adding ethanolamine and toluene, heating for reaction, and obtaining an ethanolamine derivative;

[0011] dispersing the ethanolamine derivative and ethylene glycol in ethanol to obtain an organic impregnation solution;

[0012] The preparation method of the inorganic impregnation solution is as follows:

[0013] Ammonium sulfate, ammonium chloride and ammonium bicarbonate are dispersed in water to obtain an inorganic impregnation solution.

[0014] Preferably, the preparation method of the modified phenolic resin solution is as follows:

[0015] Phenol and N-(3-aminopropyl)-N-ethylaniline are dispersed in ethanol, stirred evenly, and sodium hydroxide aqueous solution and formaldehyde aqueous solution are added to polymerize to obtain a modified phenolic resin;

[0016] The modified phenolic resin is dispersed in ethanol to obtain a modified phenolic resin solution.

[0017] Preferably, the organic impregnation solution is composed of 1-5 parts of ethanolamine derivative, 5-15 parts of ethylene glycol and 100 parts of ethanol in parts by mass.

[0018] Preferably, the inorganic impregnation solution is composed of 2-4 parts of ammonium sulfate, 2-4 parts of ammonium chloride, 4-6 parts of ammonium bicarbonate and 100 parts of water in parts by mass.

[0019] Preferably, in the polymerization reaction of the modified phenolic resin, the mass ratio of phenol, N-(3-aminopropyl)-N-ethylaniline, sodium hydroxide and formaldehyde is 100:(4-8):(0.5-1.5):(40-60).

[0020] Preferably, the modified phenolic resin solution is composed of 40-60 parts of modified phenolic resin and 100 parts of ethanol in parts by mass.

[0021] Preferably, the immersion time in the organic impregnation solution is 25-35 min; and the immersion time in the inorganic impregnation solution is 45-55 min.

[0022] Preferably, the pre-oxidation conditions are: pre-oxidation at 140-150°C for 5-15 min, pre-oxidation at 160-170°C for 10-20 min, pre-oxidation at 200-220°C for 10-20 min, pre-oxidation at 230-250°C for 10-20 min, and pre-oxidation at 260-280°C for 20-40 min.

[0023] Preferably, the immersion time in the modified phenolic resin solution is 15-25 minutes, and the curing conditions are: curing at 150-160° C. for 25-35 minutes.

[0024] Preferably, the carbonization and graphitization conditions are: treatment at 295-305°C for 10-20 min, 495-505°C for 5-15 min, 1200-1400°C for 35-45 min, 1600-1800°C for 0.5-1.5 h, and 2000-2200°C for 1-2 h.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] 1. The viscose-based carbon fiber material prepared by the present invention has high strength, low thermal conductivity, and excellent mechanical properties and thermal insulation properties.

[0027] 2. The viscose-based white felt of the present invention is double-impregnated with an organic impregnation liquid and an inorganic impregnation liquid, and pre-oxidized to obtain a viscose-based pre-oxidized felt, wherein the organic impregnation liquid is composed of an ethanolamine derivative, ethylene glycol and ethanol, and the organic and inorganic impregnation liquids promote intermolecular cross-linking, oxidation and other reactions of the viscose fiber macromolecular chains, prevent the formation of L-glucose, and improve the performance of the pre-oxidized felt.

[0028] 3. The viscose-based pre-oxidized felt is impregnated, cured, and carbonized and graphitized in a modified phenolic resin solution to obtain a viscose-based carbon fiber material. The phenolic resin is modified by N-(3-aminopropyl)-N-ethyl, and then impregnated and cured to achieve a better combination between the pre-oxidized felt and the resin. During the subsequent carbonization and graphitization, the formed graphite carbon can be well filled in the voids inside the material, thereby improving the mechanical properties and thermal insulation properties of the carbon fiber material. DETAILED DESCRIPTION

[0029] Unless otherwise specified, the raw materials and reagents used in the present invention are commercially available or can be prepared by known methods.

[0030] Preparation Example 1

[0031] Disperse 17.5 g of 1-methylindole-3-carboxylic acid in 200 g of thionyl chloride, react at 80° C. for 3 h, distill off the thionyl chloride, then add 6.2 g of ethanolamine and 100 g of toluene, react at 100° C. for 2 h, distill off the toluene, add saturated sodium bicarbonate solution and stir for 1 h, extract with ethyl acetate, concentrate and dry to obtain an ethanolamine derivative.

[0032] Preparation Example 2

[0033] Disperse 100 parts of phenol and 6 parts of N-(3-aminopropyl)-N-ethylaniline in 150 parts of anhydrous ethanol by mass, stir evenly, add 3 mol / L sodium hydroxide solution (containing 1 part of sodium hydroxide), add formaldehyde aqueous solution with a mass concentration of 20% (containing 50 parts of formaldehyde), react at 75°C for 5 hours, and obtain a modified phenolic resin.

[0034] Preparation Example 3

[0035] By mass, 100 parts of phenol were dispersed in 150 parts of anhydrous ethanol, stirred evenly, 3 mol / L sodium hydroxide solution (containing 1 part of sodium hydroxide) and 20% formaldehyde aqueous solution (containing 50 parts of formaldehyde) were added, and the mixture was reacted at 75°C for 5 hours to obtain phenolic resin. Example 1

[0036] A method for preparing a viscose-based carbon fiber material comprises the following steps:

[0037] The viscose-based white felt (weight 500g / m 2 ) is immersed in an organic impregnation liquid for 30 minutes, immersed in an inorganic impregnation liquid for 50 minutes, dried, and pre-oxidized at 145°C for 10 minutes, 165°C for 15 minutes, 210°C for 15 minutes, 240°C for 15 minutes, and 270°C for 30 minutes to obtain a viscose-based pre-oxidized felt;

[0038] The viscose-based pre-oxidized felt was immersed in the modified phenolic resin solution for 20 minutes, cured at 155°C for 30 minutes, and the carbonization and graphitization conditions were sequentially treated at 300°C for 15 minutes, 500°C for 10 minutes, 1300°C for 40 minutes, 1700°C for 1 hour, and 2100°C for 1.5 hours to obtain a viscose-based carbon fiber material.

[0039] Wherein, the organic impregnation solution is composed of 3 parts of ethanolamine derivative (obtained in Preparation Example 1), 10 parts of ethylene glycol, and 100 parts of ethanol, by weight;

[0040] The inorganic impregnation solution consists of 3 parts of ammonium sulfate, 3 parts of ammonium chloride, 5 parts of ammonium bicarbonate, and 100 parts of water by weight;

[0041] The modified phenolic resin solution is composed of 50 parts of modified phenolic resin (obtained in Preparation Example 2) and 100 parts of ethanol by mass. Example 2

[0042] The difference between this embodiment and embodiment 1 is that:

[0043] The organic impregnation solution is composed of 1 part of ethanolamine derivative (obtained in Preparation Example 1), 10 parts of ethylene glycol, and 100 parts of ethanol by weight;

[0044] The rest is exactly the same as in Example 1. Example 3

[0045] The difference between this embodiment and embodiment 1 is that:

[0046] The organic impregnation solution is composed of 5 parts of ethanolamine derivative (obtained in Preparation Example 1), 10 parts of ethylene glycol, and 100 parts of ethanol by mass;

[0047] The rest is exactly the same as in Example 1. Example 4

[0048] The difference between this embodiment and embodiment 1 is that:

[0049] The modified phenolic resin solution is composed of 40 parts of modified phenolic resin (obtained in Preparation Example 2) and 100 parts of ethanol by weight;

[0050] The rest is exactly the same as in Example 1. Example 5

[0051] The difference between this embodiment and embodiment 1 is that:

[0052] The modified phenolic resin solution is composed of 60 parts of modified phenolic resin (obtained in Preparation Example 2) and 100 parts of ethanol by weight;

[0053] The rest is exactly the same as in Example 1.

[0054] Comparative Example 1

[0055] The difference between this comparative example and Example 1 is that:

[0056] The viscose-based white felt (weight 500g / m 2 ) was immersed in the inorganic impregnation solution for 50 minutes.

[0057] That is, no organic impregnation liquid is used for impregnation;

[0058] The rest is exactly the same as in Example 1.

[0059] Comparative Example 2

[0060] The difference between this comparative example and Example 1 is that:

[0061] Immerse the viscose-based preoxidized felt in the phenolic resin solution for 20 minutes;

[0062] In parts by mass, the phenolic resin solution consists of 50 parts of phenolic resin (obtained in Preparation Example 3), 100 parts of ethanol;

[0063] The rest is exactly the same as in Example 1.

[0064] Comparative Example 3

[0065] The difference between this comparative example and Example 1 is that:

[0066] The viscose-based white felt (weight 500g / m 2 ) impregnated in an inorganic impregnation solution for 50 min, that is, impregnation without using an organic impregnation solution;

[0067] Immerse the viscose-based preoxidized felt in the phenolic resin solution for 20 minutes;

[0068] In parts by mass, the phenolic resin solution consists of 50 parts of phenolic resin (obtained in Preparation Example 3), 100 parts of ethanol;

[0069] The rest is exactly the same as in Example 1.

[0070] Results and Testing

[0071] Compression strength: The compression test was carried out using an INSTRON-5567A universal material testing machine. The sample length was 50 mm, the width was 50 mm, the thickness was 10 mm, the compression speed was 2 mm / min, and the test was stopped when the compression amount reached 5%.

[0072] Thermal conductivity: The DRS-III high temperature thermal conductivity tester was used to test the thermal conductivity of the sample sintered to a high temperature environment of 1100°C. The sample length was 25mm, width was 25mm, and thickness was 10mm.

[0073] The results are shown in Table 1.

[0074] Table 1

[0075]

[0076] From Table 1 and Examples 1-5, it can be seen that the viscose-based carbon fiber material prepared by the present invention has high strength, low thermal conductivity, and excellent mechanical properties and thermal insulation properties.

[0077] By comparing Example 1 and Comparative Examples 1-3, it can be seen that the impregnation of the organic impregnation liquid and the impregnation of the modified phenolic resin solution play a very important role in the performance of the viscose-based carbon fiber material. Regardless of the lack of impregnation of the organic impregnation liquid or the lack of impregnation of the modified phenolic resin solution, the performance of the viscose-based carbon fiber material is significantly reduced. However, when the two are used at the same time, the performance of the viscose-based carbon fiber material is significantly improved, with a synergistic enhancement effect.

[0078] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a viscose-based carbon fiber material, characterized in that: The steps include: The viscose-based white felt is impregnated in an organic impregnation liquid and an inorganic impregnation liquid, dried, and pre-oxidized to obtain a viscose-based pre-oxidized felt; The viscose-based pre-oxidized felt is impregnated in a modified phenolic resin solution, cured, carbonized and graphitized to obtain a viscose-based carbon fiber material; The preparation method of the organic impregnation solution is as follows: Dispersing 1-methylindole-3-carboxylic acid in thionyl chloride, heating for reaction, removing excess thionyl chloride, adding ethanolamine and toluene, heating for reaction, and obtaining an ethanolamine derivative; dispersing the ethanolamine derivative and ethylene glycol in ethanol to obtain an organic impregnation solution; The preparation method of the inorganic impregnation solution is as follows: Dispersing ammonium sulfate, ammonium chloride and ammonium bicarbonate in water to obtain an inorganic impregnation solution; The preparation method of the modified phenolic resin solution is as follows: Phenol and N-(3-aminopropyl)-N-ethylaniline are dispersed in ethanol, stirred evenly, and sodium hydroxide aqueous solution and formaldehyde aqueous solution are added to polymerize to obtain a modified phenolic resin; dispersing the modified phenolic resin in ethanol to obtain a modified phenolic resin solution; The organic impregnation solution is composed of 1-5 parts of ethanolamine derivative, 5-15 parts of ethylene glycol, and 100 parts of ethanol by weight; The inorganic impregnation liquid is composed of 2-4 parts of ammonium sulfate, 2-4 parts of ammonium chloride, 4-6 parts of ammonium bicarbonate and 100 parts of water by weight; The modified phenolic resin solution is composed of 40-60 parts of modified phenolic resin and 100 parts of ethanol in parts by mass.

2. The method for preparing a viscose-based carbon fiber material according to claim 1, characterized in that: In the polymerization reaction of the modified phenolic resin, the mass ratio of phenol, N-(3-aminopropyl)-N-ethylaniline, sodium hydroxide and formaldehyde is 100:(4-8):(0.5-1.5):(40-60).

3. The method for preparing a viscose-based carbon fiber material according to claim 1, characterized in that: The immersion time in the organic impregnation solution is 25-35 minutes; the immersion time in the inorganic impregnation solution is 45-55 minutes.

4. The method for preparing a viscose-based carbon fiber material according to claim 1, characterized in that: The pre-oxidation conditions are: pre-oxidation at 140-150° C. for 5-15 min, pre-oxidation at 160-170° C. for 10-20 min, pre-oxidation at 200-220° C. for 10-20 min, pre-oxidation at 230-250° C. for 10-20 min, and pre-oxidation at 260-280° C. for 20-40 min.

5. The method for preparing a viscose-based carbon fiber material according to claim 1, characterized in that: The immersion time in the modified phenolic resin solution is 15-25 minutes, and the curing conditions are: curing at 150-160° C. for 25-35 minutes.

6. The method for preparing a viscose-based carbon fiber material according to claim 1, characterized in that: The carbonization and graphitization conditions are: treating at 295-305° C. for 10-20 min, treating at 495-505° C. for 5-15 min, treating at 1200-1400° C. for 35-45 min, treating at 1600-1800° C. for 0.5-1.5 h, and treating at 2000-2200° C. for 1-2 h.