Formula and preparation method of friction plate of ternary composite non-metal friction material
By using harmless materials such as phenolic resin to prepare ternary composite non-metallic friction materials, the problem of harmful metal components in existing friction materials is solved, the high-temperature stability and wear resistance are improved, and the dual requirements of environmental protection and performance are met. .
Patent Information
- Application Number
- CN202410856247.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
AI Technical Summary
Existing friction materials contain harmful metal components such as cadmium, hexavalent chromium and mercury, which are difficult to meet domestic and foreign environmental protection standards, resulting in reduced friction coefficient and poor high-temperature stability.
Using harmless materials such as phenolic resin, calcium sulfate whiskers, glass fiber, flake graphite, barium sulfate, nitrile rubber powder, aramid pulp, polyacrylonitrile, petroleum coke, carbon black, alumina and magnesium oxide, through specific The formula and preparation method form a ternary composite non-metallic friction material to avoid the use of harmful metals.
It achieves the stability of the friction coefficient and wear resistance at high temperatures, reduces changes in the friction coefficient, improves the toughness and service life of the material, and meets the dual requirements of environmental protection and performance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_4
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of friction materials, and in particular to a friction plate formula and a preparation method of a ternary composite non-metallic friction material. Background Art
[0002] Automobile brake pads are key components of automobile braking systems, and their performance is directly related to the safety and reliability of automobile operation. Friction materials are the basic materials for manufacturing various clutch facings and brake linings. Existing friction materials are generally made of reinforcing materials, adhesives, friction performance modifiers and fillers through chemical and physical reactions. Usually, metals such as cadmium, hexavalent chromium, lead and mercury are used in friction materials, so that the friction coefficient of friction materials can be stabilized at about 0.4 at high temperatures of 300-400°C, with high friction coefficient and good high-temperature stability. However, in recent years, environmental protection has become more and more important at home and abroad, and the above metals have been listed as harmful metal components and their use has been restricted. The national standard limits the content of metal cadmium to less than 0.01%, and the content of hexavalent chromium, lead and mercury are all required to be less than 0.1%; and the above components are also restricted in friction materials exported to foreign countries; for example, the EU standard RoHS certification also stipulates that the cadmium content is less than 0.01%, and the content of hexavalent chromium, lead and mercury are all required to be less than 0.1%. Therefore, in order to adapt to domestic and international environmental protection standards, the composition of traditional friction materials has been improved. However, due to the lack of metal cadmium, chromium, etc., the friction coefficient of the material is low, and the friction coefficient is reduced to 0.36 at high temperatures, and the high-temperature stability is poor. Therefore, the existing friction material components are developed, and harmless components are used to make non-metallic friction materials, and the stability of the friction materials is improved. Summary of the invention
[0003] In view of the shortcomings of the prior art, the technical problem solved by the present invention is to provide a friction plate formula and a preparation method of a ternary composite non-metallic friction material, so as to solve the problem that the harmful components of the existing friction materials do not meet the export requirements.
[0004] In order to solve the above problems, the technical solution adopted by the present invention is: a friction plate formula of a ternary composite non-metallic friction material, which includes the following raw materials, by mass, 6-10 parts of phenolic resin, 8-12 parts of calcium sulfate whiskers, 6-10 parts of glass fiber, 10-14 parts of artificial graphite, 6-10 parts of barium sulfate, 2-5 parts of nitrile rubber powder, 2-5 parts of graphite, 0.5-1.5 parts of aramid pulp, 0.5-1.5 parts of polyacrylonitrile, 2-5 parts of petroleum coke, 1-3 parts of carbon black, 23-27 parts of aluminum oxide, and 4-7 parts of magnesium oxide.
[0005] Furthermore, the graphite is flake graphite.
[0006] A method for preparing a friction plate of a ternary composite non-metallic friction material comprises the following steps: S100: batching: weighing the ingredients according to the friction material formula, and packaging the ingredients according to pre-treated materials, non-pre-treated materials and glass fiber materials; S200: raw material pre-treatment: spreading the pre-treated raw materials flat and placing them in a drying chamber for drying; S300: mixing: firstly adding non-pre-treated materials into a mixer for blending; then adding pre-treated materials for blending, and finally adding glass fiber materials; S400: placing the uniformly mixed raw materials into a mold for pressing and forming; S500: heat treatment: placing the formed sheets into an electric oven for baking treatment, cooling after baking and checking whether there are cracks or bubbles on the surface of the sheets; S700: vulcanization: placing the heat-treated sheets into a flat vulcanizer for vulcanization treatment; S800: grinding the sheets to the required size.
[0007] Furthermore, in the step S300, the pressing temperature of the mold is 160-170° C., the hot pressing pressure is 70-90T, and the holding time is 10-15min.
[0008] Furthermore, during the drying in step S200, the drying temperature is 120-130° C. and the drying time is 24-36 hours.
[0009] Furthermore, in step S300, the pretreated material is added and mixed for 15-20 minutes, then the non-pretreated material is added and mixed for 35-40 minutes, and finally the glass fiber material is added and mixed for 3-5 minutes.
[0010] The beneficial effects of this solution are: using phenolic resin as the matrix, aramid pulp, polyacrylonitrile and glass fiber as the main reinforcing materials, calcined alumina as the friction-increasing material, flake graphite as the friction-reducing material, and adding a certain proportion of calcium sulfate whiskers and barium sulfate as fillers. Thus, harmful elements such as hexavalent chromium, lead and mercury are no longer used in the formulation of friction materials, the materials used are environmentally friendly and pollution-free, and the performance is better than traditional products, with obvious economic and environmental benefits.
[0011] By adding aramid pulp, polyacrylonitrile and glass fiber to form a random support system to disperse directional stress, and at the same time, a variety of organic and inorganic materials work together to not only improve the toughness of the material, but also obtain excellent friction and wear properties, and also help eliminate brake noise and thermal decay, and increase the service life of the product. After testing, the friction coefficient of the friction material of this scheme is 0.391 at room temperature, 0.397 at high temperature, and the wear rate is 0.0041. The friction coefficient can still be stable at about 0.39 at a high temperature above 300°C; although the friction coefficient of existing non-metallic friction materials can be maintained at about 0.4 at room temperature, the friction coefficient at 300°C drops sharply to about 0.36, a decrease of 10%, and a large change; while the difference between the friction coefficient at room temperature and the high temperature friction coefficient of this scheme is only 0.006, a change of 1.5%, which is 0.15 times the change of existing products, with extremely small changes and stable performance, and the high temperature friction coefficient of this scheme is 8% higher than that of existing products. This scheme has excellent friction performance, wear resistance and high temperature stability without adding harmful metals. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 The process flow chart of the preparation method of the present invention is as follows;
[0013] Figure 2 This is a curve chart of friction coefficient test data;
[0014] Figure 3 This is the test data curve of regrinding decay friction coefficient;
[0015] Figure 4 It is the compression performance test curve diagram;
[0016] Figure 5 This is the tensile properties test curve. DETAILED DESCRIPTION
[0017] The following is further described in detail through specific implementation methods:
[0018] Example 1, a friction plate formula of a ternary composite non-metallic friction material, including the following raw materials, by mass, 8 parts of phenolic resin, 10 parts of calcium sulfate whiskers, 8 parts of glass fiber, 12 parts of artificial graphite, 8 parts of barium sulfate, 3 parts of nitrile rubber powder, 3 parts of flake graphite, 1 part of aramid pulp, 1 part of polyacrylonitrile, 3 parts of petroleum coke, 2 parts of carbon black, 25 parts of aluminum oxide, and 6 parts of magnesium oxide.
[0019] A method for preparing a friction plate of a ternary composite non-metallic friction material comprises the following steps;
[0020] S100: batching; weighing raw materials according to the above friction material formula, and packaging the ingredients according to pre-treated materials, non-pre-treated materials and glass fiber materials; wherein the pre-treated materials include calcium sulfate whiskers, barium sulfate, aluminum oxide, and magnesium oxide; the non-pre-treated materials include phenolic resin, artificial graphite, nitrile rubber powder, flake graphite, aramid pulp, polyacrylonitrile, petroleum coke, and carbon black; and the glass fiber materials include glass fibers;
[0021] S200: Raw material pretreatment; the pretreated material is spread flat in a drying chamber for drying; the drying temperature is 125°C and the drying time is 30h;
[0022] S300: Mixing; first add non-pretreated materials into the mixer for blending; then add pretreated materials for blending, and finally add glass fiber; the mixing time is 55-65, and the stirring speed is 400 rpm;
[0023] S400: putting the uniformly mixed raw materials into a mold for pressing; during pressing, the pressing temperature of the mold is 165°C, the hot pressing pressure is 80T, and the holding time is 12 minutes.
[0024] S500: Heat treatment: Place the formed pieces into an electric oven for baking. The gap between each piece should be no less than 10mm. The oven temperature is heated and kept warm according to the set parameters. The heat treatment time is carried out according to the set parameters. After the heat treatment is completed, cool it down and check whether there are cracks or bubbles on the surface of the piece. By controlling the gap between the pieces during heat treatment, air circulation is facilitated to ensure the heat treatment effect.
[0025] Heat treatment temperature parameters are as follows:
[0026]
[0027] S700: Grind the sheet to the required size.
[0028] According to the standard SAE J661-2012, the samples were inspected and the friction coefficients of the samples were tested at room temperature and high temperature. After testing, the friction coefficient of the friction plate at room temperature was 0.391, the friction coefficient at high temperature was 0.397, and the wear rate was 0.0041. The friction coefficient between room temperature and high temperature changes little, and the friction performance of the friction plate has a high stability.
[0029] According to the standard SAE J661-2012, 100 pieces of sample were tested for friction coefficient. The friction coefficient test table was drawn by sampling equidistantly from 100 sample data at 10 intervals. The friction coefficient test table is as follows: Figure 3 The selected friction data are shown in the following table;
[0030] Table 1 Friction coefficient test data table
[0031] Sample No. Friction force (N) Friction coefficient μ 1 275 0.416 10 256 0.391 20 280 0.42 30 278 0.423 40 280 0.426 50 247 0.384 60 259 0.405 70 278 0.419 80 253 0.393 90 258 0.397 100 257 0.397
[0032] According to the standard SAE J661-2012, 8 samples were tested. When the samples were worn again, the friction coefficient changed as the temperature gradually increased. The test data results are shown in the following table, and the data are plotted as a change curve as shown in the following table. Figure 3 .
[0033] Table 2 Regrinding decay friction coefficient test data table
[0034]
[0035]
[0036] From the above data and Figure 3 It can be seen that in the process of gradually increasing temperature, the friction coefficient change curve of the friction plate is relatively gentle, indicating that the friction performance of the friction plate is stable and changes little at high temperatures; thus, during emergency braking of the vehicle, when friction generates high temperature, the friction plate will not cause a decrease in friction performance due to the high temperature, thus ensuring stable braking.
[0037] The similarities between Example 2 and Example 1 are not repeated here. The difference lies in that: in the friction plate formula of a ternary composite non-metallic friction material, phenolic resin is 9 parts, calcium sulfate whisker is 9 parts, glass fiber is 9 parts, and artificial graphite is 11 parts.
[0038] The similarities between Example 3 and Example 1 are not repeated here. The difference between them is that: in the friction plate formula of a ternary composite non-metallic friction material, calcium sulfate whiskers are 9 parts and barium sulfate is 9 parts.
[0039] The similarities between Example 4 and Example 1 are not repeated here, and the difference lies in: 26 parts of aluminum oxide and 5 parts of magnesium oxide.
[0040] The similarities between Example 5 and Example 1 are not repeated here, and the difference lies in: 0.8 parts of aramid pulp and 1.2 parts of polyacrylonitrile.
[0041] The friction materials prepared in Examples 1-5 were subjected to compression performance tests according to the national standard GB / T1041-2008. The test result curves are shown in FIG. Figure 4 The test results are shown in the following table;
[0042] Table 3 Compression performance test results of the embodiment
[0043]
[0044] The friction materials prepared in Examples 1-5 were tested for tensile strength according to the national standard GB / T1040-2006. The test result curves are shown in FIG. Figure 5 The test results are shown in the following table;
[0045] Table 4 Example tensile properties test results
[0046]
[0047]
[0048] It can be seen from the above test experiments that the average tensile strength of the friction material of this solution reaches 28.04 MPa, and the average compressive strength reaches 143.96 MPa.
[0049] The friction material of the existing formula is used as a comparative example for comparison and explanation, and the comparative example is as follows;
[0050] The comparative friction material, by mass, includes the following raw materials: 20 parts of phenolic resin, 5 parts of nitrile rubber powder, 12 parts of glass fiber, 3 parts of flake graphite, 15 parts of wollastonite, 8 parts of alumina, 8 parts of artificial graphite, 14 parts of kaolin, 5 parts of polyacrylonitrile, 5 parts of friction powder, and 5 parts of silicon carbide. Five samples of the comparative example were randomly selected and tested for compression and tensile properties according to the national standard GB / T1041-2008 and the national standard GB / T1040-2006.
[0051] The test results are shown in Table 5 and Table 6;
[0052] Table 5 Comparative Examples Compression Performance Test Results
[0053]
[0054] Table 6 Comparative Example Tensile Properties Test Results
[0055]
[0056]
[0057] The above experiments show that the average tensile strength of the friction material is 17.79MPa, and the average compressive strength is 84.11MPa, which are much lower than the average tensile strength of 28.04MPa and the average compressive strength of 143.96MPa of the present solution. The tensile strength of the present solution is 1.5 times that of the comparative example, and the compressive strength is 1.7 times that of the comparative example. The friction material prepared by the present solution has excellent performance.
[0058] Eight samples of the comparative example were selected and tested according to the standard SAE J661-2012. When the samples were worn again, the friction coefficient changed as the temperature gradually increased. The test data results are shown in the following table.
[0059] Table 5 Comparative Example Regrinding Decline Friction Coefficient Test Data Table
[0060] Sample No. Friction force (N) Friction coefficient μ Temperature.(℃) 1 269 0.411 122 2 278 0.418 150 3 291 0.429 178 4 293 0.44 206 5 287 0.430 234 6 283 0.421 262 7 269 0.401 290 8 244 0.368 318
[0061] From the experimental results in Table 5, it can be seen that although the friction material of the comparative example can maintain a friction coefficient of more than 0.4 at a high temperature below 300°C, the friction coefficient drops sharply to about 0.36 at a high temperature above 300°C, a decrease of 10%, and a large change; the stability performance at high temperature is poor. However, the friction material of the present solution can still maintain a friction coefficient of about 0.39 at a high temperature above 300°C, and has good stability performance.
[0062] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several deformations and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.
Claims
1. A friction plate formula of a ternary composite non-metallic friction material, characterized by: The invention comprises the following raw materials, by mass: 6-10 parts of phenolic resin, 8-12 parts of calcium sulfate whiskers, 6-10 parts of glass fibers, 10-14 parts of artificial graphite, 6-10 parts of barium sulfate, 2-5 parts of nitrile rubber powder, 2-5 parts of graphite, 0.5-1.5 parts of aramid pulp, 0.5-1.5 parts of polyacrylonitrile, 2-5 parts of petroleum coke, 1-3 parts of carbon black, 23-27 parts of aluminum oxide and 4-7 parts of magnesium oxide.
2. The friction plate formula of the ternary composite non-metallic friction material according to claim 1 is characterized by: The graphite is flake graphite.
3. A method for preparing a friction plate of a ternary composite non-metallic friction material, characterized in that: The following steps are included: S100: batching; weighing raw materials according to the friction material formula, and packaging the ingredients according to pre-treated materials, non-pre-treated materials and glass fiber materials; S200: Raw material pretreatment; Spread the pretreated material flat into the drying chamber for drying; S300: Mixing: firstly, adding pre-treated materials into the mixer for blending; then adding non-pre-treated materials for blending, and finally adding glass fiber; S400: putting the evenly mixed raw materials into a mold for pressing and forming; S500: Heat treatment: put the formed sheets into an electric oven for baking. After baking, cool them down and check whether there are cracks or bubbles on the surface of the sheets. S600: Grind the sheet to the required size.
4. The method for preparing a friction plate of a ternary composite non-metallic friction material according to claim 3, characterized in that: In the step S300, the pressing temperature of the mold is 160-170° C., the hot pressing pressure is 70-90° C., and the holding time is 10-15 min.
5. The method for preparing a friction plate of a ternary composite non-metallic friction material according to claim 3, characterized in that: During the drying in step S200, the drying temperature is 120-130° C. and the drying time is 24-36 hours.
6. The method for preparing a friction plate of a ternary composite non-metallic friction material according to claim 3, characterized in that: In the step S300, the pre-treated material is added and mixed for 15-20 minutes, then the non-pre-treated material is added and mixed for 35-40 minutes, and finally the glass fiber material is added and mixed for 3-5 minutes.
Citation Information
Cited By
Preparation method of acrylic pulp and aramid hybrid reinforced friction material
CN122103804A