A high temperature resistant cable
By adding modified melamine resin microspheres and other materials to the outer cover of the cable, the problem of insufficient safety of existing cables in high temperature environments is solved, and the heat resistance and flame retardant performance of the cable are significantly improved. Enhanced its safety and reliability.
Patent Information
- Application Number
- CN202411340670.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-25
AI Technical Summary
The existing commercial cables cannot meet the safe operation needs of power and signal in high temperature environments, and they produce harmful smoke during fires, posing a threat to human health.
Modified melamine resin microspheres are added to the outer cover of the cable, combined with methylvinyl silicone rubber, acrylate rubber and ultra-high molecular weight polyethylene and other materials, and a high temperature-resistant outer cover is prepared through specific process steps. Enhance the tensile strength, heat resistance and wear resistance of the cable.
It significantly improves the tensile strength, heat resistance and wear resistance of the cable, enhances safety and reliability, improves the anti-aging and corrosion resistance, and inhibits the generation of combustible small molecules under high temperature conditions, significantly improving Flame retardant and fire-resistant properties.
Smart Images

Figure CN118866439B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of cables, and in particular relates to a high temperature resistant cable. Background Art
[0002] Cables are a collection of wires used to transmit electrical energy, signals or data. They can be single wires or cables composed of multiple wires. There are many types of cables, which can be divided into different types according to their uses and characteristics, such as power cables, communication cables, optical cables, coaxial cables, etc. Some special industries such as petrochemicals, steel, aerospace, shipbuilding, military industry, pharmaceuticals, food, plastic machinery, boilers, etc., which are related to heat and high temperature, all require cables that can withstand high temperatures. These cables are usually made of conventional materials and have a rich source of sources, so they are easy to produce on a large scale and the cost is relatively low. However, general commercially available cables cannot meet the requirements of high temperature resistance and cannot guarantee the safe operation of power and signals.
[0003] With the advancement of the power industry, the demand for cables has increased dramatically. This growth has brought higher standards for cable safety. This is because when a fire occurs in electrical equipment, it is not only difficult to extinguish it quickly, but the organic materials used in cables will produce a large amount of harmful smoke during the combustion process, posing a serious threat to human health. Therefore, it is extremely important to study cables that are resistant to high temperatures and flame retardant. Summary of the invention
[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention improves the tensile strength, heat resistance and wear resistance of the cable by adding modified melamine resin microspheres into the outer sheath of the cable, thereby enhancing the safety and reliability of the cable.
[0005] In order to achieve the above-mentioned purpose, the following technical scheme is adopted: The present invention provides a high-temperature resistant cable, comprising: four mutually conflicting wire cores, an inner sheath wrapped around the outside of the wire cores, an armor layer wrapped around the outside of the inner sheath, and an outer sheath wrapped around the outside of the armor layer, wherein the outer sheath is obtained by extruding a high-temperature resistant material.
[0006] Furthermore, the high temperature resistant material comprises the following components in parts by weight: 30-40 parts of methyl vinyl silicone rubber, 20-25 parts of acrylate rubber, 15-20 parts of ultra-high molecular weight polyethylene, 5-15 parts of modified melamine resin microspheres, 0.1-5 parts of vulcanizing agent, 0.1-0.5 parts of antioxidant and 0.05-0.2 parts of stabilizer.
[0007] Furthermore, the modified melamine resin microspheres are prepared by the following steps:
[0008] S1. Dispersing (acetoxyethyl) heptamethylcyclotetrasiloxane in N-methylpyrrolidone, adding 3-thiopheneboronic acid methyliminodiacetate, reacting at 60-80° C. for 6-8 hours, then pouring the reaction solution into water, centrifuging to separate the solid, washing it three times with deionized water and ethanol, and vacuum drying it at 80-110° C. for 6-12 hours to obtain modified (acetoxyethyl) heptamethylcyclotetrasiloxane;
[0009] S2. Mix triglycidyl isocyanurate, hexahydroxymethyl melamine and deionized water, adjust the pH value of the solution to 10-12 with 2 mol / L NaOH solution, add dibenzoyl peroxide to react for 0.5-1h, then add modified (acetoxyethyl) heptamethylcyclotetrasiloxane, tetracyclyl-4,4'-diaminodiphenylmethane and silane coupling agent, add formic acid, continue to react for 1-2h, then separate the solid by centrifugation, wash it three times with deionized water and ethanol, and then dry it at 60-90°C under vacuum for 6-12h to obtain the modified melamine resin microspheres.
[0010] Furthermore, in step S1, the mass ratio of (acetoxyethyl) heptamethylcyclotetrasiloxane, N-methylpyrrolidone, and 3-thiopheneboronic acid methyliminodiacetate is 1:40-60:0.5-1.5.
[0011] Furthermore, in step S2, the mass ratio of triglycidyl isocyanurate, hexamethylolmelamine, deionized water, dibenzoyl peroxide, modified (acetoxyethyl) heptamethylcyclotetrasiloxane, tetraepoxypropyl-4,4'-diaminodiphenylmethane, silane coupling agent, and formic acid is 1:2-5:80-150:0.015-0.1:4.5-8:0.5-3:2.2-4.8:42-65.
[0012] Furthermore, the silane coupling agent is one or more of KH-550, KH-560, KH-570, KH-602 and KH-901.
[0013] Furthermore, the vulcanizing agent is one or more of tetramethylthiuram disulfide, diisobutylthiuram disulfide, tetramethylthiuram monosulfide, tetrabenzylthiuram disulfide and dipentamethylenethiuram hexasulfide.
[0014] Furthermore, the antioxidant is one or more of antioxidant 1010 , antioxidant 1076 , antioxidant 2246 and antioxidant 264 .
[0015] Furthermore, the stabilizer is one of light stabilizer 783, light stabilizer 770, light stabilizer 622 and light stabilizer 944.
[0016] Furthermore, the outer protective layer is prepared by the following steps: methyl vinyl silicone rubber, acrylate rubber and ultra-high molecular weight polyethylene are mixed in a mixer at 160-200°C for 50-80 minutes, cooled to 80-100°C, the modified melamine resin microspheres, vulcanizer, antioxidant and stabilizer are added, mixed evenly and then extruded on the outside of the armor layer to obtain the outer protective layer.
[0017] Furthermore, the wire core includes: a conductor obtained by twisting multiple copper wires, a fireproof layer coated on the outside of the conductor, an insulating layer coated on the outside of the fireproof layer, a shielding layer coated on the outside of the insulating layer, and a filling layer arranged between the shielding layer and the inner sheath.
[0018] Furthermore, the fireproof layer is a ceramic silicone rubber belt; the insulating layer is extruded from a polyimide resin; the shielding layer is extruded from an EVA6110M resin; the filling layer is extruded from a polypropylene resin; the inner protective layer is extruded from an ECTFE resin; and the armor layer is galvanized steel belt armor.
[0019] The beneficial effects of the present invention are:
[0020] (1) The present invention significantly improves the tensile strength, heat resistance and wear resistance of the cable and enhances the safety and reliability of the cable by adding modified melamine resin microspheres prepared from (acetoxyethyl) heptamethylcyclotetrasiloxane, 3-thiopheneboronic acid methyliminodiacetate, tetraepoxypropyl-4,4'-diaminodiphenylmethane and the like into the cable outer sheath. In the preparation process, the use of triglycidyl cyanurate improves the fluidity and formability of the modified melamine resin microspheres, making them more compatible with the matrix material, so that they are evenly dispersed in the cable outer sheath, effectively improving the impact resistance of the cable.
[0021] (2) The macrocyclic ring and rigid structure of (acetoxyethyl) heptamethylcyclotetrasiloxane create a stable chemical environment in the material, which not only enhances the chemical stability of the cable, but also improves its anti-aging and corrosion resistance. By modifying (acetoxyethyl) heptamethylcyclotetrasiloxane with 3-thiopheneboronic acid methyliminodiacetate, silicon, boron and sulfur elements are introduced into the modified melamine resin microspheres, which not only improves the wear resistance of the cable, but also enhances its UV resistance, thermal stability, flame retardancy and overall mechanical properties.
[0022] (3) The addition of tetracyclyl-4,4'-diaminodiphenylmethane and the modified 3-thiopheneboronic acid methyliminodiacetate synergistically promote the cross-linking reaction within the material. The epoxy group contained in tetracyclyl-4,4'-diaminodiphenylmethane facilitates the coupling of the modified material with the melamine resin and other matrix materials through a coupling agent, thereby forming a more compact and stable three-dimensional network structure and improving the overall mechanical properties of the material.
[0023] (4) Under high temperature conditions, the oxidative decomposition of the siloxane structure will generate nano-silicon dioxide, which will combine with the matrix carbon layer to form a stable and dense barrier layer. At the same time, the thiophene group and the boric acid group can promote the carbonization of the polymer at high temperature and effectively capture the combustible small molecules produced by the thermal decomposition of the polymer, thereby inhibiting the thermal decomposition of the polymer and reducing the generation of combustible small molecules. These mechanisms work together to improve the smoke suppression and anti-drip performance of the cable outer sheath, and further enhance the flame retardant and fire resistant properties of the cable. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic structural diagram of a high temperature resistant cable according to the present invention;
[0025] Figure 2 The mechanical strength test results of the cable outer sheath materials of various embodiments and comparative examples of the present invention are shown;
[0026] Figure 3 is the tensile strength retention rate of the cable outer sheath material of each embodiment of the present invention and the comparative example after aging for 30 days;
[0027] Figure 4 The wear rate test results of the cable outer sheath materials of various embodiments and comparative examples of the present invention are shown;
[0028] Figure 5 The limiting oxygen index test results of the cable outer sheath materials of various embodiments and comparative examples of the present invention;
[0029] Figure 6 The carbon residue SEM images of the cable outer sheath materials of Example 3 and Comparative Examples 1-3 after the limiting oxygen index measurement, wherein (a) is Example 3, (b) is Comparative Example 1, (c) is Comparative Example 2, and (d) is Comparative Example 3.
[0030] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention.
[0031] In the figure: 1. wire core; 11. conductor; 12. fireproof layer; 13. insulation layer; 14. shielding layer; 15. filling layer; 2. inner sheath; 3. armor layer; 4. outer sheath. DETAILED DESCRIPTION
[0032] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0033] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0034] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified. Example 1
[0035] A high temperature resistant cable
[0036] According to the attached Figure 1 As shown, the cable includes: four mutually conflicting cores 1, an inner sheath 2 coated on the outside of the core 1, an armor layer 3 coated on the outside of the inner sheath 2 and an outer sheath 4 coated on the outside of the armor layer 3, the outer sheath 4 is extruded from a high temperature resistant material, the core 1 includes: a conductor 11 obtained by twisting multiple copper wires, a fireproof layer 12 coated on the outside of the conductor 11, an insulating layer 13 coated on the outside of the fireproof layer 12, a shielding layer 14 coated on the outside of the insulating layer 13 and a filling layer 15 arranged between the shielding layer 14 and the inner sheath 2; the fireproof layer 12 is a ceramic silicone rubber belt; the insulating layer 13 is extruded from a polyimide resin; the shielding layer 14 is extruded from an EVA6110M resin; the filling layer 15 is extruded from a polypropylene resin; the inner sheath 2 is extruded from an ECTFE resin; the armor layer 3 is a galvanized steel belt armor.
[0037] The high temperature resistant material comprises the following components in parts by weight: 30 parts of methyl vinyl silicone rubber, 20 parts of acrylate rubber, 15 parts of ultra-high molecular weight polyethylene, 5 parts of modified melamine resin microspheres, 0.1 parts of vulcanizing agent, 0.1 parts of antioxidant and 0.05 parts of stabilizer.
[0038] The modified melamine resin microspheres are prepared by the following steps:
[0039] S1. Dispersing (acetoxyethyl) heptamethylcyclotetrasiloxane in N-methylpyrrolidone, adding 3-thiopheneboronic acid methyliminodiacetate, reacting at 60° C. for 6 h, then pouring the reaction solution into water, centrifuging to separate the solid, washing it three times with deionized water and ethanol, and vacuum drying it at 80° C. for 6 h to obtain modified (acetoxyethyl) heptamethylcyclotetrasiloxane;
[0040] S2. Mix triglycidyl isocyanurate, hexahydroxymethyl melamine and deionized water, adjust the pH of the solution to 10 with 2 mol / L NaOH solution, add dibenzoyl peroxide to react for 0.5 h, then add modified (acetoxyethyl) heptamethylcyclotetrasiloxane, tetracyclyl-4,4'-diaminodiphenylmethane and silane coupling agent, add formic acid, continue to react for 1 h, then centrifuge to separate the solid, wash it three times with deionized water and ethanol, and then dry it at 60°C in vacuum for 6 h to obtain the modified melamine resin microspheres.
[0041] In the step S1, the mass ratio of (acetoxyethyl) heptamethylcyclotetrasiloxane, N-methylpyrrolidone, and 3-thiopheneboronic acid methyliminodiacetate is 1:40:0.5.
[0042] In the step S2, the mass ratio of triglycidyl isocyanurate, hexahydroxymethyl melamine, deionized water, dibenzoyl peroxide, modified (acetoxyethyl) heptamethylcyclotetrasiloxane, tetraepoxypropyl-4,4'-diaminodiphenylmethane, silane coupling agent, and formic acid is 1:2:80:0.015:4.5:0.5:2.2:42.
[0043] The silane coupling agent is KH-550, KH-560, and KH-570 combined in a mass ratio of 4:1:3; the vulcanizing agent is tetramethylthiuram disulfide; the antioxidant is antioxidant 1010; and the stabilizer is light stabilizer 783.
[0044] The outer protective layer is prepared by the following steps: methyl vinyl silicone rubber, acrylate rubber and ultra-high molecular weight polyethylene are mixed in a mixer at 160° C. for 50 minutes, cooled to 80° C., the modified melamine resin microspheres, vulcanizer, antioxidant and stabilizer are added, mixed evenly and then extruded outside the armor layer to obtain the outer protective layer. Example 2
[0045] A high temperature resistant cable
[0046] The structure of the cable is the same as that of Embodiment 1.
[0047] The high temperature resistant material comprises the following components in parts by weight: 40 parts of methyl vinyl silicone rubber, 25 parts of acrylate rubber, 20 parts of ultra-high molecular weight polyethylene, 15 parts of modified melamine resin microspheres, 5 parts of vulcanizing agent, 0.5 parts of antioxidant and 0.2 parts of stabilizer.
[0048] The modified melamine resin microspheres are prepared by the following steps:
[0049] S1. Disperse (acetoxyethyl) heptamethylcyclotetrasiloxane in N-methylpyrrolidone, add 3-thiopheneboronic acid methyliminodiacetate, react at 80° C. for 8 h, then pour the reaction solution into water, separate the solid by centrifugation, wash three times with deionized water and ethanol, and then vacuum dry at 110° C. for 12 h to obtain modified (acetoxyethyl) heptamethylcyclotetrasiloxane;
[0050] S2. Mix triglycidyl isocyanurate, hexahydroxymethyl melamine and deionized water, adjust the pH of the solution to 12 with 2 mol / L NaOH solution, add dibenzoyl peroxide to react for 1 hour, then add modified (acetoxyethyl) heptamethylcyclotetrasiloxane, tetracyclyl-4,4'-diaminodiphenylmethane and silane coupling agent, add formic acid, continue to react for 2 hours, then centrifuge to separate the solid, wash it three times with deionized water and ethanol, and then dry it at 90°C in vacuum for 12 hours to obtain the modified melamine resin microspheres.
[0051] In the step S1, the mass ratio of (acetoxyethyl) heptamethylcyclotetrasiloxane, N-methylpyrrolidone, and 3-thiopheneboronic acid methyliminodiacetate is 1:60:1.5.
[0052] In the step S2, the mass ratio of triglycidyl isocyanurate, hexahydroxymethyl melamine, deionized water, dibenzoyl peroxide, modified (acetoxyethyl) heptamethylcyclotetrasiloxane, tetraepoxypropyl-4,4'-diaminodiphenylmethane, silane coupling agent, and formic acid is 1:5:150:0.1:8:3:4.8:65.
[0053] The silane coupling agent is KH-550, KH-560, and KH-570 combined in a mass ratio of 4:1:3; the vulcanizing agent is tetramethylthiuram disulfide, diisobutylthiuram disulfide, and tetramethylthiuram monosulfide combined in a mass ratio of 2:1:1; the antioxidant is antioxidant 1010, antioxidant 1076, and antioxidant 264 combined in a mass ratio of 1.5:2:1; and the stabilizer is light stabilizer 770.
[0054] The outer protective layer is prepared by the following steps: methyl vinyl silicone rubber, acrylate rubber and ultra-high molecular weight polyethylene are mixed in a mixer at 200° C. for 80 minutes, cooled to 100° C., the modified melamine resin microspheres, vulcanizer, antioxidant and stabilizer are added, mixed evenly and then extruded outside the armor layer to obtain the outer protective layer. Example 3
[0055] A high temperature resistant cable
[0056] The structure of the cable is the same as that of embodiment 1.
[0057] The high temperature resistant material comprises the following components in parts by weight: 35 parts of methyl vinyl silicone rubber, 22 parts of acrylate rubber, 16 parts of ultra-high molecular weight polyethylene, 12 parts of modified melamine resin microspheres, 2.5 parts of vulcanizing agent, 0.2 parts of antioxidant and 0.15 parts of stabilizer.
[0058] The modified melamine resin microspheres are prepared by the following steps:
[0059] S1. Dispersing (acetoxyethyl) heptamethylcyclotetrasiloxane in N-methylpyrrolidone, adding 3-thiopheneboronic acid methyliminodiacetate, reacting at 70° C. for 6.5 h, then pouring the reaction solution into water, centrifuging to separate the solid, washing it three times with deionized water and ethanol, and vacuum drying it at 100° C. for 10 h to obtain modified (acetoxyethyl) heptamethylcyclotetrasiloxane;
[0060] S2. Mix triglycidyl isocyanurate, hexahydroxymethyl melamine and deionized water, adjust the pH of the solution to 11 with 2 mol / L NaOH solution, add dibenzoyl peroxide and react for 0.8 h, then add modified (acetoxyethyl) heptamethylcyclotetrasiloxane, tetracyclyl-4,4'-diaminodiphenylmethane and silane coupling agent, add formic acid, continue to react for 1.5 h, then centrifuge to separate the solid, wash it three times with deionized water and ethanol, and then dry it at 80°C in vacuum for 8 h to obtain the modified melamine resin microspheres.
[0061] In the step S1, the mass ratio of (acetoxyethyl) heptamethylcyclotetrasiloxane, N-methylpyrrolidone, and 3-thiopheneboronic acid methyliminodiacetate is 1:50:1.
[0062] In the step S2, the mass ratio of triglycidyl isocyanurate, hexahydroxymethyl melamine, deionized water, dibenzoyl peroxide, modified (acetoxyethyl) heptamethylcyclotetrasiloxane, tetraepoxypropyl-4,4'-diaminodiphenylmethane, silane coupling agent, and formic acid is 1:3:100:0.05:6:1.5:3.5:50.
[0063] The silane coupling agent is a combination of KH-550, KH-560, KH-570 and KH-901 in a mass ratio of 2:1:3:1; the vulcanizing agent is a combination of tetramethylthiuram monosulfide, tetrabenzylthiuram disulfide and dipentamethylthiuram hexasulfide in a mass ratio of 2:1:1; the antioxidant is a combination of antioxidant 1010, antioxidant 1076, antioxidant 2246 and antioxidant 264 in a mass ratio of 2:1:1:1; the stabilizer is a combination of light stabilizer 783, light stabilizer 770, light stabilizer 622 and light stabilizer 944 in a mass ratio of 2:1:1:2.
[0064] The outer protective layer is prepared by the following steps: methyl vinyl silicone rubber, acrylate rubber and ultra-high molecular weight polyethylene are mixed in a mixer at 180° C. for 60 minutes, cooled to 90° C., the modified melamine resin microspheres, vulcanizer, antioxidant and stabilizer are added, mixed evenly and then extruded outside the armor layer to obtain the outer protective layer.
[0065] Comparative Example 1
[0066] The difference between this comparative example and Example 3 is that modified (acetoxyethyl) heptamethylcyclotetrasiloxane is not added to the modified melamine resin microspheres, and the remaining components and preparation process are the same as those in Example 3.
[0067] Comparative Example 2
[0068] The difference between this comparative example and Example 3 is that tetracyclyl-4,4'-diaminodiphenylmethane is not added to the modified melamine resin microspheres, and the remaining components and preparation process are the same as those in Example 3.
[0069] Comparative Example 3
[0070] The difference between this comparative example and Example 3 is that the melamine resin microspheres are not modified, and the other components and the preparation process are the same as those of Example 3. The preparation process of the melamine resin microspheres is as follows: triglycidyl isocyanurate, hexahydroxymethylmelamine and deionized water are mixed, the pH value of the solution is adjusted to 11 with a 2 mol / L NaOH solution, dibenzoyl peroxide is added to react for 0.8 h, and then formic acid is added to continue the reaction for 1.5 h, and then the solid is separated by centrifugation, washed three times with deionized water and ethanol, and then dried in vacuum at 80° C. for 8 h to obtain the melamine resin microspheres.
[0071] Results Analysis
[0072] According to the standard of GB / T 2951-2008, the mechanical properties of the cable outer sheath materials of each embodiment of the present invention and the comparative example were tested, including tensile strength and elongation at break, the temperature was 25°C, the sample gauge length was 25mm, the width was 6mm, the shape was dumbbell-shaped, and the tensile speed was 200mm / min. The results are shown in Figure 2 .
[0073] Depend on Figure 2 It can be seen that the tensile strength and elongation at break of the cable outer sheath material prepared by the present invention are better than those of the comparative example, and have good mechanical properties, proving that modified (acetoxyethyl) heptamethylcyclotetrasiloxane, tetracyclyl-4,4'-diaminodiphenylmethane and the synergistic effect of the two all contribute to the mechanical properties of the material.
[0074] The cable outer sheath materials prepared in the embodiments of the present invention and the comparative examples were aged at 120°C for 30 days. The initial tensile strength and the tensile strength after aging for 30 days were measured according to the standard of GB / T 2951-2008, and the tensile strength retention rate was calculated. The results are shown in Figure 3 , tensile strength retention rate = tensile strength after aging for 30 days / initial tensile strength × 100%.
[0075] Depend on Figure 3 It can be seen that the cable outer sheath material prepared by the present invention has a high 30-day aging tensile strength retention rate, and the change rate of the tensile strength before and after aging in each embodiment is <5%, showing high heat resistance and high aging resistance.
[0076] According to the standard of GB / T3960-2016, the wear rate of the cable outer sheath material of each embodiment of the present invention and the comparative example was tested, and the results are shown in Figure 4 .
[0077] Depend on Figure 4 It can be seen that the wear rate of the cable outer sheath material prepared by the present invention is low, which proves that the wear resistance of the material is greatly improved by introducing silicon, boron and sulfur elements.
[0078] According to the standard of GB / T 2406.2-2009, the limiting oxygen index of the cable outer sheath material of each embodiment of the present invention and the comparative example was measured, and the sample size was 100mm×6.5mm×3mm. The results are shown in Figure 5 .
[0079] Depend on Figure 5 It can be seen that the cable outer sheath material prepared by the present invention has a low limiting oxygen index and exhibits excellent flame retardancy, which proves that the modified melamine resin microspheres are helpful to improve the flame retardancy of the material.
[0080] The carbon residue of the cable outer sheath material of Example 3 and Comparative Examples 1-3 after the limiting oxygen index measurement was observed by scanning electron microscope. The SEM images are shown in FIG. Figure 6 , wherein (a) is Example 3, (b) is Comparative Example 1, (c) is Comparative Example 2, and (d) is Comparative Example 3.
[0081] Depend on Figure 6It can be seen that the cable outer sheath materials of each comparative example all have pores and cracks to varying degrees after burning, while the cable outer sheath material of Example 3 of the present invention forms a dense carbon layer after burning, indicating that the cable outer sheath material prepared by the present invention can quickly promote the carbonization of the polymer at high temperature to form a stable and dense barrier layer, thereby improving the smoke suppression and anti-dripping properties of the cable outer sheath, thereby reducing the fire risk and making the cable have high temperature resistance and flame retardant and fire resistant properties.
[0082] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0083] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A high temperature resistant cable, characterized in that: include: Four mutually conflicting wire cores (1), an inner sheath (2) coated on the outside of the wire core, an armor layer (3) coated on the outside of the inner sheath (2), and an outer sheath (4) coated on the outside of the armor layer (3), wherein the outer sheath (4) is obtained by extrusion of a high temperature resistant material; the high temperature resistant material comprises the following components in parts by weight: 30-40 parts of methyl vinyl silicone rubber, 20-25 parts of acrylic rubber, 15-20 parts of ultra-high molecular weight polyethylene, 5-15 parts of modified melamine resin microspheres, 0.1-5 parts of a vulcanizing agent, 0.1-0.5 parts of an anti-aging agent, and 0.05-0.2 parts of a stabilizer; The modified melamine resin microspheres are prepared by the following steps: S1. Dispersing (acetoxyethyl) heptamethylcyclotetrasiloxane in N-methylpyrrolidone, adding 3-thiopheneboronic acid methyliminodiacetate, reacting at 60-80° C. for 6-8 hours, then pouring the reaction solution into water, centrifuging to separate the solid, washing it three times with deionized water and ethanol, and vacuum drying it at 80-110° C. for 6-12 hours to obtain modified (acetoxyethyl) heptamethylcyclotetrasiloxane; S2. Mix triglycidyl isocyanurate, hexahydroxymethyl melamine and deionized water, adjust the pH value of the solution to 10-12 with 2 mol / L NaOH solution, add dibenzoyl peroxide to react for 0.5-1h, then add modified (acetoxyethyl) heptamethylcyclotetrasiloxane, tetracyclyl-4,4'-diaminodiphenylmethane and silane coupling agent, add formic acid, continue to react for 1-2h, then centrifuge to separate the solid, wash it three times with deionized water and ethanol, and vacuum dry it at 60-90°C for 6-12h to obtain the modified melamine resin microspheres.
2. A high temperature resistant cable according to claim 1, characterized in that: In the step S1, the mass ratio of (acetoxyethyl) heptamethylcyclotetrasiloxane, N-methylpyrrolidone, and 3-thiopheneboronic acid methyliminodiacetate is 1:40-60:0.5-1.
5.
3. A high temperature resistant cable according to claim 2, characterized in that: In the step S2, the mass ratio of triglycidyl isocyanurate, hexamethylolmelamine, deionized water, dibenzoyl peroxide, modified (acetoxyethyl) heptamethylcyclotetrasiloxane, tetraepoxypropyl-4,4'-diaminodiphenylmethane, silane coupling agent and formic acid is 1:2-5:80-150:0.015-0.1:4.5-8:0.5-3:2.2-4.8:42-65.
4. A high temperature resistant cable according to claim 3, characterized in that: The silane coupling agent is one or more of KH-550, KH-560, KH-570, KH-602 and KH-901.
5. A high temperature resistant cable according to claim 4, characterized in that: The vulcanizing agent is one or more of tetramethylthiuram disulfide, diisobutylthiuram disulfide, tetramethylthiuram monosulfide, tetrabenzylthiuram disulfide and dipentamethylenethiuram hexasulfide.
6. A high temperature resistant cable according to claim 5, characterized in that: The antioxidant is one or more of antioxidant 1010 , antioxidant 1076 , antioxidant 2246 and antioxidant 264 .
7. A high temperature resistant cable according to claim 6, characterized in that: The stabilizer is one of light stabilizer 783, light stabilizer 770, light stabilizer 622 and light stabilizer 944.
8. A high temperature resistant cable according to claim 7, characterized in that: The outer protective layer (4) is prepared by the following steps: methyl vinyl silicone rubber, acrylate rubber and ultra-high molecular weight polyethylene are mixed in a mixer at 160-200° C. for 50-80 minutes, the temperature is reduced to 80-100° C., the modified melamine resin microspheres, vulcanizing agent, antioxidant and stabilizer are added, mixed evenly and then extruded onto the outside of the armor layer (3) to obtain the outer protective layer (4).
9. A high temperature resistant cable according to claim 8, characterized in that: The wire core (1) comprises: a conductor (11) obtained by twisting a plurality of copper wires, a fireproof layer (12) coated on the outside of the conductor (11), an insulating layer (13) coated on the outside of the fireproof layer (12), a shielding layer (14) coated on the outside of the insulating layer (13), and a filling layer (15) arranged between the shielding layer (14) and the inner sheath (2).
10. A high temperature resistant cable according to claim 9, characterized in that: The fireproof layer (12) is a ceramic silicone rubber tape; the insulating layer (13) is obtained by extruding a polyimide resin; the shielding layer (14) is obtained by extruding an EVA6110M resin; the filling layer (15) is obtained by extruding a polypropylene resin; the inner protective layer (2) is obtained by extruding an ECTFE resin; and the armor layer (3) is a galvanized steel belt armor.
Citation Information
Patent Citations
Insulating fireproof coating for electric wires
CN105647261A
Low-smoke halogen-free flame-retardant cable for urban rail transit and preparation method of low-smoke halogen-free flame-retardant cable
CN114446535A
High-temperature insulating adhesive film material and preparation method therefor
WO2021046722A1
Ultra-soft b1-level low-smoke halogen-free flame-retardant sheath material and preparation method therefor