Preparation method and application of lithium metal negative electrode bismuth / fluorine / nitrogen hybrid composite protection layer

By forming a bismuth/fluorine/nitrogen hybrid composite protective layer on the surface of the lithium metal anode, the existing technology problems of lithium dendrite growth and lithium volume expansion under high current density and large area capacity are solved, achieving high cycle stability and The effect of low capacity attenuation has commercial application potential.

CN118867142AActive Publication Date: 2024-10-29HEFEI UNIV OF TECH

Patent Information

Application Number
CN202410893219.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-29
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

The existing artificial protective layer of lithium metal anode is difficult to effectively inhibit the growth of lithium dendrites and lithium volume expansion under conditions of high current density and large area capacity, resulting in poor battery cycle stability and problems such as solvent residue.

Method used

A method is used to prepare the bismuth/fluorine/nitrogen hybrid composite protective layer of the lithium metal negative electrode by magnetically stirring bismuth trifluoromethanesulfonate and lithium nitrate in an organic solvent until they are completely dissolved, and then adding them dropwise on the surface of the lithium sheet and allowing them to stand still. Leave it until the solvent evaporates to form a bismuth/fluorine/nitrogen hybrid composite protective layer, which is rich in Bi, Li3Bi, -CF3, LiF, and LixNOy components and provides ionic conductivity, mechanical strength, and electrochemical stability.

Benefits of technology

This protective layer effectively inhibits the growth of lithium dendrites and lithium volume expansion under conditions of high current density and large area capacity, significantly improves the cycle stability of the lithium metal anode, extends the service life of the battery, and reduces capacity fading, with Commercial application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118867142A_ABST
    Figure CN118867142A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a bismuth / fluorine / nitrogen hybrid composite protective layer of a lithium metal negative electrode, and the preparation method comprises the following steps: mixing and stirring bismuth trifluoromethanesulfonate and lithium nitrate in an organic solvent until the bismuth trifluoromethanesulfonate and the lithium nitrate are completely dissolved, and then dropwise adding the obtained reaction solution to the surface of a lithium sheet, namely generating the bismuth / fluorine / nitrogen hybrid composite protective layer on the surface of the lithium sheet in situ. The obtained composite protective layer is rich in Bi, Li3Bi,-CF3, LiF and LixNOy components, under the synergistic effect of all the components, the protective layer which is ionic conductive, high in mechanical strength and stable in electrochemistry is successfully constructed, the protective layer can adapt to the working conditions of large current density and large-area capacity, and growth of lithium dendrites and the lithium volume expansion effect are effectively restrained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium metal batteries, and specifically relates to a preparation method and application of a bismuth / fluorine / nitrogen hybridized composite protective layer for a lithium metal negative electrode. Background Art

[0002] With the rapid development of consumer electronics, new energy vehicles, and energy storage systems, the market demand for high-energy-density lithium-ion batteries has gradually increased. The energy density of lithium-ion batteries with graphite as the negative electrode has reached its limit, and it is difficult to achieve a major breakthrough in a short period of time. Lithium metal batteries with metallic lithium as the negative electrode material have been widely studied in recent years due to their high energy density. However, poor cycle stability and worrying safety issues have always remained to be resolved. Highly active metallic lithium can react chemically with electrolyte components to form a solid electrolyte interface composed of inorganic and organic substances. Although the thinner solid electrolyte interface can prevent the lithium metal negative electrode from directly contacting the electrolyte to a certain extent, thereby reducing the occurrence of side reactions, the poor mechanical strength during long-term cycling will still lead to the growth of lithium dendrites and the occurrence of lithium volume expansion. When fresh lithium metal is exposed as the solid electrolyte interface breaks, the electrolyte components will react with it, resulting in a decrease in the coulombic efficiency of the battery and poor cycle stability. The inherent defects on the lithium metal surface and the repeated changes in the negative electrode / electrolyte interface during lithium insertion / stripping will accelerate the formation and growth of dendritic lithium. Once the growing lithium dendrites pierce the separator, the battery will face safety issues caused by short circuit. Therefore, in order to promote the development of high energy density lithium metal batteries, it is necessary to solve the complex interface problems faced by lithium metal anodes. Many strategies have been designed to address these challenges, such as electrolyte engineering, solid electrolytes, three-dimensional conductive skeletons, and artificial protective layers. Among these strategies, designing an artificial protective layer on the surface of the lithium metal anode is considered to be a simple and effective strategy to achieve lithium metal anode protection.

[0003] Different protective layer materials have different physical and electrochemical properties. Some materials may have better mechanical strength to inhibit the growth of lithium dendrites, while others may have higher ionic conductivity to promote lithium ion transport. Different composite material structures will also have different shielding and supporting effects on lithium metal. For example, some structures are more effective in preventing side reactions, while others may be better at homogenizing lithium ion flow. In addition, different protective layers have different chemical compatibilities with electrolytes and lithium metal, which affects the way and effect of their function. Some protective layers provide better resistance to electrolyte corrosion and chemical reactions. They exhibit different interfacial behaviors at the interface with lithium metal and electrolyte, including interfacial energy, interfacial resistance, etc., which will directly affect the lithium insertion / stripping process and the overall performance of the battery. Therefore, the rational design of artificial protective layers on the surface of lithium metal anodes is particularly important.

[0004] Patent CN 110071284 A designs a lithium antimony alloy / lithium fluoride composite layer, but it has a low current density and low area capacity (1mA cm) in ether electrolyte. -2 , 1mAh cm -2 ) test conditions, the cycle life of its symmetrical battery can only reach 600h. Patent CN 109037594 A designed a self-healing organic protective layer to protect the lithium metal negative electrode, but in an ether electrolyte containing 1wt.% LiNO3 additive, its symmetrical battery has a low current density and low area capacity (1mA cm -2 , 1mAh cm -2 ) under the test conditions of only about 300h of cycling, polarization phenomenon gradually occurred. The document "ALi3Bi / LiF interfacial layer enabling highly stable lithium metal Anode" designed a lithium metal negative electrode protective layer containing Li3Bi and LiF. The boiling point of the solvent methyl sulfoxide used in its preparation process is 189℃, which is a high-boiling-point substance with low volatility at room temperature. There will be problems with solvent residue. Moreover, this purely inorganic composite protective layer is difficult to achieve long-term cycling at high current density and large area capacity even in ether electrolyte containing 2wt.% LiNO3 additive. Even at 10mA cm -2 、1mAh cm -2 The battery can only cycle for 400h under the test conditions. The literature "Rational construction Ag / LiF / sulfide rich protective layer for remarkably enhancing the stability of Li metal anodes" designed a composite protective layer containing silver / fluorine / sulfur. Its symmetrical battery was tested in an ether electrolyte containing 2wt.% LiNO3 additive and a current density of 5mAcm -2 , area capacity of 5mAh cm -2 Under the test conditions, its cycle life failed to exceed 200h.

[0005] In summary, the existing artificial protective layer is limited to the working conditions of small current density and small cycle area capacity. When the current density and cycle area capacity are increased, the protective layer often does not have a long-term effective effect, so the interface problem of lithium metal negative electrode has not been substantially solved. Therefore, it is urgent to design an artificial protective layer that can be applied to large current density and large area capacity working conditions to solve the interface problem faced by lithium metal negative electrode, so as to achieve long-term stable cycle of the battery. Summary of the invention

[0006] In order to solve the complex interface problems of lithium metal negative electrodes, the present invention proposes a method for preparing a bismuth / fluorine / nitrogen hybrid composite protective layer for lithium metal negative electrodes. The protective layer can adapt to the working conditions of high current density and large area capacity, and effectively inhibits the growth of lithium dendrites and the occurrence of lithium volume expansion effect.

[0007] In order to achieve the purpose, the present invention adopts the following technical scheme:

[0008] A method for preparing a bismuth / fluorine / nitrogen hybridized composite protective layer for a lithium metal negative electrode, the specific steps are as follows:

[0009] Step 1, adding bismuth trifluoromethanesulfonate to an organic solvent, stirring magnetically at room temperature until the mixture is completely dissolved, then adding lithium nitrate and continuing to stir magnetically at room temperature until the mixture is completely dissolved, to obtain a reaction solution;

[0010] Step 2: under an inert gas atmosphere: drip the reaction solution obtained in step 1 onto the surface of the lithium sheet, let it stand until the organic solvent is completely volatilized, then wash with an organic solvent to remove excess impurities, and dry at room temperature, so as to in situ generate a bismuth / fluorine / nitrogen hybrid composite protective layer on the surface of the lithium sheet.

[0011] Preferably, the organic solvent is ethylene glycol dimethyl ether. As a commonly used solvent for ether electrolytes, ethylene glycol dimethyl ether has a low boiling point and high volatility at room temperature, and can effectively solve the negative effects caused by residual low-volatility solvents.

[0012] Preferably, the mass percentage of bismuth trifluoromethanesulfonate and lithium nitrate is 20-80%:80-20%. Different mass ratios of bismuth trifluoromethanesulfonate and lithium nitrate in the reaction solution will cause different chemical reaction environments on the surface of the lithium metal negative electrode, so the structure of the generated protective layer is different, which leads to different effects.

[0013] The present invention also provides a lithium metal negative electrode, comprising a lithium sheet and a bismuth / fluorine / nitrogen hybrid composite protective layer generated in situ on the surface of the lithium sheet.

[0014] The present invention further provides a lithium metal battery, comprising the above-mentioned lithium metal negative electrode, a separator, an electrolyte and a positive electrode.

[0015] Preferably, the diaphragm is a dry-process polypropylene diaphragm.

[0016] Preferably, the electrolyte is an ester electrolyte or an ether electrolyte.

[0017] Preferably, the active material of the positive electrode is lithium iron phosphate or nickel cobalt aluminum.

[0018] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0019] The composite protective layer obtained by the present invention is rich in Bi, Li3Bi, -CF3, LiF, Li x NO y Components, among which: the presence of Bi can guide the uniform deposition of lithium, Li3Bi as a fast ion conductor can effectively alleviate the growth of lithium dendrites and the volume expansion effect of lithium, components - CF3, LiF and Li x NO y It provides a certain degree of insulation and mechanical stability for the interface, thus ensuring the long-term circulation of lithium under the protective layer. With the synergistic effect of all components, a protective layer with ion conductivity, high mechanical strength and electrochemical stability is successfully constructed. This protective layer can adapt to the working conditions of high current density and large area capacity, and effectively inhibits the growth of lithium dendrites and the occurrence of lithium volume expansion effect. When matched with commercial nickel-cobalt-aluminum ternary positive electrode or lithium iron phosphate positive electrode, batteries with protective layer show low capacity attenuation, so they have good prospects for commercial application. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The scanning electron microscope images of the surface (a) and cross-section (b) of a lithium sheet protected by the bismuth / fluorine / nitrogen hybrid composite protective layer prepared in Example 1. The inset in (a) is an optical photograph of the protective layer.

[0021] Figure 2 This is the surface element analysis diagram of the bismuth / fluorine / nitrogen hybrid composite protective layer prepared in Example 1.

[0022] Figure 3 This is the X-ray photoelectron spectrum of the bismuth / fluorine / nitrogen hybrid composite protective layer prepared in Example 1.

[0023] Figure 4 This is a diagram of the Young's modulus of the bismuth / fluorine / nitrogen hybridized composite protective layer prepared in Example 1.

[0024] Figure 5 The symmetrical battery composed of the lithium sheet with the bismuth / fluorine / nitrogen hybrid composite protective layer and the lithium sheet without the protective layer in Example 1 was charged at 5 mA cm -2 、5mAh cm -2 Voltage-time graph under test conditions.

[0025] Figure 6 The symmetrical battery composed of the lithium sheet with the bismuth / fluorine / nitrogen hybrid composite protective layer and the lithium sheet without the protective layer in Example 1 was charged at 5 mA cm -2 、5mAh cm -2 Charge and discharge curves under test conditions.

[0026] Figure 7The symmetrical battery composed of the lithium sheet with the bismuth / fluorine / nitrogen hybrid composite protective layer and the lithium sheet without the protective layer in Example 1 was subjected to 10 mA cm -2 、5mAh cm -2 Voltage-time graph under test conditions.

[0027] Figure 8 The symmetrical battery composed of the lithium sheet with the bismuth / fluorine / nitrogen hybrid composite protective layer and the lithium sheet without the protective layer in Example 1 was subjected to 10 mA cm -2 、10mAh cm -2 Voltage-time graph under test conditions.

[0028] Fig. 9 The symmetrical battery composed of the lithium sheet with the bismuth / fluorine / nitrogen hybrid composite protective layer and the lithium sheet without the protective layer in Example 1 was charged at 5 mA cm -2 、5mAh cm -2 Scanning electron microscope images after 20 cycles under test conditions, where (a) and (b) correspond to lithium sheets without a protective layer, and (c) and (d) correspond to lithium sheets with a protective layer.

[0029] Fig.10 1 is a performance diagram of a Li / LFP full battery assembled from a lithium sheet with a bismuth / fluorine / nitrogen hybrid composite protective layer and a lithium sheet without a protective layer in Example 1.

[0030] Fig.11 1 is a performance diagram of a Li / NCA full battery assembled from a lithium sheet with a bismuth / fluorine / nitrogen hybrid composite protective layer and a lithium sheet without a protective layer in Example 1.

[0031] Fig.12 The symmetrical battery assembled from the lithium sheet with the bismuth / fluorine / nitrogen hybrid composite protective layer in Example 2 was -2 、5mAh cm -2 Voltage-time graph under test conditions.

[0032] Fig.13 The symmetrical battery of Comparative Example 1 is at 5 mA cm -2 、5mAh cm -2 Voltage-time curve under test conditions, with the inset being an optical photograph of the protective layer.

[0033] Fig.14 The symmetrical battery of Comparative Example 2 is at 5 mA cm -2 、5mAh cm -2 Voltage-time curve under test conditions, with the inset being an optical photograph of the protective layer.

[0034] Fig.15The symmetrical battery of Comparative Example 3 is at 5 mA cm -2 、5mAh cm -2 Voltage-time curve under test conditions, with the inset being an optical photograph of the protective layer. DETAILED DESCRIPTION

[0035] The technical solution of the present invention is further described and explained below in conjunction with embodiments, but these embodiments are not intended to limit the protection scope of the present invention.

[0036] Example 1

[0037] This embodiment provides a method for preparing a bismuth / fluorine / nitrogen hybridized composite protective layer for a lithium metal negative electrode, comprising the following steps:

[0038] Step 1: Add 104 mg of bismuth trifluoromethanesulfonate to 2 mL of ethylene glycol dimethyl ether, stir magnetically for 12 h at room temperature until completely dissolved, then add 26 mg of lithium nitrate, stir magnetically for 12 h at room temperature until completely dissolved, to obtain a uniformly mixed reaction solution.

[0039] Step 2, in an argon-protected glove box: 50 μL of the reaction solution obtained in step 1 is added dropwise to one side of a lithium sheet with a diameter of 16 cm, and allowed to stand until the organic solvent is completely volatilized, and then washed with ethylene glycol dimethyl ether to remove excess impurities and dried at room temperature, thereby in situ forming a bismuth / fluorine / nitrogen hybridized composite protective layer on the surface of the lithium sheet.

[0040] The lithium sheet protected by the bismuth / fluorine / nitrogen hybrid composite protective layer obtained in this example was characterized as follows:

[0041] 1. Characterization of protective layer morphology and components

[0042] Figure 1 The scanning electron microscope images of the surface and cross section of the lithium sheet protected by the bismuth / fluorine / nitrogen hybrid composite protective layer prepared in Example 1 show that the protective layer on the surface of the lithium sheet presents a dense morphology and has a thickness of 19 μm.

[0043] Figure 2 The surface element analysis of the bismuth / fluorine / nitrogen hybridized composite protective layer prepared in Example 1 shows that the elements C, O, Bi, F, and N are evenly distributed on the surface of the lithium sheet. The presence of these elements indicates that bismuth trifluoromethanesulfonate and lithium nitrate have chemically reacted with lithium, respectively.

[0044] In order to further determine the composition of the protective layer, Figure 3 The X-ray photoelectron spectrum of the bismuth / fluorine / nitrogen hybrid composite protective layer prepared in Example 1 is given. The results show that the main components of the protective layer are Bi, Li3Bi, -CF3, LiF and Li x NO y .

[0045] Figure 4 This is a graph of the Young's modulus of the bismuth / fluorine / nitrogen hybridized composite protective layer prepared in Example 1, and its average Young's modulus is 6.04 GPa. This higher Young's modulus will help to enhance the inhibitory effect on lithium dendrites and volume expansion.

[0046] 2. Half-cell performance characterization

[0047] The lithium sheet with bismuth / fluorine / nitrogen hybrid composite protective layer prepared in Example 1 was used as an electrode, and was assembled into a symmetrical battery with an ether electrolyte and a dry polypropylene separator. A comparative study was conducted using a lithium sheet without a protective layer as a reference. The composition of the ether electrolyte used was: 1M LiTFSI dissolved in a mixed solution of 1,3-dioxolane / ethylene glycol dimethyl ether (volume ratio of 1:1), and 1wt% LiNO3 was added as an additive. The injection volume of the electrolyte was 50μL.

[0048] Figure 5 For two symmetrical cells at 5 mA cm -2 、5mAh cm -2 The voltage-time curve under the test conditions shows that the symmetrical battery with bismuth / fluorine / nitrogen hybrid composite protective layer can stably cycle for more than 2000 hours at high current density and large cycle area capacity without obvious polarization, while the symmetrical battery without protective layer has serious polarization at 210 hours.

[0049] Figure 6 For two symmetrical cells at 5 mA cm -2 、5mAh cm -2 The charge and discharge curves for different numbers of cycles under the test conditions show that compared with the symmetrical battery without a protective layer, the symmetrical battery with a bismuth / fluorine / nitrogen hybrid composite protective layer shows a smaller charge and discharge voltage platform, which is consistent with the lower voltage polarization.

[0050] In order to further verify the cycling capability of the symmetrical battery with bismuth / fluorine / nitrogen hybridized composite protective layer at higher current density and higher cycling area capacity, Figure 7 and Figure 8 The results of two symmetrical batteries at (10 mA cm -2 、5mAh cm -2 ) and (10mAcm -2 、10mAh cm -2) The voltage-time curve diagram under the test conditions shows that the symmetrical battery with bismuth / fluorine / nitrogen hybrid composite protective layer can still exhibit better cycling performance than the symmetrical battery without protective layer. This shows that even under high current density and large cycle area capacity, the protective layer can still effectively alleviate the growth of lithium dendrites and the volume expansion effect of lithium.

[0051] Fig. 9 The lithium metal anode with bismuth / fluorine / nitrogen hybrid protective layer and the lithium metal anode without protective layer are 5mAcm -2 、5mAh cm -2 From the scanning electron microscope images after 20 cycles under the test conditions, it is not difficult to find that the lithium without a protective layer shows more cracks and is accompanied by a larger volume expansion, while the lithium surface protected by the bismuth / fluorine / nitrogen hybrid composite protective layer still maintains a relatively dense morphology, which intuitively reflects the inhibitory effect of the prepared protective layer on the growth of lithium dendrites and the volume expansion effect of lithium.

[0052] 3. Li / LFP full battery performance characterization

[0053] The lithium sheet with bismuth / fluorine / nitrogen hybrid composite protective layer prepared in Example 1 was used as the metal negative electrode and assembled with lithium iron phosphate positive electrode sheet, ether electrolyte (1M LiTFSI dissolved in a mixed solution of 1,3-dioxolane / ethylene glycol dimethyl ether (volume ratio of 1:1) and 1wt% LiNO3 added as an additive) and dry polypropylene separator to form a Li / LFP full battery. At the same time, a full battery assembled with a lithium sheet without protective layer as the metal negative electrode was used as a reference example for comparative study. Among them, the preparation process of lithium iron phosphate positive electrode sheet is as follows: the positive electrode active material lithium iron phosphate, carbon black, and polyvinylidene fluoride are dispersed in 1-methyl-2-pyrrolidone at a mass ratio of 8:1:1, ball milled for 1h, and then coated on the surface of aluminum foil, vacuum dried at 80°C for 12h, and punched into a disc with a diameter of 14mm for standby use.

[0054] The cycle test conditions of the battery are: voltage range is 2-3.8V, and the electrolyte injection coefficient is 0.1mL / mg.

[0055] Fig.10 The cycle performance diagram of two Li / LFP full batteries shows that the battery protected by the protective layer maintains a capacity retention rate of up to 91.1% after 400 cycles, while the battery without protective layer protection shows a faster capacity decay trend.

[0056] 4. Li / NCA full battery performance characterization

[0057] The lithium sheet with bismuth / fluorine / nitrogen hybrid composite protective layer prepared in Example 1 was used as the metal negative electrode and assembled with nickel-cobalt-aluminum ternary positive electrode sheet, ester electrolyte (1M LiPF6 dissolved in ethylene carbonate / ethyl methyl carbonate / dimethyl carbonate (volume ratio of 1:1:1)) and dry polypropylene separator to form a Li / NCA full battery. At the same time, a full battery assembled with a lithium sheet without protective layer as the metal negative electrode was used as a reference example for comparative study. Among them, the preparation process of nickel-cobalt-aluminum ternary positive electrode sheet is as follows: the positive electrode active material NCA (LiNi 0.8 Co 0.15 Al 0.05 O2), carbon black and polyvinylidene fluoride were dispersed in 1-methyl-2-pyrrolidone in a mass ratio of 8:1:1, ball-milled for 1 hour, and then coated on the surface of aluminum foil. After vacuum drying at 80°C for 12 hours, they were punched into discs with a diameter of 14 mm for standby use.

[0058] The cycle test conditions of the full battery are: voltage range is 3-4.3V, and the electrolyte injection coefficient is 0.1mL / mg.

[0059] Fig.11 The performance diagram of two Li / NCA full batteries shows that after 200 cycles, the capacity attenuation rate of the battery protected by the protective layer is significantly lower than that of the battery without the protective layer. This indicates that the introduction of the bismuth / fluorine / nitrogen hybrid composite protective layer reduces the negative effects caused by interface problems.

[0060] The above results show that the introduction of the bismuth / fluorine / nitrogen hybrid composite protective layer inhibits the growth of lithium dendrites and the volume expansion effect of lithium under high current density and large cycle area capacity, effectively solving the complex interface problems faced by lithium metal negative electrodes. When matched with commercial lithium iron phosphate positive electrodes or nickel-cobalt-aluminum ternary positive electrodes, batteries with protective layers show low capacity attenuation and have great prospects for commercial applications.

[0061] Example 2

[0062] This embodiment provides a method for preparing a bismuth / fluorine / nitrogen hybridized composite protective layer for a lithium metal negative electrode, comprising the following steps:

[0063] Step 1, add 78 mg of bismuth trifluoromethanesulfonate to 2 mL of ethylene glycol dimethyl ether, stir magnetically for 12 h at room temperature until completely dissolved, then add 52 mg of lithium nitrate, stir magnetically for 12 h at room temperature until completely dissolved, to obtain a uniformly mixed reaction solution.

[0064] Step 2, in an argon-protected glove box: 50 μL of the reaction solution obtained in step 1 is added dropwise to one side of a lithium sheet with a diameter of 16 cm, and allowed to stand until the organic solvent is completely volatilized, and then washed with ethylene glycol dimethyl ether to remove excess impurities and dried at room temperature, thereby in situ forming a bismuth / fluorine / nitrogen hybridized composite protective layer on the surface of the lithium sheet.

[0065] The lithium sheet with the bismuth / fluorine / nitrogen hybrid composite protective layer prepared in this example was used as an electrode to assemble a symmetrical battery in the same manner as in Example 1. Fig.12 For a symmetrical battery at 5 mA cm -2 、5mAh cm -2 Voltage-time curve under test conditions. The results show that by changing the mass of bismuth trifluoromethanesulfonate and lithium nitrate, the designed composite protective layer can still achieve the inhibitory effect on the growth of lithium dendrites and the volume expansion effect of lithium under high current density and large cycle area capacity.

[0066] Comparative Example 1

[0067] The difference from Examples 1 and 2 is that the solute of the reaction solution is only bismuth trifluoromethanesulfonate, specifically:

[0068] Step 1: Add 130 mg of bismuth trifluoromethanesulfonate to 2 mL of ethylene glycol dimethyl ether and stir magnetically at room temperature for 12 h until completely dissolved to obtain a reaction solution.

[0069] Step 2, in an argon-protected glove box: 50 μL of the reaction solution obtained in step 1 is added dropwise to one side of a lithium sheet with a diameter of 16 cm, and allowed to stand until the organic solvent is completely volatilized, and then washed with ethylene glycol dimethyl ether to remove excess impurities and dried at room temperature, thereby in situ forming a bismuth / fluorine composite protective layer on the surface of the lithium sheet.

[0070] The lithium sheet with the bismuth / fluorine composite protective layer prepared in this comparative example was used as an electrode to assemble into a symmetrical battery in the same manner as in Example 1. Fig.13 The symmetrical battery of Comparative Example 1 is at 5 mA cm -2 、5mAh cm -2 Voltage-time curve under test conditions. The embedded image shows that the protective layer presents a black surface, which is the result of the reaction between bismuth trifluoromethanesulfonate and lithium. From the curve, it can be seen that the symmetrical battery cannot withstand the test conditions of high current density and large area capacity, and a short circuit occurs.

[0071] Comparative Example 2

[0072] The difference from Examples 1 and 2 is that the solute of the reaction solution is only lithium nitrate, specifically:

[0073] Step 1: Add 130 mg of lithium nitrate to 2 mL of ethylene glycol dimethyl ether and stir magnetically at room temperature for 12 h until completely dissolved to obtain a reaction solution.

[0074] Step 2, in an argon-protected glove box: 50 μL of the reaction solution obtained in step 1 is added dropwise to one side of a lithium sheet with a diameter of 16 cm, and allowed to stand until the organic solvent is completely volatilized, and then washed with ethylene glycol dimethyl ether to remove excess impurities and dried at room temperature, thereby generating a nitrogen protective layer in situ on the surface of the lithium sheet.

[0075] The lithium sheet with nitrogen protective layer prepared in this comparative example was used as an electrode to assemble into a symmetrical battery in the same manner as in Example 1. Fig.14 The symmetrical battery of Comparative Example 2 is at 5 mA cm -2 、5mAh cm -2 Voltage-time curve under test conditions. The embedded picture shows that there are sporadic white areas on the surface of the lithium sheet, which is the result of the reaction between lithium nitrate and lithium. From the curve, it can be seen that the cycle stability of the symmetrical battery is poor, and polarization begins to occur after 72 hours of cycling.

[0076] Comparative Example 3

[0077] The difference from Examples 1 and 2 is that the solute of the reaction solution is bismuth nitrate, specifically:

[0078] Step 1: Add 130 mg of bismuth nitrate to 2 mL of ethylene glycol dimethyl ether and stir magnetically at room temperature for 12 h until completely dissolved to obtain a reaction solution.

[0079] Step 2, in an argon-protected glove box: 50 μL of the reaction solution obtained in step 1 is added dropwise to one side of a lithium sheet with a diameter of 16 cm, and allowed to stand until the organic solvent is completely volatilized, and then washed with ethylene glycol dimethyl ether to remove excess impurities and dried at room temperature, thereby in situ forming a bismuth / nitrogen protective layer on the surface of the lithium sheet.

[0080] The lithium sheet with bismuth / nitrogen protective layer prepared in this comparative example was used as an electrode to assemble into a symmetrical battery in the same manner as in Example 1. Fig.15 The symmetrical battery of Comparative Example 3 is at 5 mA cm -2 、5mAh cm -2 Voltage-time curve under test conditions. The embedded image shows that the protective layer presents a black surface, which is the result of the reaction between bismuth nitrate and lithium. From the curve, it can be seen that the polarization phenomenon of the symmetrical battery gradually becomes serious after 210h of cycling under the test conditions of high current density and large area capacity.

[0081] The above embodiments are only preferred examples of the present invention, which are intended to illustrate the technical concept and features of the present invention, but not to limit the implementation methods. For those skilled in the art, changes and modifications can be made according to the spirit of the present invention, and these changes and modifications should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a bismuth / fluorine / nitrogen hybrid composite protective layer for a lithium metal negative electrode, It is characterized in that Here are the steps: Step 1, adding bismuth trifluoromethanesulfonate to an organic solvent, stirring magnetically at room temperature until the mixture is completely dissolved, then adding lithium nitrate and continuing to stir magnetically at room temperature until the mixture is completely dissolved, to obtain a reaction solution; Step 2: under an inert gas atmosphere: drip the reaction solution obtained in step 1 onto the surface of the lithium sheet, let it stand until the organic solvent is completely volatilized, then wash with an organic solvent and dry at room temperature, so as to in situ generate a bismuth / fluorine / nitrogen hybrid composite protective layer on the surface of the lithium sheet.

2. A method for preparing a lithium metal negative electrode bismuth / fluorine / nitrogen hybrid composite protective layer according to claim 1, Features: The organic solvent is ethylene glycol dimethyl ether.

3. The method for preparing a lithium metal negative electrode bismuth / fluorine / nitrogen hybrid composite protective layer according to claim 1, Features: The mass percentages of the bismuth trifluoromethanesulfonate and lithium nitrate are 20-80%:80-20%.

4. A lithium metal negative electrode, It is characterized in that The invention comprises a lithium sheet and a bismuth / fluorine / nitrogen hybrid composite protective layer generated in situ on the surface of the lithium sheet.

5. A lithium metal battery, It is characterized in that The lithium metal negative electrode according to claim 4 is used.

Citation Information

Patent Citations

  • Metal lithium negative electrode for secondary battery and preparation and application thereof

    CN110783529A

  • Preparation method of lithium fluoride and organic fluoride hybridized lithium metal negative electrode protection layer, lithium metal negative electrode and lithium battery

    CN115172668A

  • Preparation method of lithium metal surface air stability protective layer

    CN116288301A

  • Lithium-containing electrode, preparation method therefor and lithium battery containing same

    WO2019019407A1

  • Lithium-ion battery based on in-situ negative-electrode lithium supplementation, and preparation method therefor

    WO2024109853A1

Cited By

  • Directional double-layer structure mixed ion / electron conductor intermediate layer and preparation method and application thereof

    CN121460586A