Modified graphite felt, preparation method thereof and flow battery
Through chemical vapor deposition and strong acid corrosion technology, the problem of insufficient improvement in specific surface area and mechanical properties of graphite felt in the existing technology has been solved, and a high-energy-efficiency flow battery electrode material has been realized, ensuring the stability of carbon nanotubes and electrodes. of long life.
Patent Information
- Application Number
- CN202411177821.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-10-29
AI Technical Summary
The existing technology has shortcomings in improving the specific surface area and mechanical properties of graphite felt. The hydrothermal method of growing carbon nanotubes has a limited load capacity and damages the graphite felt itself, which cannot meet the high energy efficiency requirements of flow batteries for electrode materials.
The chemical vapor deposition method is used to grow carbon nanotubes in situ on the surface of graphite felt, and etch them in strong acid to control the catalyst ratio and gas flow, adjust the carbon nanotube loading, increase the specific surface area and hydrophilicity, and enhance the active site of the electrode. point.
The specific surface area and hydrophilicity of the graphite felt are significantly improved, the energy efficiency of the flow battery is improved, and the stability of the carbon nanotubes and the long life of the electrode are ensured.
Smart Images

Figure CN118867286A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of batteries, and in particular relates to a modified graphite felt and a preparation method thereof, and a liquid flow battery. Background Art
[0002] With the rapid development of the global economy, the energy crisis has become increasingly prominent, and the development of new energy industries has become a strategic goal for countries around the world. The current new energy industry mainly includes clean energy such as solar energy, wind energy, and tidal energy. However, these energy sources are greatly affected by climate, geography and other characteristics, and the supply of energy has shortcomings such as intermittent. Only a small part of the electricity is connected to the grid, and the phenomenon of wind and power abandonment is serious. Therefore, safe and efficient large-scale energy storage technology is particularly important for the development of the new energy industry.
[0003] In recent years, people have paid more and more attention to the safety of energy storage batteries. Liquid flow batteries have gradually gained attention due to their advantages such as ultra-high safety, long service life and relatively flexible design. After decades of development, liquid flow batteries have made great progress. Electrodes, as important components in liquid flow batteries, play a vital role in the overall electrochemical performance of liquid flow batteries.
[0004] The current mainstream electrodes include metal electrodes, composite conductive plastic electrodes and carbon electrodes. Among them, the polyacrylonitrile-based graphite felt in the carbon electrode has the advantages of good chemical stability, high conductivity, strong mechanical properties and a wide electrochemical potential range, which are suitable for liquid flow batteries. However, the specific surface area of graphite felt is limited and its hydrophilicity is poor. The prior art is to use a hydrothermal method to catalytically grow carbon nanotubes on the surface of graphite felt to increase the specific surface area of graphite felt. The hydrothermal method loads carbon nanotubes on the surface of graphite felt: the graphite felt and the solvent providing the carbon source are placed in a high-pressure container, the high-pressure container is placed in a heating container, and the carbon nanotubes are catalytically grown on the surface of the graphite felt by controlling the reaction time, the reaction temperature and the concentration of the solvent. However, the hydrothermal method is limited in the amount of carbon nanotubes grown on graphite felt, and the specific surface area of the graphite felt is not greatly improved, and the hydrothermal method has a large damage to the mechanical properties of the graphite felt itself. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a modified graphite felt and a preparation method thereof and a liquid flow battery.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] A modified graphite felt, comprising graphite felt and carbon nanotubes in situ grown on the surface of the graphite felt; preferably, the loading amount of the carbon nanotubes is greater than 0.48 mg / cm 2 ; preferably 0.48-0.65mg / cm 2 The specific surface area of the modified graphite felt is greater than 46m2 g -1 ; preferably 46-62m 2 g -1 ; Preferably, the contact angle of the modified graphite felt is 0°.
[0008] The present invention also includes a method for preparing a modified graphite felt, comprising the following steps:
[0009] 1) In-situ growth of carbon nanotubes on graphite felt using chemical vapor deposition;
[0010] 2) Add strong acid for corrosion.
[0011] The specific steps of step 1) are:
[0012] 1.1) adding graphite felt into the catalyst solution for impregnation and drying;
[0013] 1.2) The dried graphite felt is reduced in hydrogen;
[0014] 1.3) The reduced graphite felt is in-situ grown in a mixture of an inert gas, hydrogen and a carbon source gas to obtain a graphite felt with carbon nanotubes grown on the surface.
[0015] In step 1.1), the graphite felt is pre-treated, specifically, the steps are: completely immersed in acetone for ultrasonic cleaning to remove surface impurities; then washed with deionized water and placed in a drying oven for drying; preferably, the graphite felt is polyacrylonitrile-based graphite felt.
[0016] Preferably, the catalyst solution in step 1.1) is a mixture aqueous solution of copper salt, yttrium salt and nickel salt;
[0017] Preferably, the molar ratio of the copper salt, yttrium salt and nickel salt is (0.001-0.04): (0.001-0.03): (0.001-0.04); preferably (0.005-0.014): (0.003-0.01): (0.005-0.021);
[0018] Preferably, the copper salt, yttrium salt and nickel salt are all nitrates.
[0019] In step 1.2), the amount of hydrogen introduced is (10-60) sccm;
[0020] Preferably, the reduction temperature is 100-500° C. and the time is 1-120 min.
[0021] In step 1.3), the ratio of the amount of hydrogen, inert gas and carbon source gas introduced is: (10-50):
[0022] (50-300): (5-30); preferably (10-30): 100: (10-20);
[0023] Preferably, the in-situ growth temperature is 100-800°C and the time is 10-80 min; preferably, the growth temperature is 400-600°C and the time is 10 min;
[0024] Preferably, the inert gas is Ar; and the carbon source gas is C2H2.
[0025] The strong acid in step 2) is concentrated nitric acid; the specific steps of step 2) are: the graphite felt treated in step 1) is completely immersed in concentrated nitric acid for chemical corrosion for 1-5 hours, taken out and repeatedly rinsed with deionized water until neutral, and then dried to obtain the modified graphite felt.
[0026] The present invention also includes a liquid flow battery, comprising the modified graphite felt as an electrode, a positive electrode electrolyte, a negative electrode electrolyte and a diaphragm.
[0027] The negative electrode electrolyte includes FeCl3, NaOH, and TEOA; the positive electrode electrolyte includes K4[Fe(CN)6] and NaOH; and the diaphragm is a SPEEK membrane.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The technical solution of the present application adopts chemical vapor deposition to grow carbon nanotubes in situ on the surface of graphite felt. Under the premise of not destroying the mechanical properties of the graphite felt, the loading amount of carbon nanotubes per unit area is regulated by controlling the ratio of catalyst, the flow rate of gas introduced and the growth temperature, so that the loading amount of carbon nanotubes reaches 0.48 mg / cm 2 Above, even up to 0.65mg / cm 2 ; The specific surface area of graphite felt was greatly increased without obvious carbon nanotube shedding, reaching 46m 2 g -1 Above, even up to 62m 2 g -1 ; and the contact angle is 0°. When assembled into a liquid flow battery, it provides more active sites for the reaction of ions during the charge and discharge process. After strong acid corrosion, more oxygen-containing functional groups are introduced to improve the hydrophilicity of the material, thereby achieving the purpose of improving the energy efficiency of the liquid flow battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is an electron microscope image of the modified graphite felt obtained in Example 1 of the present invention. DETAILED DESCRIPTION
[0031] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiments.
[0032] A modified graphite felt is prepared by in-situ growing carbon nanotubes on the graphite felt and then immersing the graphite felt in a strong acid for corrosion.
[0033] The present invention also includes a method for preparing a modified graphite felt, comprising the following steps:
[0034] 1) In-situ growth of carbon nanotubes on graphite felt by chemical vapor deposition; 1.1) The graphite felt is pre-treated, specifically by soaking it in acetone for ultrasonic cleaning to remove surface impurities; then washing it with deionized water and drying it in a drying oven; the graphite felt is polyacrylonitrile-based graphite felt. The graphite felt is added to a catalyst solution for immersion and drying; 1.2) The dried graphite felt is reduced in hydrogen; 1.3) The reduced graphite felt is in-situ grown in a mixture of inert gas, hydrogen and carbon source gas to obtain graphite felt with carbon nanotubes grown on its surface.
[0035] 2) Add strong acid for corrosion. The strong acid is concentrated nitric acid; the specific steps are: Step 1) The treated graphite felt is completely immersed in concentrated nitric acid for chemical corrosion for 1-5 hours, and after being taken out, it is repeatedly rinsed with deionized water until it is neutral, and the modified graphite felt is obtained after drying.
[0036] The catalyst solution in step 1.1) is a mixture aqueous solution of copper salt, yttrium salt and nickel salt; the molar ratio of the copper salt, yttrium salt and nickel salt is (0.001-0.04):(0.001-0.03):(0.001-0.04); specifically, it can be 0.001:0.001:0.001, 0.005:0.01:0.021, 0.04:0.03:0.04, etc., preferably (0.005-0.014):(0.003-0.01):(0.005-0.021); the copper salt, yttrium salt and nickel salt are all nitrates.
[0037] In step 1.2), the amount of hydrogen introduced is (10-60) sccm; specifically, it can be 10 sccm, 30 sccm, 60 sccm, and 30 sccm is used as an example in this application. The reduction temperature is 100-500°C, and the time is 1-120 min. Specifically, it can be 100°C, 120 min; 500°C, 1 min; 100°C, 30 min, etc., and 100°C, 30 min is used as a preferred example for description.
[0038] In step 1.3), the ratio of the amount of hydrogen, inert gas and carbon source gas introduced is: (10-50):
[0039] (50-300): (5-30); specifically, it can be 10:50:5, 50:300:30, 10:100:20, 30:100:20, etc., preferably (10-30): 100: (10-20);
[0040] The in-situ growth temperature is 100-800°C and the time is 10-80min. Specifically, it can be 100°C, 80min, 400°C, 10min, 800°C, 10min, 600°C, 10min. Preferably, the growth temperature is 400-600°C and the time is 10min.
[0041] Preferably, the inert gas is Ar; and the carbon source gas is C2H2.
[0042] The present invention also includes a liquid flow battery, comprising the modified graphite felt as an electrode, a positive electrode electrolyte, a negative electrode electrolyte and a diaphragm.
[0043] The negative electrode electrolyte includes FeCl3, NaOH, and TEOA; the positive electrode electrolyte includes K4[Fe(CN)6] and NaOH; and the diaphragm is a SPEEK membrane.
[0044] The following is an explanation with reference to specific embodiments.
[0045] Example 1
[0046] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0047] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and immerse it completely in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven and dry it at 50°C for 24 h. Then take it out for use.
[0048] (2) Weigh 2 g of copper nitrate hexahydrate, 3.8 g of yttrium nitrate hexahydrate, and 2.9 g of nickel nitrate hexahydrate, add them to 1 L of ethanol, and mechanically stir until the chemicals are completely dissolved to obtain a Cu-Y-Ni mixed solution.
[0049] (3) The graphite felt treated in step (1) is completely immersed in the Cu-Y-Ni mixed solution prepared in step (2) for 24 hours.
[0050] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0051] (5) The graphite felt treated in step (4) was reduced at 100°C with a H2 flow rate of 30 sccm (standard cubic centimeters per minute) for 30 min, and then grown in situ at 500°C for 10 min in an atmosphere of H2:Ar:C2H2 flow rate = 30:100:10 sccm. After the growth was completed, the felt was taken out and cooled to room temperature.
[0052] (6) The graphite felt treated in step (5) is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 1 hour, and after being taken out, it is repeatedly rinsed with deionized water until it becomes neutral, and then dried to obtain a graphite felt composite material.
[0053] The modified polyacrylonitrile-based graphite felt prepared in this embodiment is as follows: Figure 1 As shown in the figure, carbon nanotubes are grown on the surface to increase its specific surface area, which is 11m higher than the original graphite felt. 2 g -1 The specific surface area of the modified graphite felt reaches 53m 2 g -1 , which is nearly 5 times higher. Carbon nanotube loading 0.5mg / cm 2 After treatment with nitric acid, the contact angle was measured to be 0°, which improved the hydrophilicity.
[0054] It was assembled into a flow battery (the negative electrode electrolyte was prepared by 0.2 mol / L FeCl3, 3 mol / L NaOH, and 2 mol / L TEOA; the positive electrode electrolyte was prepared by 0.2 mol / L K4[Fe(CN)6] and 1 mol / L NaOH; the diaphragm was a SPEEK membrane; and the graphite plate was used as the current collector). 2 At a current density of 1.5 V and 0.7 V, respectively, the charge and discharge voltages were 1.5 V and 0.7 V, respectively, and the cycle was 50 times. Under this condition, compared with the unmodified graphite felt, the energy efficiency was increased from the original 65.4% to 74.2%.
[0055] Example 2
[0056] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0057] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and immerse it completely in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven and dry it at 50°C for 24 h. Then take it out for use.
[0058] (2) Weigh 4 g of copper nitrate hexahydrate, 1.2 g of yttrium nitrate hexahydrate, and 2.9 g of nickel nitrate hexahydrate, add them to 1 L of ethanol, and mechanically stir until the chemicals are completely dissolved to obtain a Cu-Y-Ni mixed solution.
[0059] (3) The graphite felt treated in step (1) is completely immersed in the Cu-Y-Ni mixed solution prepared in step (2) for 12 hours.
[0060] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 80° C. for 12 h.
[0061] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm of H2 for 30 min, and then grown in situ at 600°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:20. After the growth was completed, the felt was taken out and cooled to room temperature.
[0062] (6) The graphite felt treated in step (5) is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 1 hour, and after being taken out, it is repeatedly rinsed with deionized water until it becomes neutral, and then dried to obtain a graphite felt composite material.
[0063] The modified polyacrylonitrile-based graphite felt prepared in this embodiment has carbon nanotubes grown on its surface to increase its specific surface area. Compared with the specific surface area of the original graphite felt of 11m 2 g -1 The specific surface area of the modified graphite felt reaches 54m 2 g -1 , carbon nanotube loading 0.52mg / cm 2 After nitric acid treatment, the contact angle was measured to be 0°, which improved the hydrophilicity. It was assembled into a flow battery (the negative electrode electrolyte was prepared by 0.2 mol / L FeCl3, 3 mol / L NaOH, and 2 mol / L TEOA; the positive electrode electrolyte was prepared by 0.2 mol / L K4[Fe(CN)6] and 1 mol / L NaOH; the diaphragm was SPEEK membrane; the graphite plate was used as the current collector), and the flow rate was 150 mA / cm 2 At a current density of 1.5 V and 0.7 V, respectively, the charge and discharge voltages were 1.5 V and 0.7 V, respectively, and the cycle was 50 times. Under this condition, compared with the unmodified graphite felt, the energy efficiency was increased from the original 62.4% to 73.3%.
[0064] Example 3
[0065] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0066] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and immerse it completely in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven and dry it at 50°C for 24 h. Then take it out for use.
[0067] (2) Weigh 2 g of copper nitrate hexahydrate, 7.6 g of yttrium nitrate hexahydrate, and 4.3 g of nickel nitrate hexahydrate, add them to 1 L of ethanol, and mechanically stir until the chemicals are completely dissolved to obtain a Cu-Y-Ni mixed solution.
[0068] (3) Completely immerse the treated graphite felt in the Cu-Y-Ni mixed solution prepared in step (2) for 24 hours.
[0069] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 60° C. for 12 h.
[0070] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm of H2 for 30 min, and then grown in situ at 500°C for 20 min in an atmosphere of H2:Ar:C2H2=10:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0071] The treated graphite felt is completely immersed in concentrated nitric acid (68%) for chemical etching for 3 hours, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0072] The modified polyacrylonitrile-based graphite felt prepared in this embodiment has carbon nanotubes grown on its surface to increase its specific surface area. Compared with the specific surface area of the original graphite felt of 11m 2 g -1 The specific surface area of the modified graphite felt reaches 58m 2 g -1 , carbon nanotube loading 0.65mg / cm 2 After being treated with nitric acid, the contact angle was measured to be 0°, which improved the hydrophilicity. It was assembled into a flow battery (the negative electrode electrolyte was prepared by 0.2 mol / L FeCl3, 3 mol / L NaOH, and 2 mol / L TEOA; the positive electrode electrolyte was prepared by 0.2 mol / L K4[Fe(CN)6] and 1 mol / L NaOH; the diaphragm was SPEEK membrane; the graphite plate was used as the current collector), and the flow rate was 100 mA / cm 2 At a current density of 1.5 V and 0.7 V, respectively, the charge and discharge voltages were 1.5 V and 0.7 V, respectively, and the cycle was 50 times. Under this condition, compared with the unmodified graphite felt, the energy efficiency was increased from the original 65.4% to 75.6%.
[0073] Example 4
[0074] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0075] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and immerse it completely in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven and dry it at 50°C for 24 h. Then take it out for use.
[0076] (2) Weigh 2 g of copper nitrate hexahydrate, 3.8 g of yttrium nitrate hexahydrate, and 1.5 g of nickel nitrate hexahydrate, add them to 1 L of ethanol, and mechanically stir until the chemicals are completely dissolved to obtain a Cu-Y-Ni mixed solution.
[0077] (3) The graphite felt treated in step (1) is completely immersed in the Cu-Y-Ni mixed solution prepared in step (2) for 12 hours.
[0078] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 80° C. for 12 h.
[0079] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm (standard cubic centimeters per minute) of H2 for 10 min, and then grown in situ at 300°C for 30 min in an atmosphere of H2:Ar:C2H2=30:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0080] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68%) for chemical corrosion for 1 hour, taken out and repeatedly rinsed with deionized water until it becomes neutral, and dried to obtain a graphite felt composite material.
[0081] The modified polyacrylonitrile-based graphite felt prepared in this embodiment has carbon nanotubes grown on its surface to increase its specific surface area. Compared with the specific surface area of the original graphite felt of 11m 2 g -1 The specific surface area of the modified graphite felt reaches 46m 2 g -1 , carbon nanotube loading 0.48mg / cm 2 After nitric acid treatment, the contact angle was 0°, which improved the hydrophilicity. It was assembled into a flow battery (the negative electrode electrolyte was prepared by 0.2 mol / L FeCl3, 3 mol / L NaOH, and 2 mol / L TEOA; the positive electrode electrolyte was prepared by 0.2 mol / L K4[Fe(CN)6] and 1 mol / L NaOH; the diaphragm was SPEEK membrane; the graphite plate was used as the current collector), and the flow rate was 50 mA / cm 2At a current density of 1.5 V and 0.7 V, respectively, the charge and discharge voltages were 1.5 V and 0.7 V, respectively, and after 50 cycles, the energy efficiency was increased from 67.2% to 72.6% compared with the unmodified graphite felt.
[0082] Example 5
[0083] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0084] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and completely immerse it in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven at 50°C and dry it for 24 h. Then take it out for use.
[0085] (2) Weigh 3 g of copper nitrate hexahydrate, 2.6 g of yttrium nitrate hexahydrate, and 1.5 g of nickel nitrate hexahydrate, add them to 1 L of ethanol, and mechanically stir until the chemicals are completely dissolved to obtain a Cu-Y-Ni mixed solution.
[0086] (3) The graphite felt treated in step (1) is completely immersed in the Cu-Y-Ni mixed solution prepared in step (2) for 12 hours.
[0087] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0088] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm of H2 introduced for 20 min, and then grown in situ at 400°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:20. After the growth was completed, the felt was taken out and cooled to room temperature.
[0089] (6) The graphite felt treated in step (5) is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 1 hour, and after being taken out, it is repeatedly rinsed with deionized water until it becomes neutral, and then dried to obtain a graphite felt composite material.
[0090] The modified polyacrylonitrile-based graphite felt prepared in this embodiment has carbon nanotubes grown on its surface to increase its specific surface area. Compared with the specific surface area of the original graphite felt of 11m 2 g -1 The specific surface area of the modified graphite felt reaches 47m 2 g -1 , carbon nanotube loading 0.43mg / cm 2After being treated with nitric acid, the contact angle was measured to be 0°, which improved the hydrophilicity. It was assembled into a flow battery (the negative electrode electrolyte was prepared by 0.2 mol / L FeCl3, 3 mol / L NaOH, and 2 mol / L TEOA; the positive electrode electrolyte was prepared by 0.2 mol / L K4[Fe(CN)6] and 1 mol / L NaOH; the diaphragm was SPEEK membrane; the graphite plate was used as the current collector), and the flow rate was 100 mA / cm 2 At a current density of 1.5 V and 0.7 V, respectively, after 50 cycles, the energy efficiency was increased from 65.4% to 71.5% compared with the unmodified graphite felt.
[0091] Example 6
[0092] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0093] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and immerse it completely in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven and dry it at 50°C for 24 h. Then take it out for use.
[0094] (2) Weigh 1.5 g of copper nitrate hexahydrate, 3.8 g of yttrium nitrate hexahydrate, and 2 g of nickel nitrate hexahydrate, add them to 1 L of ethanol, and mechanically stir until the chemicals are completely dissolved to obtain a Cu-Y-Ni mixed solution.
[0095] (3) The graphite felt treated in step (1) is completely immersed in the prepared Cu-Y-Ni mixed solution for 24 hours.
[0096] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0097] (5) The graphite felt treated in step (4) was reduced at 100°C with an H2 flow rate of 30 sccm (standard cubic centimeters per minute) for 30 min, and then grown in situ at 600°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:20. After the growth was completed, the felt was taken out and cooled to room temperature.
[0098] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 1 hour, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0099] The modified polyacrylonitrile-based graphite felt prepared in this embodiment has carbon nanotubes grown on its surface to increase its specific surface area. Compared with the specific surface area of the original graphite felt of 11m2 g -1 The specific surface area of the modified graphite felt reaches 52m 2 g -1 , carbon nanotube loading 0.54mg / cm 2 After nitric acid treatment, the contact angle was 0°, which improved the hydrophilicity. It was assembled into a flow battery (the negative electrode electrolyte was prepared by 0.2 mol / L FeCl3, 3 mol / L NaOH, and 2 mol / L TEOA; the positive electrode electrolyte was prepared by 0.2 mol / L K4[Fe(CN)6] and 1 mol / L NaOH; the diaphragm was SPEEK membrane; the graphite plate was used as the current collector), and the flow rate was 50 mA / cm 2 At a current density of 1.5 V and 0.7 V, respectively, after 50 cycles, the energy efficiency was increased from 67.2% to 75.3% compared with the unmodified graphite felt.
[0100] Example 7
[0101] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0102] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and immerse it completely in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven and dry it at 50°C for 24 h. Then take it out for use.
[0103] (2) Weigh 4 g of copper nitrate hexahydrate, 3.8 g of yttrium nitrate hexahydrate, and 6 g of nickel nitrate hexahydrate, add them to 1 L of ethanol, and stir mechanically until the chemicals are completely dissolved to obtain a Cu-YNi mixed solution.
[0104] (3) The graphite felt treated in step (2) is completely immersed in the prepared Cu-Y-Ni mixed solution for 12 hours.
[0105] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0106] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm of H2 introduced for 20 min, and then grown in situ at 500°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0107] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 1 hour, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0108] The modified polyacrylonitrile-based graphite felt prepared in this embodiment has carbon nanotubes grown on its surface to increase its specific surface area. Compared with the specific surface area of the original graphite felt of 11m 2 g -1 The specific surface area of the modified graphite felt reaches 62m 2 g -1 , carbon nanotube loading 0.58mg / cm 2 After nitric acid treatment, the contact angle was 0°, which improved the hydrophilicity. It was assembled into a flow battery (the negative electrode electrolyte was prepared by 0.2 mol / L FeCl3, 3 mol / L NaOH, and 2 mol / L TEOA; the positive electrode electrolyte was prepared by 0.2 mol / L K4[Fe(CN)6] and 1 mol / L NaOH; the diaphragm was SPEEK membrane; the graphite plate was used as the current collector), and the flow rate was 50 mA / cm 2 At a current density of 1.5 V and 0.7 V, respectively, after 50 cycles, the energy efficiency was increased from 67.2% to 76.3% compared with the unmodified graphite felt.
[0109] Example 8
[0110] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0111] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and completely immerse it in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven at 50°C and dry it for 24 h. Then take it out for use.
[0112] (2) Weigh 3 g of copper nitrate hexahydrate, 2.6 g of yttrium nitrate hexahydrate, and 3 g of nickel nitrate hexahydrate, add them to 1 L of ethanol, and mechanically stir until the chemicals are completely dissolved to obtain a Cu-YNi mixed solution.
[0113] (3) The graphite felt treated in step (1) is completely immersed in the Cu-Y-Ni mixed solution prepared in step (2) for 12 hours.
[0114] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0115] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm (standard cubic centimeters per minute) of H2 introduced for 30 min, and then grown in situ at 600°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0116] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 3 h, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0117] The modified polyacrylonitrile-based graphite felt prepared in this embodiment has carbon nanotubes grown on its surface to increase its specific surface area. Compared with the specific surface area of the original graphite felt of 11m 2 g -1 The specific surface area of the modified graphite felt reaches 52m 2 g -1 , carbon nanotube loading 0.54mg / cm 2 After nitric acid treatment, the contact angle was 0°, which improved the hydrophilicity. It was assembled into a flow battery (the negative electrode electrolyte was prepared by 0.2 mol / L FeCl3, 3 mol / L NaOH, and 2 mol / L TEOA; the positive electrode electrolyte was prepared by 0.2 mol / L K4[Fe(CN)6] and 1 mol / L NaOH; the diaphragm was SPEEK membrane; the graphite plate was used as the current collector), and the flow rate was 50 mA / cm 2 At a current density of 1.5 V and 0.7 V, respectively, the charge and discharge voltages were 1.5 V and 0.7 V, respectively, and after 50 cycles, the energy efficiency was increased from 67.2% to 74.2% compared with the unmodified graphite felt.
[0118] Comparative Example 1
[0119] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0120] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and completely immerse it in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven at 50°C and dry it for 24 h. Then take it out for use.
[0121] (2) Weigh 3 g of nickel nitrate hexahydrate, add it to 1 L of ethanol, and stir mechanically until the drug is completely dissolved to obtain a nickel solution.
[0122] (3) The graphite felt treated in step (1) is completely immersed in the nickel solution prepared in step (2) for 12 hours.
[0123] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0124] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm (standard cubic centimeters per minute) of H2 introduced for 30 min, and then grown in situ at 600°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0125] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 3 h, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0126] The modified polyacrylonitrile-based graphite felt prepared in this comparative example catalytically grows carbon nanotubes on the surface. The distribution is uneven visually, and some places have no obvious load. Compared with the original graphite felt with a specific surface area of 11m 2 g -1 The specific surface area of the modified graphite felt was not significantly increased, only reaching 23m 2 g -1 After nitric acid treatment, the contact angle was 0°, which improved the hydrophilicity. It was assembled into a flow battery (the negative electrode electrolyte was prepared by 0.2 mol / L FeCl3, 3 mol / L NaOH, and 2 mol / L TEOA; the positive electrode electrolyte was prepared by 0.2 mol / L K4[Fe(CN)6] and 1 mol / L NaOH; the diaphragm was SPEEK membrane; the graphite plate was used as the current collector), and the flow rate was 50 mA / cm 2 At a current density of , the charge and discharge voltages were 1.5V and 0.7V respectively. After 50 cycles, the energy efficiency was increased from 67.2% to 69% compared with the unmodified graphite felt, which was not a significant improvement.
[0127] Comparative Example 2
[0128] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0129] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and completely immerse it in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven at 50°C and dry it for 24 h. Then take it out for use.
[0130] (2) Weigh 3 g of yttrium nitrate hexahydrate, add it to 1 L of ethanol, and stir mechanically until the drug is completely dissolved to obtain a yttrium solution.
[0131] (3) The graphite felt treated in step (1) is completely immersed in the yttrium solution prepared in step (2) for 12 hours.
[0132] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0133] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm (standard cubic centimeters per minute) of H2 introduced for 30 min, and then grown in situ at 600°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0134] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 3 h, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0135] The modified polyacrylonitrile-based graphite felt prepared in this comparative example had no obvious load observed on the surface, and the growth of carbon nanotubes was unsuccessful, so it was not suitable for use as an electrode.
[0136] Comparative Example 3
[0137] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0138] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and completely immerse it in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven at 50°C and dry it for 24 h. Then take it out for use.
[0139] (2) Weigh 3 g of copper nitrate hexahydrate, add it to 1 L of ethanol, and stir mechanically until the drug is completely dissolved to obtain a copper solution.
[0140] (3) The graphite felt treated in step (1) is completely immersed in the copper solution prepared in step (2) for 12 hours.
[0141] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0142] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm (standard cubic centimeters per minute) of H2 introduced for 30 min, and then grown in situ at 600°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0143] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 3 h, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0144] The modified polyacrylonitrile-based graphite felt prepared in this comparative example has only a small amount of load observed on the surface and the load is unevenly distributed, so it is not suitable for use as an electrode.
[0145] Comparative Example 4
[0146] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0147] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and completely immerse it in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven at 50°C and dry it for 24 h. Then take it out for use.
[0148] (2) Weigh 3 g of copper nitrate hexahydrate and 3 g of yttrium nitrate hexahydrate, add them to 1 L of ethanol, and stir mechanically until the chemicals are completely dissolved to obtain a Cu-Y mixed solution.
[0149] (3) The graphite felt treated in step (1) is completely immersed in the Cu-Y mixed solution prepared in step (2) for 12 hours.
[0150] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0151] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm (standard cubic centimeters per minute) of H2 introduced for 30 min, and then grown in situ at 600°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0152] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 3 h, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0153] The modified polyacrylonitrile-based graphite felt prepared in this comparative example has only a small amount of loading material on the surface of the graphite felt and is not suitable for use as an electrode.
[0154] Comparative Example 5
[0155] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0156] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and completely immerse it in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven at 50°C and dry it for 24 h. Then take it out for use.
[0157] (2) Weigh 3 g of nickel nitrate hexahydrate and 3 g of yttrium nitrate hexahydrate, add them to 1 L of ethanol, and stir mechanically until the chemicals are completely dissolved to obtain a NiY mixed solution.
[0158] (3) The graphite felt treated in step (1) is completely immersed in the NiY mixed solution prepared in step (2) for 12 hours.
[0159] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0160] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm (standard cubic centimeters per minute) of H2 introduced for 30 min, and then grown in situ at 600°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0161] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 3 h, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0162] The modified polyacrylonitrile-based graphite felt prepared in this comparative example has uneven distribution of the load on the surface of the graphite felt and is not suitable for use as an electrode.
[0163] Comparative Example 6
[0164] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0165] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and completely immerse it in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven at 50°C and dry it for 24 h. Then take it out for use.
[0166] (2) Weigh 3 g of nickel nitrate hexahydrate and 3 g of copper nitrate hexahydrate, add them to 1 L of ethanol, and mechanically stir until the chemicals are completely dissolved to obtain a Ni-Cu mixed solution.
[0167] (3) The graphite felt treated in step (1) is completely immersed in the Ni-Cu mixed solution prepared in step (2) for 12 hours.
[0168] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0169] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm (standard cubic centimeters per minute) of H2 introduced for 30 min, and then grown in situ at 600°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0170] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 3 h, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0171] The modified polyacrylonitrile-based graphite felt prepared in this comparative example has a significantly uneven distribution of the load on the surface of the graphite felt, which will affect the test and is not suitable for use as an electrode.
[0172] Comparative Example 7
[0173] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0174] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and completely immerse it in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven at 50°C and dry it for 24 h. Then take it out for use.
[0175] (2) Weigh 0.1 g of copper nitrate hexahydrate, 0.1 g of yttrium nitrate hexahydrate, and 0.1 g of nickel nitrate hexahydrate, add them to 1 L of ethanol, and mechanically stir until the chemicals are completely dissolved to obtain a Ni-Y-Cu mixed solution.
[0176] (3) The graphite felt treated in step (1) is completely immersed in the Ni mixed solution prepared in step (2) for 12 hours.
[0177] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0178] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm (standard cubic centimeters per minute) of H2 introduced for 30 min, and then grown in situ at 600°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0179] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 3 h, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0180] The modified polyacrylonitrile-based graphite felt prepared in this comparative example has too little catalyst, and only a small amount of load is observed on the surface and the distribution is uneven, so it is not suitable for use as an electrode.
[0181] Comparative Example 8
[0182] A modified polyacrylonitrile-based graphite felt, wherein the modification is to in-situ grow carbon nanotubes on the polyacrylonitrile-based graphite felt, and then immerse the felt in a strong acid for corrosion, and the felt is prepared by the following steps:
[0183] (1) Take a piece of graphite felt of 3 cm*3 cm*5 mm and completely immerse it in a beaker filled with acetone. Place the beaker in an ultrasonic cleaner for ultrasonic cleaning for 30 min. Take it out and rinse it with deionized water. Place it in a drying oven at 50°C and dry it for 24 h. Then take it out for use.
[0184] (2) Weigh 20 g of nickel nitrate hexahydrate, 20 g of yttrium nitrate hexahydrate and 20 g of copper nitrate hexahydrate, add them to 1 L of ethanol, and stir mechanically until the drugs are completely dissolved to obtain a NiY mixed solution.
[0185] (3) The graphite felt treated in step (1) is completely immersed in the NiY mixed solution prepared in step (2) for 12 hours.
[0186] (4) Take out the graphite felt treated in step (3) and place it in a drying oven at 50° C. for 12 h.
[0187] (5) The graphite felt treated in step (4) was reduced at 100°C with 30 sccm (standard cubic centimeters per minute) of H2 introduced for 30 min, and then grown in situ at 600°C for 10 min in an atmosphere of H2:Ar:C2H2=30:100:10. After the growth was completed, the felt was taken out and cooled to room temperature.
[0188] (6) The treated graphite felt is completely immersed in concentrated nitric acid (68 wt.%) for chemical corrosion for 3 h, taken out and repeatedly rinsed with deionized water until neutral, and dried to obtain a graphite felt composite material.
[0189] The modified polyacrylonitrile-based graphite felt prepared in this comparative example has a large amount of carbon nanotubes catalytically grown on the surface due to the excess catalyst, and the carbon nanotubes are easily detached from the surface of the graphite felt, so it is not suitable for use as an electrode of a liquid flow battery.
[0190] In summary, the technical solution of the present application adopts chemical vapor deposition to grow carbon nanotubes in situ on the surface of graphite felt. Under the premise of not destroying the mechanical properties of graphite felt, the loading amount of carbon nanotubes per unit area is regulated by controlling the ratio of catalysts, the flow rate of gas introduced and the growth temperature, and the specific surface area of graphite felt is greatly increased without obvious shedding of carbon nanotubes. When assembled into a liquid flow battery, it provides more active sites for the reaction of ions during the charging and discharging process, and then after strong acid corrosion, more oxygen-containing functional groups are introduced to improve the hydrophilicity of the material, thereby achieving the purpose of improving the energy efficiency of the liquid flow battery.
[0191] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A modified graphite felt, characterized in that: The invention comprises graphite felt and carbon nanotubes grown in situ on the surface of the graphite felt; preferably, the loading amount of the carbon nanotubes is greater than 0.48 mg / cm 2 ; preferably 0.48-0.65mg / cm 2 The specific surface area of the modified graphite felt is greater than 46m 2 g -1 ; preferably 46-62m 2 g -1 ; Preferably, the contact angle of the modified graphite felt is 0°.
2. A method for preparing the modified graphite felt according to claim 1, characterized in that: The steps include: 1) In-situ growth of carbon nanotubes on graphite felt using chemical vapor deposition; 2) Add strong acid for corrosion.
3. The method for preparing modified graphite felt according to claim 2, characterized in that: The specific steps of step 1) are: 1).1 Add graphite felt into the catalyst solution for impregnation and drying; 1).2 The dried graphite felt is reduced in hydrogen; 1).3 The reduced graphite felt is in-situ grown in a mixture of inert gas, hydrogen and carbon source gas to obtain graphite felt with carbon nanotubes grown on the surface.
4. The method for preparing modified graphite felt according to claim 3, characterized in that: In step 1.1), the graphite felt is pre-treated, and the specific steps are: the graphite felt is completely immersed in acetone for ultrasonic cleaning to remove surface impurities; then washed with deionized water and placed in a drying oven for drying; preferably, the graphite felt is polyacrylonitrile-based graphite felt.
5. The method for preparing modified graphite felt according to claim 3, characterized in that: Preferably, the catalyst solution in step 1.1) is a mixture aqueous solution of copper salt, yttrium salt and nickel salt; Preferably, the molar ratio of the copper salt, yttrium salt and nickel salt is (0.001-0.04): (0.001-0.03): (0.001-0.04); preferably (0.005-0.014): (0.003-0.01): (0.005-0.021); Preferably, the copper salt, yttrium salt and nickel salt are all nitrates.
6. The method for preparing modified graphite felt according to claim 3, characterized in that: In step 1.2), the amount of hydrogen introduced is (10-60) sccm; Preferably, the reduction temperature is 100-500° C. and the time is 1-120 min.
7. The method for preparing modified graphite felt according to claim 3, characterized in that: In step 1.3), the ratio of the amount of hydrogen, inert gas and carbon source gas introduced is: (10-50): (50-300): (5-30); preferably (10-30): 100: (10-20); Preferably, the in-situ growth temperature is 100-800°C and the time is 10-80 min; preferably, the growth temperature is 400-600°C and the time is 10 min; Preferably, the inert gas is Ar; and the carbon source gas is C2H2.
8. The method for preparing modified graphite felt according to claim 2, characterized in that: The strong acid in step 2) is concentrated nitric acid; the specific steps of step 2) are: the graphite felt treated in step 1) is completely immersed in concentrated nitric acid for chemical corrosion for 1-5 hours, taken out and repeatedly rinsed with deionized water until neutral, and then dried to obtain the modified graphite felt.
9. A liquid flow battery, characterized in that: The modified graphite felt according to claim 1 is used as an electrode, a positive electrode electrolyte, a negative electrode electrolyte and a separator.
10. The liquid flow battery according to claim 9, characterized in that: The negative electrode electrolyte includes FeCl3, NaOH, and TEOA; the positive electrode electrolyte includes K4[Fe(CN)6] and NaOH; and the diaphragm is a SPEEK membrane.
Citation Information
Cited By
Three-dimensional carbon nanotube modified graphite felt as well as preparation method and application thereof
CN120767345A