Liquid crystal polyester resin, liquid crystal polyester resin composition, and molded article formed therefrom

By adjusting the proportions of aromatic hydroxycarboxylic acid, aromatic diol and aromatic dicarboxylic acid in the liquid crystal polyester resin, and controlling the temperature sensitivity coefficient and curing start temperature, the problems of dripping, drawing and gas during molding of the liquid crystal polyester resin are solved. problem, achieving molding stability and flow consistency over a wide range of temperatures, suitable for the production of small electrical/electronic components.

CN118871499APending Publication Date: 2024-10-29TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026674.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-05-26
Filing Date
2023-04-07
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing liquid crystal polyester resins are prone to dripping, stringing or gas generation during molding, resulting in reduced productivity and quality of molded products. Molding stability and fluidity are highly dependent on thickness, making it difficult to achieve a wide range of molding temperatures. Molding with excellent stability.

Method used

A liquid crystal polyester resin containing 15 to 80 mol% of aromatic hydroxycarboxylic acid, 2 to 40 mol% of aromatic diol and 2 to 40 mol% of aromatic dicarboxylic acid is used, and the temperature sensitivity coefficient and curing start are controlled. temperature, ensuring that the liquid crystal polyester resin has excellent molding stability and small fluidity thickness dependence over a wide range of molding temperatures.

Benefits of technology

It achieves efficient molding under a wide range of molding temperatures, improves the consistency of molding stability and fluidity, and is suitable for the production of small electrical/electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118871499A_ABST
    Figure CN118871499A_ABST
Patent Text Reader

Abstract

The present invention provides a liquid crystal polyester resin containing a structural unit derived from an aromatic hydroxycarboxylic acid, a structural unit derived from an aromatic diol, and a structural unit derived from an aromatic dicarboxylic acid, the content of the structural unit derived from the aromatic hydroxycarboxylic acid being 15-80 mol% with respect to 100 mol% of all the structural units of the liquid crystal polyester resin, and the content of the structural unit derived from the aromatic diol being 10-80 mol% with respect to 100 mol% of all the structural units of the liquid crystal polyester resin. The content of a structural unit derived from an aromatic diol is 2-40 mol%, the content of a structural unit derived from an aromatic dicarboxylic acid is 2-40 mol%, and the temperature sensing coefficient and the curing initiation temperature obtained from a rheology spectrum are within certain ranges. The liquid crystal polyester resin can be molded over a wide range of molding temperatures, has excellent molding stability, and has little thickness dependence of fluidity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a liquid crystal polyester resin, a liquid crystal polyester resin composition and a molded product formed therefrom. Background Art

[0002] Since liquid crystal polyester resins have excellent heat resistance, fluidity and dimensional stability, they are used in electrical / electronic components that require these characteristics. In recent years, due to the miniaturization of smartphones, etc., there is a further demand for high integration, thin-walled, low-height, etc. of components. For example, it has been proposed to use liquid crystal polyester resins containing structural units derived from p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 4,4'-dihydroxybiphenyl, hydroquinone and terephthalic acid (for example, Patent Documents 1 to 4), liquid crystal polyester resins containing structural units derived from p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 4,4'-dihydroxybiphenyl, terephthalic acid and isophthalic acid (for example, Patent Document 5), liquid crystal polyester resins containing structural units derived from p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, hydroquinone, terephthalic acid and isophthalic acid (for example, Patent Document 6), which have excellent fluidity while taking into account high strength, anti-foaming, etc. In addition, it has been proposed to achieve both rigidity and retention stability by using a liquid crystal polyester resin containing structural units derived from p-hydroxybenzoic acid, 4,4′-dihydroxybiphenyl, hydroquinone, terephthalic acid, and isophthalic acid (for example, Patent Documents 7 and 8).

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2021-24985

[0006] Patent Document 2: Japanese Patent Application Publication No. 2017-137438

[0007] Patent Document 3: International Publication No. 2018 / 101214

[0008] Patent Document 4: Japanese Patent Application Publication No. 2012-126842

[0009] Patent Document 5: International Publication No. 2012 / 137636

[0010] Patent Document 6: International Publication No. 2013 / 51346

[0011] Patent Document 7: Japanese Patent Application No. 2016-523291

[0012] Patent Document 8: Japanese Patent Application Publication No. 2004-256656 Summary of the invention

[0013] Problems to be solved by the invention

[0014] However, when the molding temperature is high, resins with excellent fluidity may produce dripping (a phenomenon in which the resin leaks from the front end of the nozzle and droops during molding), stringing (a phenomenon in which the resin that is not completely solidified extends in a filamentary form from the top of the sprue when the mold is opened), or gas during molding, which may lead to a decrease in productivity and, therefore, a decrease in the quality of the molded product. In order to prevent such problems, the molding temperature is sometimes lowered, but in the techniques described in the above-mentioned patent documents 1 to 8, if the molding temperature is excessively lowered, part of the resin solidifies, which easily leads to a deviation in fluidity and a narrow molding temperature range. In addition, since the fluidity is highly dependent on thickness, when molding molded products with different thicknesses, there is a problem in which fluidity deviation is easily generated. In addition, in production based on injection molding, the molding machine is repeatedly stopped and restarted (restored) due to product switching, molding failures, etc., so it is important to shorten the time required to obtain a good product after recovery and improve molding stability. The methods described in patent documents 1 to 8 have problems in molding stability.

[0015] An object of the present invention is to provide a liquid crystal polyester resin, a liquid crystal polyester resin composition, and a molded article formed therefrom, which can be molded at a wide range of molding temperatures, has excellent molding stability, and has low thickness dependence of fluidity.

[0016] Means of solving the problem

[0017] The present inventors have repeatedly conducted intensive studies to solve the above-mentioned problems. As a result, they have found that a liquid crystal polyester resin containing 15 to 80 mol % of structural units derived from aromatic hydroxycarboxylic acids, 2 to 40 mol % of structural units derived from aromatic diols, and 2 to 40 mol % of structural units derived from aromatic dicarboxylic acids, relative to 100 mol % of all structural units of the liquid crystal polyester resin, and a liquid crystal polyester resin in which the temperature sensitivity coefficient and the curing start temperature described later are controlled, can be molded at a wide range of molding temperatures, has excellent molding stability, and has low thickness dependence of fluidity, thereby completing the present invention.

[0018] That is, the present invention is as follows:

[0019] (1) A liquid crystal polyester resin comprising a structural unit derived from an aromatic hydroxycarboxylic acid, a structural unit derived from an aromatic diol, and a structural unit derived from an aromatic dicarboxylic acid, wherein the content of the structural unit derived from the aromatic hydroxycarboxylic acid is 15 to 80 mol%, the content of the structural unit derived from the aromatic diol is 2 to 40 mol%, and the content of the structural unit derived from the aromatic dicarboxylic acid is 2 to 40 mol%, relative to 100 mol% of all structural units of the liquid crystal polyester resin, and the following condition (α) is satisfied:

[0020] (α): The temperature sensitivity coefficient measured as follows is less than 0.020, and B(x) is -35 to -15°C;

[0021] When the melting point of the liquid crystal polyester resin is set to Tm (°C), the liquid crystal polyester resin is measured using a rheometer as follows. In the rheological spectrum curve of the liquid crystal polyester resin obtained by setting the x-axis to ΔT (°C) = measurement temperature - Tm (°C) and the y-axis to the logarithm of the complex viscosity (log (η (Pa·s))), the point where ΔT = 20°C is set as point A, the point where ΔT = 10°C is set as point A', and the point below the melting point and the complex viscosity η is 10000 Pa·s is set as point C , the point where the complex viscosity η is 5000 Pa·s is set as point C', the straight line passing through point A and point A' is set as straight line t, the straight line passing through point C and point C' is set as straight line u, the intersection of straight line t and straight line u is set as point B', the straight line passing through point B' and parallel to the y-axis is set as straight line v, the intersection of straight line v and the rheological spectrum curve is set as point B, the absolute value of the slope of the straight line w connecting point A and point B is defined as the temperature sensitivity coefficient, and the ΔT value of point B is defined as B(x);

[0022] The above rheological spectrum curve is obtained by setting the gap between parallel plates to 1 mm, the strain to 10% and the frequency to 1 Hz in the vibration measurement mode of the rheometer, maintaining the temperature at Tm+30°C for 5 minutes, and then cooling the temperature at 0.17°C / sec to a temperature at which the complex viscosity reaches 50,000 (Pa·s);

[0023] The melting point Tm of the above-mentioned liquid crystal polyester resin is the endothermic peak temperature Tm1 observed when the liquid crystal polyester resin is heated from room temperature at a heating condition of 20°C / min in differential calorimetry, then maintained at a temperature of Tm1+20°C for 5 minutes, then temporarily cooled to room temperature at a cooling condition of 20°C / min, and heated again at a heating condition of 20°C / min.

[0024] (2) The liquid crystal polyester resin according to claim 1, comprising a structural unit selected from the following structural units (I) to (V), and satisfying the following conditions (a) to (d):

[0025] 25≤[I]≤75 ···(a)

[0026] 1≤[II]≤20 ···(b)

[0027] 2≤[III]+[IV]≤35···(c)

[0028] 2≤[V]≤35···(d)

[0029] [I] to [V] represent the content (mol %) of each of the following structural units (I) to (V) relative to 100 mol % of all structural units of the liquid crystal polyester resin.

[0030]

[0031] (3) The liquid crystal polyester resin according to claim 1 or 2, comprising the following structural units (II) and (VI), and satisfying the following conditions (e) and (f):

[0032] 0.01≤[VI]≤10 ···(e)

[0033] [VI] / [II]<1 ···(f)

[0034] [II] and [VI] represent the content (mol %) of each of the following structural units (II) and (VI), respectively, relative to 100 mol % of all structural units of the liquid crystal polyester resin.

[0035]

[0036] (4) The liquid crystal polyester resin according to any one of claims 1 to 3, comprising a structural unit selected from the following structural units (I) to (VI), and satisfying the following conditions (g) to (l):

[0037] 25≤[I]≤75 ···(g)

[0038] 1≤[II]≤20 ···(h)

[0039] 2≤[III]+[IV]≤35···(i)

[0040] 2≤[V]≤35 ···(j)

[0041] 0.01≤[VI]≤10 ···(k)

[0042] [VI] / [II]<1 ···(l)

[0043] [I] to [VI] represent the content (mol %) of each of the following structural units (I) to (VI) relative to 100 mol % of all structural units of the liquid crystal polyester resin.

[0044]

[0045] (5) The liquid crystal polyester resin according to any one of claims 1 to 4, further satisfying the following condition (m):

[0046] 0<[III] / [IV]<1.5···(m)

[0047] [III] and [IV] represent the content (mol %) of each of the structural units (III) and (IV) relative to 100 mol % of all structural units of the liquid crystal polyester resin.

[0048] (6) The liquid crystal polyester resin according to any one of claims 1 to 5, further satisfying the following condition (n):

[0049] 99≤[I]+[II]+[III]+[IV]+[V]+[VI]≤100···(n)

[0050] [I] to [VI] represent the content (mol %) of each of the above-mentioned structural units (I) to (VI) relative to 100 mol % of all structural units of the liquid crystal polyester resin.

[0051] (7) A liquid crystal polyester resin composition comprising 10 to 200 parts by weight of a filler based on 100 parts by weight of the liquid crystal polyester resin according to any one of (1) to (6).

[0052] (8) A molded article comprising the liquid crystal polyester resin according to any one of (1) to (6) or the liquid crystal polyester resin composition according to (7).

[0053] (9) The molded article according to (8), wherein the molded article is any one selected from a connector, a relay, a switch, a coil bobbin, and an actuator element of a camera module.

[0054] Effects of the Invention

[0055] The liquid crystal polyester resin of the present invention can be molded at a wide range of molding temperatures, has excellent molding stability, and has low thickness dependence of fluidity. The liquid crystal polyester resin of the present invention is particularly suitable for molding small electrical / electronic components and the like. BRIEF DESCRIPTION OF THE DRAWINGS

[0056] Figure 1 This is a rheological spectrum graph illustrating the condition (α) satisfied by the liquid crystal polyester resin of the present invention.

[0057] Figure 2 The graphs are rheological spectra of the present invention and conventional liquid crystal polyester resins.

[0058] Figure 3 This is a perspective view showing a connector molded product used for evaluation of molding stability. DETAILED DESCRIPTION

[0059] Hereinafter, the present invention will be described in detail.

[0060] <Liquid Crystal Polyester Resin>

[0061] Liquid crystal polyester resins are polyesters that form an anisotropic melt phase. Examples of such polyester resins include polyesters composed of structural units selected from oxycarbonyl units, dioxy units, dicarbonyl units, etc. described below so as to form an anisotropic melt phase.

[0062] Next, the temperature sensitivity of the liquid crystal polyester resin obtained from the rheological curve will be described. The liquid crystal polyester resin of the present invention satisfies the following condition (α).

[0063] (α): The temperature sensitivity coefficient measured as follows is less than 0.020, and B(x) is -35 to -15°C;

[0064] based on Figure 1 The above temperature sensitivity coefficient and the method for calculating B(x) are described below. When the melting point of the liquid crystal polyester resin is set to Tm(℃), the liquid crystal polyester resin is measured using a rheometer as follows, and the x-axis is set to ΔT(℃) = measurement temperature - Tm(℃), and the y-axis is set to the logarithm of the complex viscosity (log(η(Pa·s))), and the following is obtained: Figure 1 The rheological spectrum curve 1 of the liquid crystal polyester resin shown. In the rheological spectrum curve 1, the point where ΔT=20°C is set as point A, the point where ΔT=10°C is set as point A', the point below the melting point and the complex viscosity η is set as point C, and the point where the complex viscosity η is 5000 Pa·s is set as point C'. When the straight line passing through point A and point A' is set as straight line t, the straight line passing through point C and point C' is set as straight line u, the intersection of straight line t and straight line u is set as point B', the straight line passing through point B' and parallel to the y-axis is set as straight line v, and the intersection of straight line v and the rheological spectrum curve is set as point B, the absolute value of the slope of the straight line w connecting point A and point B is defined as the temperature sensitivity coefficient, and the ΔT value of point B is defined as B(x).

[0065] The above rheological spectrum curve is obtained by setting the gap between parallel plates to 1 mm, the strain to 10% and the frequency to 1 Hz in the vibration measurement mode of the rheometer, maintaining the temperature at Tm+30°C for 5 minutes, and then cooling the temperature at 0.17°C / sec to a temperature at which the complex viscosity reaches 50,000 (Pa·s);

[0066] The melting point Tm of the above-mentioned liquid crystal polyester resin is the endothermic peak temperature Tm1 observed when the liquid crystal polyester resin is heated from room temperature at a heating condition of 20°C / min in differential calorimetry, then maintained at a temperature of Tm1+20°C for 5 minutes, then temporarily cooled to room temperature at a cooling condition of 20°C / min, and heated again at a heating condition of 20°C / min.

[0067] Rheometer measurement is a method for evaluating the rheological properties (flow properties) as one of the important properties of a resin. The above-mentioned temperature sensitivity coefficient is a coefficient obtained from the rheometer spectrum as described above, and is a value defined by the absolute value of the slope of the straight line w connecting point A and point B. The temperature sensitivity coefficient indicates the magnitude of the change in the dynamic viscosity (complex viscosity) of the liquid crystal polyester resin relative to the temperature under shear conditions. The lower the temperature sensitivity coefficient, the more difficult it is for the liquid crystal polyester resin to change its flow properties for external factors such as temperature and shear. In the present invention, it is found that, in particular, liquid crystal polyester resins with a temperature sensitivity coefficient of 0.020 or less can be molded at a wide range of molding temperatures, have excellent molding stability, and have a small thickness dependence of fluidity. If the temperature sensitivity coefficient is greater than 0.020, it is difficult to control the behavior of the liquid crystal polyester resin from melting to solidification, the temperature range that can be molded becomes narrower, and the thickness dependence of the fluidity becomes larger. In addition, for liquid crystal polyester resins with a temperature sensitivity coefficient higher than 0.020, slight differences in the temperatures of various parts of the molding machine will cause changes in fluidity, so it takes time from the stop of the molding machine to the recovery of a good product, and the molding stability is reduced. In view of the molding temperature range, molding stability and thickness dependence of fluidity, the temperature sensitivity coefficient is preferably 0.018 or less, and more preferably 0.016 or less. It should be noted that the lower the temperature sensitivity coefficient, the better, and the lowest value is 0.

[0068] Furthermore, the value B(x) of ΔT of the point B shown in the above condition (α) of the liquid crystal polyester resin of the present invention is -35 to -15°C. B(x) is the temperature at which the liquid crystal polyester resin begins to solidify under shear conditions (hereinafter, B(x) is sometimes recorded as the solidification start temperature). When B(x) is lower than -35°C, burrs during molding and dripping from the front end of the nozzle become problems, and the temperature range in which molding can be performed becomes narrower. In addition, when B(x) is greater than -15°C, it is difficult to control the curing behavior of the liquid crystal polyester resin, the temperature range in which molding can be performed becomes narrower, the molding stability is poor, and the thickness dependence of the fluidity becomes greater. B(x) is preferably above -30°C, and more preferably above -28°C. In addition, B(x) is preferably below -16°C, more preferably below -18°C, and further preferably below -20°C.

[0069] Figure 2 An example of the rheological spectrum curve of the liquid crystal polyester resin of the present invention (S1) and an example of the rheological spectrum curve of the conventional liquid crystal polyester resin (S2) are shown. In addition, straight lines L1 and L2 representing the temperature sensitivity coefficient defined above are respectively shown. Figure 2 As shown, it can be seen that the absolute value of the slope of L1 is smaller than that of L2, and the temperature sensitivity coefficient of the liquid crystal polyester resin of the present invention is smaller than the temperature sensitivity coefficient of the conventional liquid crystal polyester resin.

[0070] If Figure 2By comparing the spectrum curves of S1 and S2 in the above, it can be seen that the viscosity change of S1 is suppressed above the curing start temperature B(x), and as the temperature decreases, the viscosity rises sharply from near the curing start temperature. The liquid crystal polyester resin of the present invention that shows the viscosity change behavior of S1 can be molded at a wide range of molding temperatures, and has the characteristics of excellent molding stability and low thickness dependence of fluidity. The value that quantitatively shows that the rheological spectrum curve is the same shape as S1 is the temperature sensitivity coefficient defined above.

[0071] As a method for controlling the above-mentioned temperature sensitivity coefficient and curing start temperature within an appropriate range, for example, the structural unit constituting the liquid crystal polyester resin is set to a preferred range described later, and / or the method for producing the liquid crystal polyester resin is set to a preferred method described later. The details are described in the structural unit constituting the liquid crystal polyester resin below and the "method for producing the liquid crystal polyester resin" described later.

[0072] Next, the structural units constituting the liquid crystal polyester resin will be described.

[0073] The liquid crystal polyester resin of the present invention comprises a structural unit derived from an aromatic hydroxycarboxylic acid, a structural unit derived from an aromatic diol, and a structural unit derived from an aromatic dicarboxylic acid.

[0074] The liquid crystal polyester resin of the present invention, as an oxycarbonyl unit, contains 15 to 80 mol% of a structural unit derived from an aromatic hydroxycarboxylic acid relative to 100 mol% of all structural units of the liquid crystal polyester resin. When the content of the structural unit derived from the aromatic hydroxycarboxylic acid is less than 15%, the liquid crystallinity is impaired, and therefore, the temperature range in which molding can be performed becomes narrower. The content is preferably 20 mol% or more, more preferably 25 mol% or more. On the other hand, if the content is more than 80 mol%, it becomes difficult to control the crystallinity and melting point of the liquid crystal polyester resin, and the temperature range in which molding can be performed becomes narrower. The content is preferably 75 mol% or less, more preferably 70 mol% or less. As a specific example of a structural unit derived from an aromatic hydroxycarboxylic acid, a structural unit derived from p-hydroxybenzoic acid, m-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, etc. can be used.

[0075] The liquid crystal polyester resin of the present invention, as a dioxy unit, contains 2 to 40 mol% of a structural unit derived from an aromatic diol relative to 100 mol% of all structural units of the liquid crystal polyester resin. If the content of the structural unit derived from the aromatic diol is less than 2 mol%, the control of the crystallinity and melting point of the liquid crystal polyester resin becomes difficult, and the temperature range in which molding can be performed becomes narrower. The content is preferably 7 mol% or more, more preferably 10 mol% or more. On the other hand, when the content is more than 40 mol%, the liquid crystallinity is impaired, and therefore the temperature range in which molding can be performed becomes narrower. The content is preferably 37 mol% or less, more preferably 35 mol% or less. Examples of the structural unit derived from the aromatic diol include structural units derived from 4,4'-dihydroxybiphenyl, hydroquinone, resorcinol, tert-butylhydroquinone, phenylhydroquinone, chlorohydroquinone, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 3,4'-dihydroxybiphenyl, 2,2-bis(4-hydroxyphenyl)propane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxybenzophenone, etc. From the viewpoint of excellent availability and excellent molding temperature range, it is preferable to use a structural unit derived from 4,4'-dihydroxybiphenyl or hydroquinone.

[0076] The liquid crystal polyester resin of the present invention, as a dicarbonyl unit, contains 2 to 40 mol% of a structural unit derived from an aromatic dicarboxylic acid relative to 100 mol% of all structural units of the liquid crystal polyester resin. If the content of the structural unit derived from the aromatic dicarboxylic acid is less than 2 mol%, it becomes difficult to control the crystallinity and melting point of the liquid crystal polyester resin, and the temperature range in which molding can be performed becomes narrower. The content is preferably 7 mol% or more, more preferably 10 mol% or more. On the other hand, when the content is more than 40 mol%, the liquid crystallinity is impaired, and therefore the temperature range in which molding can be performed becomes narrower. The content is preferably 37 mol% or less, more preferably 35 mol% or less. Examples of the structural unit derived from an aromatic dicarboxylic acid include structural units derived from terephthalic acid, isophthalic acid, 2,6-naphthalene dicarboxylic acid, 4,4'-diphenyl dicarboxylic acid, 3,3'-diphenyl dicarboxylic acid, 2,2'-diphenyl dicarboxylic acid, 1,2-bis(phenoxy)ethane-4,4'-dicarboxylic acid, 1,2-bis(2-chlorophenoxy)ethane-4,4'-dicarboxylic acid, and 4,4'-diphenyl ether dicarboxylic acid. In view of excellent availability and excellent molding temperature range, it is preferred to contain a structural unit derived from terephthalic acid or isophthalic acid.

[0077] Next, the structural units constituting the liquid crystal polyester resin are described in more detail. From the perspective of being able to be molded at a wide range of molding temperatures, having excellent molding stability, and having low thickness dependence of fluidity, the liquid crystal polyester resin of the present invention preferably comprises a structural unit selected from the following structural units (I) to (V), and satisfies the following conditions (a) to (d).

[0078] 25≤[I]≤75 ···(a)

[0079] 1≤[II]≤20 ···(b)

[0080] 2≤[III]+[IV]≤35···(c)

[0081] 2≤[V]≤35···(d)

[0082] [I] to [V] represent the content (mol %) of each of the following structural units (I) to (V) relative to 100 mol % of all structural units of the liquid crystal polyester resin.

[0083]

[0084] The liquid crystal polyester resin of the present invention preferably contains 25 mol% or more of the structural unit (I) as an oxycarbonyl unit relative to 100 mol% of all structural units of the liquid crystal polyester resin. The structural unit (I) is a structural unit derived from p-hydroxybenzoic acid. From the perspective of being able to be molded at a wide range of molding temperatures, excellent molding stability, and low thickness dependence of fluidity, the content of the structural unit (I) is more preferably 35 mol% or more, and further preferably 45 mol% or more.

[0085] On the other hand, the liquid crystal polyester resin of the present invention preferably contains 75 mol% or less of the structural unit (I) relative to 100 mol% of all structural units of the liquid crystal polyester resin. From the perspective of being able to be molded at a wide range of molding temperatures, having excellent molding stability, and having low thickness dependence of fluidity, the content of the structural unit (I) is preferably 65 mol% or less, and more preferably 55 mol% or less.

[0086] The liquid crystal polyester resin of the present invention preferably contains 1 mol% or more of the structural unit (II) as an oxycarbonyl unit relative to 100 mol% of all structural units of the liquid crystal polyester resin. The structural unit (II) is a structural unit derived from 6-hydroxy-2-naphthoic acid. From the perspective of being able to be molded at a wide range of molding temperatures, excellent molding stability, and low thickness dependence of fluidity, the content of the structural unit (II) is preferably 2 mol% or more, more preferably 3 mol% or more.

[0087] On the other hand, the liquid crystal polyester resin of the present invention preferably contains 20 mol% or less of the structural unit (II) relative to 100 mol% of all structural units of the liquid crystal polyester resin. From the perspective of being able to be molded at a wide range of molding temperatures, having excellent molding stability, and having low thickness dependence of fluidity, the content of the structural unit (II) is preferably 15 mol% or less, more preferably 10 mol% or less.

[0088] The liquid crystal polyester resin of the present invention preferably has a molar ratio ([I] / [II]) of the contents of the structural units (I) and (II) of 3 or more, more preferably 5 or more, and even more preferably 7 or more, from the viewpoints of being moldable over a wide range of molding temperatures, having excellent molding stability, and having low thickness dependence of fluidity. On the other hand, from the viewpoints of being moldable over a wide range of molding temperatures and having low thickness dependence of fluidity, [I] / [II] is preferably 20 or less, more preferably 18 or less, and even more preferably 16 or less.

[0089] Furthermore, as the oxycarbonyl unit, a structural unit derived from m-hydroxybenzoic acid or the like may be used within a range not impairing the effects of the present invention.

[0090] The liquid crystal polyester resin of the present invention preferably includes a structural unit (III) as a dioxy unit. The structural unit (III) is a structural unit derived from 4,4'-dihydroxybiphenyl. From the perspective of being able to be molded at a wide range of molding temperatures, excellent molding stability, and having a small thickness dependence of fluidity, the content of the structural unit (III) is preferably 1 mol% or more, more preferably 3 mol% or more, and further preferably 5 mol% or more relative to 100 mol% of all structural units of the liquid crystal polyester resin. On the other hand, from the perspective of being able to be molded at a wide range of molding temperatures and having a small thickness dependence of fluidity, the content of the structural unit (III) is preferably 25 mol% or less, more preferably 20 mol% or less, and more preferably 15 mol% or less.

[0091] The liquid crystal polyester resin of the present invention preferably includes a structural unit (IV) as a dioxy unit. The structural unit (IV) is a structural unit derived from hydroquinone. From the perspective of being able to be molded at a wide range of molding temperatures, excellent molding stability, and a small thickness dependence of fluidity, relative to 100 mol% of all structural units of the liquid crystal polyester resin, the content of the structural unit (IV) is preferably 1 mol% or more, more preferably 4 mol% or more, and further preferably 7 mol% or more. On the other hand, from the perspective of being able to be molded at a wide range of molding temperatures, excellent molding stability, and a small thickness dependence of fluidity, the content of the structural unit (IV) is preferably 30 mol% or less, more preferably 25 mol% or less, and more preferably 20 mol% or less.

[0092] The liquid crystal polyester resin of the present invention preferably has a total content of structural units (III) and (IV) of 2 mol% or more relative to 100 mol% of all structural units of the liquid crystal polyester resin. From the perspective of being able to be molded at a wide range of molding temperatures, having excellent molding stability, and having low thickness dependence of fluidity, the total content of structural units (III) and (IV) is preferably 5 mol% or more, more preferably 10 mol% or more, and even more preferably 15 mol% or more.

[0093] On the other hand, in the liquid crystal polyester resin of the present invention, the total content of the structural units (III) and (IV) is preferably 35 mol% or less relative to 100 mol% of all structural units of the liquid crystal polyester resin. From the perspectives of being able to be molded at a wide range of molding temperatures, excellent molding stability, and low thickness dependence of fluidity, the total content of the structural units (III) and (IV) is preferably 30 mol% or less, more preferably 25 mol% or less.

[0094] The liquid crystal polyester resin of the present invention preferably has a molar ratio ([III] / [IV]) of the contents of the structural units (III) and (IV) greater than 0, more preferably greater than 0.3, and further preferably greater than 0.6, from the viewpoint that the liquid crystal polyester resin can be molded at a wide range of molding temperatures, has excellent molding stability, and has a low thickness dependence of fluidity. On the other hand, from the viewpoint that the liquid crystal polyester resin can be molded at a wide range of molding temperatures, and has a low thickness dependence of fluidity, [III] / [IV] is preferably less than 1.5, more preferably less than 1.2, and further preferably less than 1.0.

[0095] As the dioxy unit, there may be used a structural unit derived from an aromatic diol such as resorcinol, tert-butylhydroquinone, phenylhydroquinone, chlorohydroquinone, 2,6-dihydroxynaphthalene, 2,7-dihydroxynaphthalene, 3,4'-dihydroxybiphenyl, 2,2-bis(4-hydroxyphenyl)propane, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfide, 4,4'-dihydroxybenzophenone; a structural unit derived from an aliphatic diol such as ethylene glycol, propylene glycol, 1,4-butanediol, 1,6-hexanediol, neopentyl glycol; or a structural unit derived from an alicyclic diol such as 1,4-cyclohexanediol and 1,4-cyclohexanedimethanol.

[0096] The liquid crystal polyester resin of the present invention preferably contains 2 mol% or more of the structural unit (V) as a dicarbonyl unit relative to 100 mol% of all structural units of the liquid crystal polyester resin. The structural unit (V) is a structural unit derived from terephthalic acid. From the perspective of being able to be molded at a wide range of molding temperatures, excellent molding stability, and low thickness dependence of fluidity, the content of the structural unit (V) is preferably 5 mol% or more, more preferably 10 mol% or more, and further preferably 15 mol% or more.

[0097] On the other hand, the liquid crystal polyester resin of the present invention preferably contains 35 mol% or less of the structural unit (V) relative to 100 mol% of all structural units of the liquid crystal polyester resin. From the perspective of being able to be molded at a wide range of molding temperatures, excellent molding stability, and low thickness dependence of fluidity, the content of the structural unit (V) is preferably 30 mol% or less, more preferably 25 mol% or less.

[0098] Furthermore, the liquid crystal polyester resin of the present invention more preferably contains the following structural units (II) and (VI), and satisfies the following conditions (e) and (f).

[0099] 0.01≤[VI]≤10 ···(e)

[0100] [VI] / [II]<1 ···(f)

[0101] [II] and [VI] represent the content (mol %) of each of the following structural units (II) and (VI), respectively, relative to 100 mol % of all structural units of the liquid crystal polyester resin.

[0102]

[0103] The liquid crystal polyester resin of the present invention preferably contains 0.01 mol% or more of the structural unit (VI) as a dicarbonyl unit relative to 100 mol% of all structural units of the liquid crystal polyester resin. The structural unit (VI) is a structural unit derived from isophthalic acid. From the perspective of being able to be molded at a wide range of molding temperatures, having excellent molding stability, and having low thickness dependence of fluidity, the content of the structural unit (VI) is preferably 0.05 mol% or more, and more preferably 0.1 mol% or more.

[0104] On the other hand, the liquid crystal polyester resin of the present invention preferably contains 10 mol% or less of the structural unit (VI) relative to 100 mol% of all structural units of the liquid crystal polyester resin. Considering that it can be molded at a wide range of molding temperatures, has excellent molding stability, and has low thickness dependence of fluidity, the content of the structural unit (VI) is preferably 7 mol% or less, and more preferably 4 mol% or less.

[0105] In addition, as the dicarbonyl unit, a structural unit derived from an aromatic dicarboxylic acid such as 2,6-naphthalene dicarboxylic acid, 4,4'-diphenyl dicarboxylic acid, 3,3'-diphenyl dicarboxylic acid, 2,2'-diphenyl dicarboxylic acid, 1,2-bis(phenoxy)ethane-4,4'-dicarboxylic acid, 1,2-bis(2-chlorophenoxy)ethane-4,4'-dicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid; a structural unit derived from an aliphatic dicarboxylic acid such as adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, hexahydroterephthalic acid; and a structural unit derived from an alicyclic dicarboxylic acid such as 1,4-cyclohexane dicarboxylic acid and 1,3-cyclohexane dicarboxylic acid can be used within a range that does not impair the effects of the present invention.

[0106] In the liquid crystal polyester resin of the present invention, the molar ratio of the content of the structural unit (VI) to that of (II) ([VI] / [II]) is preferably less than 1. From the perspective of being able to be molded at a wide range of molding temperatures, having excellent molding stability, and having a low thickness dependence of fluidity, the molar ratio of the content of the structural unit (VI) to that of (II) ([VI] / [II]) is preferably 0.9 or less. On the other hand, the lower limit of [VI] / [II] is not particularly limited, but is preferably 0.005 or more. From the perspective of being able to be molded at a wide range of molding temperatures and having a low thickness dependence of fluidity, [VI] / [II] is preferably 0.01 or more, and more preferably 0.05 or more.

[0107] The liquid crystal polyester resin of the present invention is more preferably a liquid crystal polyester resin containing all of the following structural units (I) to (VI) and satisfying the following conditions (g) to (l), from the viewpoints that the above-mentioned temperature sensitivity coefficient and curing start temperature can be more easily controlled within an appropriate range, can be molded at a wide range of molding temperatures, has excellent molding stability, and further reduces the thickness dependence of fluidity.

[0108] 25≤[I]≤75 ···(g)

[0109] 1≤[II]≤20 ···(h)

[0110] 2≤[III]+[IV]≤35···(i)

[0111] 2≤[V]≤35 ···(j)

[0112] 0.01≤[VI]≤10 ···(k)

[0113] [VI] / [II]<1 ···(l)

[0114] [I] to [VI] represent the content (mol %) of each of the following structural units (I) to (VI) relative to 100 mol % of all structural units of the liquid crystal polyester resin.

[0115]

[0116] The structural units (I) to (VI) are as described above.

[0117] In addition, in the liquid crystal polyester resin, in addition to the above-mentioned structural units (I) to (VI), structural units derived from p-aminobenzoic acid, p-aminophenol, etc. may be used within a range not impairing the effects of the present invention.

[0118] The liquid crystal polyester resin of the present invention is preferably such that the temperature sensitivity coefficient and the curing start temperature can be more easily controlled within an appropriate range, the molding temperature can be formed in a wide range, the molding stability is excellent, and the thickness dependence of the fluidity is small by including all the above-mentioned structural units (I) to (VI) within the above-mentioned range. In order not to impair the effects of the present invention, the total content of the above-mentioned structural units (I) to (VI) is preferably 99 mol% or more, preferably 99.5 mol% or more, and more preferably 100 mol% relative to 100 mol% of all the structural units of the liquid crystal polyester resin.

[0119] From the viewpoint of controlling polymerizability, the ratio of the total amount of the structural units (III) and (IV) to the total amount of the structural units (V) and (VI) ([III] + [IV]) / ([V] + [VI]) is preferably 0.9 or more and 1.1 or less.

[0120] The monomers that become the raw materials constituting the above-mentioned various structural units are not particularly limited as long as they are structures that can form various structural units. In addition, derivatives after the hydroxyl groups of such monomers are acylated, carboxylic acid derivatives after the carboxyl groups are converted into esters, acyl halides, acid anhydrides, etc., etc. can also be used.

[0121] Regarding the liquid crystal polyester resin, the calculation method of the content of each structural unit is shown below. First, the liquid crystal polyester resin is crushed, tetramethylammonium hydroxide is added, and a GC / MS analyzer (such as Shimadzu GCMS-QP5050A) is used to perform thermal decomposition GC / MS measurement, thereby the content of each structural unit can be obtained. The content of structural units that are not detected or below the detection limit is calculated as 0 mol%.

[0122] From the perspective of heat resistance, the melting point (Tm) of the liquid crystal polyester resin is preferably 280°C or higher, more preferably 300°C or higher, and further preferably 320°C or higher. On the other hand, from the perspective of processability, the melting point (Tm) of the liquid crystal polyester resin is preferably 370°C or lower, more preferably 360°C or lower, and further preferably 350°C or lower. It should be noted that Tm is a value measured using a differential scanning calorimeter as described below.

[0123] From the perspective of heat resistance, the melt viscosity of the liquid crystal polyester resin is preferably 3 Pa·s or more, more preferably 5 Pa·s or more, and further preferably 7 Pa·s or more. On the other hand, from the perspective of fluidity, the melt viscosity of the liquid crystal polyester resin is preferably 50 Pa·s or less, preferably 30 Pa·s or less, and further preferably 20 Pa·s or less.

[0124] The melt viscosity is a value measured using a high-pressure flow tester at a temperature of the melting point (Tm) of the liquid crystal polyester resin + 20° C. and a shear rate of 1000 / sec.

[0125] <Method for producing liquid crystal polyester resin>

[0126] The method for producing the liquid crystal polyester resin of the present invention includes a method of copolymerizing monomers providing structural units (I) to (VI) in a content within the above range, and a method of blending two or more liquid crystal polyester resins obtained by copolymerizing monomers providing structural units (I) to (VI) in a content outside the above range to adjust the content of structural units (I) to (VI) to the above range. The method of copolymerizing monomers providing structural units (I) to (VI) in a content within the above range is preferred from the viewpoints of not inheriting the properties of the liquid crystal polyester resin before mixing, facilitating the control of the above temperature sensitivity coefficient and curing start temperature within an appropriate range, enabling molding at a wide range of molding temperatures, excellent molding stability, and reduced thickness dependence of fluidity.

[0127] As a method for manufacturing the liquid crystal polyester resin of the present invention, there is no particular limitation, and a known polyester polycondensation method can be used. Considering that the above-mentioned temperature sensitivity coefficient and the curing start temperature are controlled within a suitable range, when taking the method for manufacturing a liquid crystal polyester resin comprising structural units (I) to (VI) as an example, the following method is preferred: reacting acetic anhydride with p-hydroxybenzoic acid, 6-hydroxy-2-naphthoic acid, 4,4'-dihydroxybiphenyl, hydroquinone, terephthalic acid and isophthalic acid, acetylating the phenolic hydroxyl group, and then performing deacetication polymerization to manufacture a liquid crystal polyester resin.

[0128] Furthermore, in the above-mentioned production method, by satisfying the following conditions 1 to 3, it is easy to control the temperature sensitivity coefficient and the curing start temperature within an appropriate range, which is preferred.

[0129] 1. Deacetic acid polymerization is carried out without catalyst.

[0130] 2. Deacetic acid polymerization is carried out under heating conditions, and the average heating rate from 145°C to 270°C is set to 0.3-0.8°C / min.

[0131] 3. In the step of acetylation of the monomer, the amount of acetic anhydride used is set to 1.05 to 1.20 molar equivalents of the total of the phenolic hydroxyl groups of the aromatic hydroxycarboxylic acid and the aromatic diol.

[0132] Regarding the above condition 1, if a catalyst is added in the deacetic acid polymerization, the reaction is carried out at a high speed, and on the other hand, the generation of a long chain formed by an aromatic hydroxycarboxylic acid is induced. The long chain of an aromatic hydroxycarboxylic acid is highly crystalline, so when the liquid crystal polyester resin contains a long chain of an aromatic hydroxycarboxylic acid, the physical properties such as heat resistance are improved, but on the other hand, not only infusible crystals and foreign matter are generated, but also the solidification crystallization starting from the molten state is rapidly carried out, so the control of the above-mentioned temperature sensitivity coefficient and the solidification start temperature becomes difficult. Therefore, it is preferred to carry out deacetic acid polymerization without a catalyst. It should be noted that as a specific example of a catalyst when a catalyst is added, metal salts containing alkali metals and alkaline earth metal salts, potassium acetate and sodium acetate, etc. containing organic acids and alkali metals, alkaline earth metals, antimony trioxide, magnesium metal, etc. can be listed.

[0133] Regarding the above condition 2, within the range of polymerization temperature of 145°C to 270°C, acetylation of aromatic hydroxycarboxylic acid and aromatic diol to oligomer formation is carried out. At this time, by setting the average temperature rise rate to 0.3 to 0.8°C / minute, oligomers are easily formed accompanied by ester exchange, which promotes the randomization of the structural units of the main chain. Therefore, the long chain generation of the above-mentioned aromatic hydroxycarboxylic acid is suppressed, and therefore, the control of the above-mentioned temperature sensitivity coefficient and curing start temperature becomes easy. The average temperature rise rate is preferably 0.35°C / minute or more, and more preferably 0.4°C / minute or more. In addition, the average temperature rise rate is preferably 0.7°C / minute or less, more preferably 0.65°C / minute or less, and further preferably 0.6°C / minute or less.

[0134] Regarding the above condition 3, by setting the amount of acetic anhydride to 1.05 to 1.20 molar equivalents of the total phenolic hydroxyl groups, the process of molecular weight increase from oligomer formation is easily accompanied by transesterification, which promotes the randomization of the structural units of the main chain. As a result, the long chain generation of the above aromatic hydroxycarboxylic acid is suppressed, and therefore, the control of the above temperature sensitivity coefficient and curing start temperature becomes easy. The amount of acetic anhydride is preferably 1.06 molar equivalents or more, and more preferably 1.07 molar equivalents or more. In addition, the amount of acetic anhydride is preferably 1.18 or less, and more preferably 1.15 or less.

[0135] As described above, by satisfying the above conditions 1 to 3, the generation of long chains of aromatic hydroxycarboxylic acids in the liquid crystal polyester resin can be suppressed, and the above temperature sensitivity coefficient and curing start temperature can be easily controlled within appropriate ranges.

[0136] <Packing>

[0137] In order to impart mechanical strength and other characteristics to the liquid crystal polyester resin, a liquid crystal polyester resin composition containing the liquid crystal polyester resin of the present invention and a filler can be prepared. The filler used in the present invention is not particularly limited, and for example, fibrous, whisker-like, plate-like, powdery, granular and other fillers can be cited. Specifically, as fibrous and whisker-like fillers, glass fibers; carbon fibers of PAN and asphalt; metal fibers such as stainless steel fibers, aluminum fibers, and brass fibers; organic fibers such as aromatic polyamide fibers and liquid crystal polyester fibers; gypsum fibers, ceramic fibers, asbestos fibers, zirconium oxide fibers, aluminum oxide fibers, silica fibers, titanium oxide fibers, silicon carbide fibers, rock wool, potassium titanate whiskers, barium titanate whiskers, aluminum borate whiskers, silicon nitride whiskers, and needle-shaped titanium oxide, etc. As plate-like fillers, mica, talc, kaolin, glass flakes, clay, molybdenum disulfide, and wollastonite, etc. can be cited. As powdery and granular fillers, silica, glass beads, titanium oxide, zinc oxide, calcium polyphosphate, and graphite, etc. can be cited. The surface of the filler may be treated with a surface treatment agent such as a known coupling agent (for example, a silane coupling agent, a titanate coupling agent, etc.) or the like. In addition, two or more types of the fillers may be used in combination.

[0138] Among the above-mentioned fillers, glass fiber is preferably used from the viewpoint of excellent mechanical strength such as tensile strength and flexural strength, heat resistance, and dimensional stability. There is no particular restriction on the type of glass fiber, as long as it is a glass fiber commonly used for the reinforcement of resins, and examples thereof include chopped strands of long fiber type or short fiber type, milled fibers, etc. In addition, plate-like fillers are also preferably used from the viewpoint of excellent thin-wall fluidity.

[0139] The surface of the glass fiber can be treated with a known coupling agent (for example, a silane coupling agent, a titanate coupling agent, or the like). In addition, the glass fiber can be coated or bundled with a thermoplastic resin such as an ethylene / vinyl acetate copolymer or a thermosetting resin such as an epoxy resin.

[0140] In the liquid crystal polyester resin composition of the present invention, conventional additives selected from antioxidants, heat stabilizers (such as hindered phenols, hydroquinone, phosphites, thioethers and their substitutes, etc.), ultraviolet absorbers (such as resorcinol, salicylate), anti-coloring agents such as phosphites and hypophosphites, lubricants and release agents (montanic acid and its metal salts, its esters, its half esters, stearyl alcohol, stearamide and polyethylene wax, etc.), colorants including dyes or pigments, carbon black as a conductive agent or colorant, crystal nucleating agents, plasticizers, flame retardants (bromine flame retardants, phosphorus flame retardants, red phosphorus, silicone flame retardants, etc.), flame retardant aids, and antistatic agents can be further formulated within a range that does not impair the effects of the present invention.

[0141] In the liquid crystal polyester resin composition of the present invention, the content of filler relative to 100 parts by weight of the liquid crystal polyester resin is preferably 10 to 200 parts by weight. If the filler content is 10 parts by weight or more, the mechanical strength of the molded product can be improved. The filler content is more preferably 15 parts by weight or more, and more preferably 20 parts by weight or more. On the other hand, when the filler content is less than 200 parts by weight, a liquid crystal polyester resin composition having excellent moldability and thin-wall fluidity and which can be easily injection molded into a small thin-walled molded product can be obtained, so it is preferred. The filler content is more preferably less than 150 parts by weight, and more preferably less than 100 parts by weight.

[0142] As a method for blending the filler and the additive, for example, a dry blending method of blending the filler and other solid additives into the liquid crystal polyester resin, a solution blending method of blending the filler and other liquid additives into the liquid crystal polyester resin, a method of adding the filler and other additives during polymerization of the liquid crystal polyester resin, a method of melt-kneading the filler and other additives into the liquid crystal polyester resin, etc. Among them, the melt-kneading method is preferred.

[0143] The melt kneading can be carried out by a known method. As the apparatus used in the melt kneading, for example, a Banbury mixer, a rubber roll machine, a kneader, a single screw or twin screw extruder, etc. can be cited. Among them, a twin screw extruder is preferred. The melt kneading temperature is preferably above the melting point of the liquid crystal polyester resin and below the melting point + 50°C.

[0144] Examples of the kneading method include 1) a method in which a liquid crystal polyester resin, a filler and other additives are fed at once from a rear feeder and kneaded (a one-time kneading method), 2) a method in which a liquid crystal polyester resin and other additives are fed from a rear feeder and kneaded, and then fillers and other additives as required are added from a side feeder and kneaded (a side feed method), and 3) a method in which a liquid crystal polyester composition (masterbatch) containing other additives at a high concentration in a liquid crystal polyester resin is prepared, and then the masterbatch is kneaded with the liquid crystal polyester resin and the filler in such a way that the additives have a predetermined concentration (a masterbatch method).

[0145] <Molding products>

[0146] The liquid crystal polyester resin and liquid crystal polyester resin composition of the present invention can be processed into molded products with excellent surface appearance (color tone), mechanical properties and heat resistance by melt molding such as injection molding, extrusion molding, spinning, and molding methods such as press molding and solution casting. As the molded products mentioned here, injection molded products, extrusion molded products, press molded products, sheets, pipes, various films such as unstretched films, uniaxially stretched films, and biaxially stretched films, various fibers such as unstretched yarns and super-stretched yarns, etc. can be listed. In particular, from the perspective of processability, injection molding is preferred as a molding method. In the case of melt molding, from the perspective of suppressing the deterioration of the liquid crystal polyester resin composition and improving the mechanical strength, it is preferred to perform melt molding at a temperature below 370°C, and more preferably below 360°C.

[0147] The molded articles obtained by molding the liquid crystal polyester resin and the liquid crystal polyester resin composition of the present invention can be preferably used as electrical / electronic components. As electrical / electronic components, for example, flexible printed substrates, laminated circuit substrates, printed wiring substrates and three-dimensional circuit substrates used in antennas of mobile communication / electronic devices such as personal computers, GPS built-in devices, mobile phones, millimeter wave and quasi-millimeter wave radars such as anti-collision radars, tablet computers, smart phones, etc. can be listed; LED and other light reflectors, lamp holders, communication base stations of mobile communication terminals, small base stations, micro base station components, antenna covers, housings, sensors, actuator elements of camera modules, connectors, relay housings and bases, switches, coil frames, capacitors, etc. Among them, considering that it can be molded at a wide range of molding temperatures and the thickness dependence of fluidity is small, it is useful for connectors, relays, switches, coil frames, actuator elements of camera modules, etc. with thin-walled complex shape parts.

[0148] Example

[0149] Hereinafter, the present invention will be described using examples, but the present invention is not limited to the examples. In the examples, the composition and property evaluation of the liquid crystal polyester resin were measured by the following methods.

[0150] (1) Composition analysis of liquid crystal polyester resin

[0151] To 0.1 mg of the pulverized liquid crystal polyester resin particles, 2 μL of a 25% methanol solution of tetramethylammonium hydroxide was added, and thermal decomposition GC / MS measurement was performed using GCMS-QP5050A manufactured by Shimadzu Corporation to determine the composition ratio of each constituent in the liquid crystal polyester resin.

[0152] (2) Determination of melting point (Tm) of liquid crystal polyester resin

[0153] Using a differential scanning calorimeter DSC-7 (manufactured by Perkin Elmer), the liquid crystal polyester resin was heated from room temperature at a heating rate of 20°C / min. After the endothermic peak temperature (Tm1) was observed, it was maintained at Tm1+20°C for 5 minutes, then temporarily cooled to room temperature at a cooling rate of 20°C / min, and again heated from room temperature to Tm1+20°C at a heating rate of 20°C / min. The endothermic peak temperature observed at this time was taken as the melting point (Tm).

[0154] (3) Melt viscosity of liquid crystal polyester resin

[0155] The melt viscosity of the liquid crystal polyester resin was measured using a Koka flow tester CFT-500D (orifice 0.5φ×10 mm) (manufactured by Shimadzu Corporation) at a temperature of Tm+20° C. and a shear rate of 1000 / s.

[0156] (4) Evaluation of the temperature range in which molding is possible

[0157] After the liquid crystal polyester resin was dried at 150°C for 3 hours using a hot air dryer, it was supplied to a ファナックα30C injection molding machine (manufactured by ファナック) and a mold capable of molding a molded product of 5.0mm in width × 50mm in length × 0.2mm in thickness was used. Under the molding conditions of mold temperature 90°C and injection speed 200mm / s, the molding pressure was adjusted so that the average length of the obtained molded product became 40mm, and 100 injection continuous moldings were performed. At this time, the barrel temperature was changed in increments of 5°C within the range of the melting point ±0°C to the melting point + 40°C of the liquid crystal polyester resin, and the molding was performed. For the obtained test piece, the barrel temperature at which the number of injections of 39mm or less or 41mm or more in length was less than 5 times in 100 injections was taken as the molding temperature, and the molding temperature range = (the highest molding temperature) - (the lowest molding temperature). The larger the value, the wider the molding temperature range.

[0158] (5) Evaluation of thickness dependence of fluidity

[0159] After the liquid crystal polyester resin was dried at 150°C for 3 hours using a hot air dryer, it was supplied to a Fanac α30C injection molding machine (manufactured by Fanac), and a mold capable of molding a molded product of 5.0 mm in width × 50 mm in length × 0.2 mm in thickness was used. The barrel temperature was set to the melting point of the liquid crystal polyester resin + 10°C, the mold temperature was set to 90°C, and the molding conditions were adjusted to an average length of 40 mm for the obtained molded product under the molding conditions of an injection speed of 200 mm / s. Then, the mold was replaced with a mold capable of molding a molded product of 5.0 mm in width × 50 mm in length × 0.5 mm in thickness at the flow end side, and a mold capable of molding a molded product of 5.0 mm in width × 30 mm in length × 0.2 mm in thickness. In addition, 10 molds were molded under the same molding conditions, and the average flow length of the 0.2 mm thick portion of the obtained molded product was calculated. The larger the flow length of the 0.2 mm thick portion, the smaller the thickness dependence of the fluidity, and the better.

[0160] (6) Molding stability (evaluation of the number of shots required for recovery)

[0161] The liquid crystal polyester resin pellets obtained in each example and comparative example were dried at 150° C. for 3 hours using a hot air dryer, and then supplied to a Fanac α30C injection molding machine manufactured by Fanac. The injection barrel temperature was set to the melting point of the liquid crystal polyester + 15° C., the mold temperature was set to 90° C., the injection pressure was set to 100 MPa, and the speed was set to the minimum filling speed, and injection molding was performed to obtain Figure 3 Connector molding shown. Figure 3 The connector molded product is a three-dimensional diagram having a long surface (2) and a short surface (3), and the outer dimensions are width (6) 3mm × height (5) 2mm × length (4) 30mm. It has terminals separated by a partition wall portion (8), the distance (7) between the terminals is 0.4mm, and the thickness of the partition wall portion (8) as the minimum wall thickness portion of the product is 0.2mm. Liquid crystal polyester resin or resin composition is filled from the needle-shaped gate G1 (gate diameter 0.3mm) provided on the short surface (3) on one side of the connector molded product, and is fully filled to the wall corner on the opposite side of the gate. After 100 injection continuous moldings, the molding is temporarily stopped, the injection barrel temperature is lowered to 150°C, and the mold is left to stand for 120 minutes. Then, the injection barrel temperature was raised to the melting point of the liquid crystal polyester + 15°C, and the same liquid crystal polyester resin or resin composition as in the above molding was used to perform a purge injection, and then continuous molding was performed under the same conditions and in the same mold, and the number of injections required to obtain a molded product that was fully filled to the corner on the opposite side of the gate, that is, the number of injections required for recovery, was evaluated in the same manner as in the above molding. The corner is a part that is prone to unfilling after recovery, and when the number of injections required for recovery is less than 10, the molding stability is excellent.

[0162] (7) Evaluation of temperature sensitivity and curing start temperature

[0163] After the liquid crystal polyester resin was dried at 150°C for 3 hours using a hot air dryer, it was measured using a rheometer Physica MCR501 (rheometer manufactured by Anthon Palton Co., Ltd.) as described below. The liquid crystal polyester resin was placed between parallel plates with a diameter of 25 mm. In the vibration measurement mode of the rheometer, the gap between the parallel plates was set to 1 mm, the strain was set to 10%, and the frequency was set to 1 Hz. After maintaining the temperature at Tm+30°C for 5 minutes, the temperature was lowered at 0.17°C / second to a temperature at which the complex viscosity became 50,000 (Pa·s) while measuring to obtain a rheometer spectrum. The x-axis was set to ΔT(°C)=measurement temperature-Tm(°C), and the y-axis was set to the logarithm of the complex viscosity (log(η(Pa·s))), and the rheometer spectrum was obtained. Figure 1 The rheological spectrum curve 1 shown is obtained by calculating B(x) (curing start temperature) and the absolute value of the slope of the straight line w connecting point A and point B (temperature sensitivity coefficient) through the above-mentioned steps from the obtained rheometer spectrum. It should be noted that the temperature sensitivity coefficient is calculated by the following formula.

[0164] Temperature sensitivity coefficient = |(log(η(Pa·s)) of point A - log(η(Pa·s)) of point B) / (20-B(x))|

[0165] [Example 1]

[0166] In a 5 L reaction vessel equipped with a stirring blade and a distillation tube, 808 parts by weight of p-hydroxybenzoic acid (HBA), 88 parts by weight of 6-hydroxy-2-naphthoic acid (HNA), 229 parts by weight of 4,4'-dihydroxybiphenyl (DHB), 161 parts by weight of hydroquinone (HQ), 428 parts by weight of terephthalic acid (TPA), 19 parts by weight of isophthalic acid (IPA) and 1278 parts by weight of acetic anhydride (1.07 equivalents of the total phenolic hydroxyl groups) were added, and the mixture was reacted at 145°C for 120 minutes under a nitrogen atmosphere while stirring. The temperature was then raised from 145°C to 360°C over 4 hours (the average temperature rise rate from 145°C to 270°C was 0.9°C / min). Then, the polymerization temperature was maintained at 360°C, the pressure was reduced to 1.0 mmHg (133 Pa) over 1.0 hour, the reaction was further continued, and the polymerization was terminated when a predetermined stirring torque was reached. Next, the polymer was discharged in the form of strands through a die having a circular discharge port with a diameter of 6 mm, and granulated by a cutter to obtain a liquid crystal polyester resin (A-1).

[0167] [Example 2]

[0168] A liquid crystal polyester resin (A-2) was obtained by performing the same operation as in Example 1 except that the monomer addition amounts were changed to 776 parts by weight of HBA, 66 parts by weight of HNA, 251 parts by weight of DHB, 168 parts by weight of HQ, 447 parts by weight of TPA, and 29 parts by weight of IPA.

[0169] [Example 3]

[0170] A liquid crystal polyester resin (A-3) was obtained by performing the same operation as in Example 1 except that the monomer addition amounts were changed to 1018 parts by weight of HBA, 264 parts by weight of HNA, 44 parts by weight of DHB, 135 parts by weight of HQ, 214 parts by weight of TPA, and 29 parts by weight of IPA.

[0171] [Example 4]

[0172] A liquid crystal polyester resin (A-4) was obtained by carrying out the same operation as in Example 1 except that the monomer addition amounts were changed to 905 parts by weight of HBA, 88 parts by weight of HNA, 109 parts by weight of DHB, 193 parts by weight of HQ, 321 parts by weight of TPA and 68 parts by weight of IPA.

[0173] [Example 5]

[0174] A liquid crystal polyester resin (A-5) was obtained by performing the same operation as in Example 1 except that the monomer addition amounts were changed to 469 parts by weight of HBA, 242 parts by weight of HNA, 131 parts by weight of DHB, 309 parts by weight of HQ, 564 parts by weight of TPA, and 19 parts by weight of IPA.

[0175] [Example 6]

[0176] A liquid crystal polyester resin (A-6) was obtained by carrying out the same operation as in Example 1 except that the monomer addition amounts were changed to 986 parts by weight of HBA, 88 parts by weight of HNA, 360 parts by weight of DHB, 13 parts by weight of HQ, 321 parts by weight of TPA and 19 parts by weight of IPA.

[0177] [Example 7]

[0178] The monomer feed amounts were changed to 792 parts by weight of HBA, 88 parts by weight of HNA, 251 parts by weight of DHB, 155 parts by weight of HQ, 457 parts by weight of TPA, and 1314 parts by weight of acetic anhydride (1.10 equivalents of the total phenolic hydroxyl groups), and the temperature was increased from 145°C to 270°C at an average heating rate of 0.5°C / min. Except for this, the same operations as in Example 1 were performed to obtain a liquid crystal polyester resin (A-7).

[0179] [Example 8]

[0180] The monomer feed amounts were changed to 905 parts by weight of HBA, 88 parts by weight of HNA, 436 parts by weight of DHB, 321 parts by weight of TPA, 68 parts by weight of IPA, and 1314 parts by weight of acetic anhydride (1.10 equivalents of the total phenolic hydroxyl groups), and the temperature was increased from 145°C to 270°C at an average heating rate of 0.5°C / min. Otherwise, the same operations as in Example 1 were performed to obtain a liquid crystal polyester resin (A-8).

[0181] [Example 9]

[0182] A liquid crystal polyester resin (A-9) was obtained by performing the same operation as in Example 1 except that the temperature was increased at an average temperature increase rate of 0.5° C. / min from 145° C. to 270° C.

[0183] [Comparative Example 1]

[0184] A liquid crystal polyester resin (A'-10) was obtained by the same operation as in Example 1 except that the monomer feed amounts were changed to 870 parts by weight of HBA, 352 parts by weight of DHB, 89 parts by weight of HQ, 292 parts by weight of TPA, and 157 parts by weight of IPA.

[0185] [Comparative Example 2]

[0186] A liquid crystal polyester resin (A'-11) was obtained by the same operation as in Example 1 except that the monomers charged were changed to 808 parts by weight of HBA, 88 parts by weight of HNA, 501 parts by weight of DHB, 408 parts by weight of TPA, and 39 parts by weight of IPA.

[0187] [Comparative Example 3]

[0188] A liquid crystal polyester resin (A'-12) was obtained by the same operation as in Example 1 except that the monomer feed amounts were changed to 970 parts by weight of HBA, 88 parts by weight of HNA, 196 parts by weight of DHB, 116 parts by weight of HQ and 350 parts by weight of TPA.

[0189] [Comparative Example 4]

[0190] A liquid crystal polyester resin (A'-13) was obtained by the same operation as in Example 1 except that the monomer feed amounts were changed to 743 parts by weight of HBA, 176 parts by weight of HNA, 296 parts by weight of HQ, 292 parts by weight of TPA, and 156 parts by weight of IPA.

[0191] [Comparative Example 5]

[0192] The same operation as in Example 1 was carried out to obtain a liquid crystal polyester resin (A'-14) except that the monomer addition amounts were changed to 937 parts by weight of HBA, 44 parts by weight of HNA, 261 parts by weight of DHB, 103 parts by weight of HQ, 292 parts by weight of TPA, and 97 parts by weight of IPA.

[0193] [Comparative Example 6]

[0194] The monomer feed amounts were changed to 792 parts by weight of HBA, 88 parts by weight of HNA, 251 parts by weight of DHB, 155 parts by weight of HQ, 457 parts by weight of TPA, and 1231 parts by weight of acetic anhydride (1.03 equivalents of the total phenolic hydroxyl groups), 1 part by weight of potassium acetate was added as a catalyst, and the temperature was increased from 145°C to 270°C at an average heating rate of 0.5°C / min. Except for this, the same operations as in Example 1 were performed to obtain a liquid crystal polyester resin (A'-15).

[0195] [Comparative Example 7]

[0196] A liquid crystal polyester resin (A'-16) was obtained by the same operation as in Example 1 except that the monomers charged were changed to 792 parts by weight of HBA, 88 parts by weight of HNA, 251 parts by weight of DHB, 155 parts by weight of HQ and 457 parts by weight of TPA.

[0197] [Comparative Example 8]

[0198] A liquid crystal polyester resin (A'-17) was obtained by the same operation as in Example 1 except that the monomers charged were changed to 905 parts by weight of HBA, 88 parts by weight of HNA, 436 parts by weight of DHB, 321 parts by weight of TPA, and 68 parts by weight of IPA.

[0199] The liquid crystal polyester resins obtained in Examples 1 to 9 and Comparative Examples 1 to 8 were evaluated in the following (1) to (7). The results are shown in Tables 1 and 2.

[0200]

[0201]

[0202] A filler was further added to the liquid crystal polyester resin obtained in Example 1 and Comparative Example 5 to prepare a liquid crystal polyester resin composition. The fillers used in each of the Examples and Comparative Examples are shown below.

[0203] Filler (B)

[0204] (B-1) Made by Nippon Electric Glass, ground fiber (40M-10A)

[0205] [Example 10, Comparative Example 9]

[0206] The liquid crystal polyester resins (A-1, A'-14) obtained in each manufacturing example were fed from a hopper in the amounts shown in Table 3 using a TEM35B twin-screw extruder manufactured by Toshiba Machine Co., Ltd. equipped with a side feeder, and the filler (B-1) was added from the side feeder in the amounts shown in Table 3, and the cylinder temperature was set to the melting point of the liquid crystal polyester resin + 10°C, and melt kneading was performed to obtain pellets. The pellets of the obtained liquid crystal polyester resin composition were hot-air dried, and the same evaluations as (4) to (6) were performed, and the results are shown in Table 3.

[0207] Table 3

[0208]

[0209] From the results in Tables 1 to 3, it can be seen that by using a liquid crystal polyester resin having a temperature sensitivity coefficient of less than 0.020 and a curing start temperature of -35 to -15°C, or a liquid crystal polyester resin composition using such a resin, molding can be performed at a wide range of molding temperatures, and a molded product with excellent molding stability and low thickness dependence of fluidity can be obtained.

[0210] Industrial Applicability

[0211] The liquid crystal polyester resin and liquid crystal polyester resin composition of the present invention can be molded at a wide range of molding temperatures, have excellent molding stability, and have low thickness dependence of fluidity, and are therefore suitable for use in electrical / electronic components and mechanical components such as connectors, relays, switches, coil frames, and actuator elements of camera modules.

[0212] Explanation of symbols

[0213] 1 Rheological curve of liquid crystal polyester resin

[0214] A point on the rheological spectrum curve where ΔT is 20°C

[0215] The point on the A' rheological spectrum curve where ΔT is 10°C

[0216] tThe straight line passing through points A' and A

[0217] C is a point below the melting point on the rheological spectrum curve where the complex viscosity is 10000 Pa·s.

[0218] The point below the melting point on the C' rheological spectrum curve with a complex viscosity of 5000 Pa·s

[0219] uThe straight line passing through points C and C'

[0220] B'The intersection of line t and line u

[0221] vA straight line passing through point B' and parallel to the y-axis

[0222] The intersection of straight line B and rheological spectrum curve

[0223] wThe straight line connecting point A and point B

[0224] S1 Example of rheological spectrum curve of the liquid crystal polyester resin of the present invention

[0225] S2 Example of rheological spectrum curve of existing liquid crystal polyester resin

[0226] L1 is equivalent to Figure 1 The straight line representing the temperature sensitivity coefficient of S1 is

[0227] L2 is equivalent to Figure 1 The straight line representing the temperature sensitivity coefficient of S2 is

[0228] 2 Long surface

[0229] 3 Short surface

[0230] 4 Length

[0231] 5 Height

[0232] 6 Width

[0233] 7 Terminal distance

[0234] 8 Partition wall

[0235] G1 Pin Gate

Claims

1. A liquid crystal polyester resin comprising a structural unit derived from an aromatic hydroxycarboxylic acid, a structural unit derived from an aromatic diol and a structural unit derived from an aromatic dicarboxylic acid, wherein the content of the structural unit derived from the aromatic hydroxycarboxylic acid is 15 to 80 mol%, the content of the structural unit derived from the aromatic diol is 2 to 40 mol%, and the content of the structural unit derived from the aromatic dicarboxylic acid is 2 to 40 mol%, relative to 100 mol% of all structural units of the liquid crystal polyester resin, and the following condition (α) is satisfied: (α): The temperature sensitivity coefficient measured as follows is less than 0.020, and B(x) is -35 to -15°C; When the melting point of the liquid crystal polyester resin is set to Tm (°C), the liquid crystal polyester resin is measured using a rheometer as follows. In the rheological spectrum curve of the liquid crystal polyester resin obtained by setting the x-axis to ΔT (°C) = measurement temperature - Tm (°C) and the y-axis to the logarithm of the complex viscosity (log (η (Pa·s))), the point where ΔT = 20°C is set as point A, the point where ΔT = 10°C is set as point A', and the point below the melting point and the complex viscosity η is 10000 Pa·s is set as point C , the point where the complex viscosity η is 5000 Pa·s is set as point C', the straight line passing through point A and point A' is set as straight line t, the straight line passing through point C and point C' is set as straight line u, the intersection of straight line t and straight line u is set as point B', the straight line passing through point B' and parallel to the y-axis is set as straight line v, the intersection of straight line v and the rheological spectrum curve is set as point B, the absolute value of the slope of the straight line w connecting point A and point B is defined as the temperature sensitivity coefficient, and the ΔT value of point B is defined as B(x); The above rheological spectrum curve is obtained by setting the gap between parallel plates to 1 mm, the strain to 10% and the frequency to 1 Hz in the vibration measurement mode of the rheometer, maintaining the temperature at Tm+30°C for 5 minutes, and then cooling the temperature at 0.17°C / sec to a temperature at which the complex viscosity reaches 50,000 (Pa·s); The melting point Tm of the above-mentioned liquid crystal polyester resin is the endothermic peak temperature Tm1 observed when the liquid crystal polyester resin is heated from room temperature at a heating condition of 20°C / min in differential calorimetry, then maintained at a temperature of Tm1+20°C for 5 minutes, then temporarily cooled to room temperature at a cooling condition of 20°C / min, and heated again at a heating condition of 20°C / min.

2. The liquid crystal polyester resin according to claim 1, comprising a structural unit selected from the following structural units (I) to (V), and satisfying the following conditions (a) to (d): 25≤[I]≤75···(a) 1≤[II]≤20···(b) 2≤[III]+[IV]≤35···(c) 2≤[V]≤35···(d) [I] to [V] represent the content (mol %) of each of the following structural units (I) to (V) relative to 100 mol % of all structural units of the liquid crystal polyester resin, respectively.

3. The liquid crystal polyester resin according to claim 1 or 2, comprising the following structural units (II) and (VI), and satisfying the following conditions (e) and (f): 0.01≤[VI]≤10···(e) [VI] / [II]<1···(f) [II] and [VI] represent the content (mol %) of each of the following structural units (II) and (VI), respectively, relative to 100 mol % of all structural units of the liquid crystal polyester resin.

4. The liquid crystal polyester resin according to any one of claims 1 to 3, comprising a structural unit selected from the following structural units (I) to (VI), and satisfying the following conditions (g) to (l): 25≤[I]≤75···(g) 1≤[II]≤20···(h) 2≤[III]+[IV]≤35···(i) 2≤[V]≤35···(j) 0.01≤[VI]≤10···(k) [VI] / [II]<1···(l) [I] to [VI] represent the content (mol %) of each of the following structural units (I) to (VI) relative to 100 mol % of all structural units of the liquid crystal polyester resin, respectively.

5. The liquid crystal polyester resin according to any one of claims 1 to 4, further satisfying the following condition (m): 0<[III] / [IV]<1.5···(m) [III] and [IV] represent the content (mol %) of each of the structural units (III) and (IV) relative to 100 mol % of all structural units of the liquid crystal polyester resin.

6. The liquid crystal polyester resin according to any one of claims 1 to 5, further satisfying the following condition (n): 99≤[I]+[II]+[III]+[IV]+[V]+[VI]≤100···(n) [I] to [VI] represent the content (mol %) of each of the above-mentioned structural units (I) to (VI) relative to 100 mol % of all structural units of the liquid crystal polyester resin. 7 . A liquid crystal polyester resin composition comprising 10 to 200 parts by weight of a filler based on 100 parts by weight of the liquid crystal polyester resin according to claim 1 . 8 . A molded article, comprising the liquid crystal polyester resin according to claim 1 or the liquid crystal polyester resin composition according to claim 7 . 9 . The molded article according to claim 8 , wherein the molded article is any one selected from a connector, a relay, a switch, a coil bobbin, and an actuator element of a camera module.