460MPa strength grade steel and manufacturing method thereof

By introducing B and Cr elements into 460MPa strength grade steel and adopting open-flat cutting board treatment process, the problems of poor quality stability and high production cost are solved, and 460MPa with good straightness and high molding stability are achieved efficiently produced. Strength grade steel.

CN118957434AActive Publication Date: 2024-11-15HUNAN VALIN LIANYUAN IRON & STEEL CO LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410887811.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-15
Estimated Expiration
2044-07-03

AI Technical Summary

Technical Problem

The 460MPa strength grade steel produced in the prior art has problems of poor quality stability and high production costs.

Method used

By introducing B and Cr elements into the chemical composition of 460MPa strength grade steel, the content is controlled at 0.0015wt%≤B≤0.0025wt%, Cr≤0.30wt%, and using open-flat cutting board treatment process, combined with hot-rolled material Phosphorus removal, rough rolling, finishing rolling and coiling treatments control the straightness and internal stress of the steel plate, and improve the hardenability and molding stability of the steel plate.

Benefits of technology

The yield strength of the steel plate is <500MPa, the plate shape is good straightness, high quality stability, and low cost, which is suitable for large-scale promotion and application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957434A_ABST
    Figure CN118957434A_ABST
Patent Text Reader

Abstract

The invention provides 460MPa strength grade steel and a manufacturing method thereof. The steel plate comprises the following chemical components in percentage by mass: more than or equal to 0.05 wt% and less than or equal to 0.08 wt% of C, more than or equal to 0.15 wt% and less than or equal to 0.30 wt% of Si, more than or equal to 1.10 wt% and less than or equal to 1.30 wt% of Mn, less than or equal to 0.02 wt% of P, less than or equal to 0.005 wt% of S, more than or equal to 0.018 wt% and less than or equal to 0.045 wt% of Als, more than or equal to 0.025 wt% and less than or equal to 0.038 wt% of Ti, more than or equal to 0.015 wt% and less than or equal to 0.030 wt% of Nb, less than or equal to 0.0055 wt% of N, more than or equal to 0.0015 Compared with the prior art, grains are uniform, and the yield strength of the steel plate is 1t; and the flatness of the plate shape is good, and the quality stability is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal casting, and in particular to a 460MPa strength grade steel and a manufacturing method thereof. Background Art

[0002] 460MPa strength grade steel belongs to low alloy structural steel, with relatively low material grade, mainly used for ordinary structural components, etc., and the quality requirements for materials are not high. However, with the popularization of automation such as laser cutting and automatic welding in downstream processing and supporting plants, steel plates need to meet high quality dimensional requirements such as cutting without warping and high dimensional accuracy of welding during use. In order to meet the use requirements of steel plates, steel plates need to have the characteristics of low internal stress, good straightness and good mechanical property stability, so that steel plates can reflect the processing ability and aesthetics of materials. Therefore, it is necessary to have a comprehensive quality requirement of good quality and low price for this material. 460MPa strength grade belongs to low alloy structural steel, with a large amount of material used, mainly used for structural components, etc. With the popularization of automation in downstream processing and supporting plants using automatic laser cutting, automatic welding and assembly and other process production means, steel plates need to meet high quality requirements such as cutting without warping, straightening of warping, welding and assembly dimensional accuracy during use. In order to meet the use of steel plate materials, product quality requirements such as low internal stress and good straightness are required, so that steel plates can meet the use requirements of downstream customers. Therefore, the material has stringent comprehensive quality requirements of good quality and low price.

[0003] However, due to the particularity of the production process, the hot-rolled coil folding steel plate has an inherent disadvantage in the quality control of the internal stress of the product, which is not as good as the single-rolled steel plate rolled products; in addition, in order to control production costs, Ti micro-alloys are used to enhance the mechanical properties, and the rolling and folding processes pursue high efficiency, resulting in poor quality stability of the steel plate, which affects the control of the internal stress of the material. Summary of the invention

[0004] The main purpose of the present invention is to provide a 460MPa strength grade steel and a manufacturing method thereof, aiming to solve the problems of poor quality stability and high production cost of the 460MPa strength grade steel produced by the prior art.

[0005] To achieve the above object, the present invention provides a 460MPa strength grade steel, wherein the chemical composition mass percentage of the 460MPa strength grade steel is 0.05wt%≤C≤0.08wt%, 0.15wt%≤Si≤0.30wt%, 1.10wt%≤Mn≤1.30wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt%≤Als≤0.045wt%, 0.0 25wt%≤Ti≤0.038wt%, 0.015wt%≤Nb≤0.030wt%, N≤0.0055wt%, 0.0015wt%≤B≤0.0025wt%, Cr≤0.30wt%, and the rest are iron and other inevitable impurities; and the metallographic surface layer of the 460MPa strength grade steel has a 30-50μm decarburized layer structure, and the main microstructures are ferrite, pearlite and bainite.

[0006] The present invention also provides a method for manufacturing 460MPa strength grade steel, comprising the steps of: providing a hot-rolled material; the chemical composition mass percentage of the hot-rolled material is 0.05wt%≤C≤0.08wt%, 0.15wt%≤Si≤0.30wt%, 1.10wt%≤Mn≤1.30wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt%≤Als≤0.045wt%, 0.025wt%≤Ti≤0.038wt%, 0.015wt%≤Nb≤0.030wt%, N≤0.0055wt%, 0.0015wt%≤B≤0.0025wt%, Cr≤0.30wt%, and the rest is iron and other inevitable impurities.

[0007] When the hot-rolled material is cooled to below 60°C, it is cut into plates according to the order specification thickness to obtain 460MPa strength grade steel.

[0008] When the order specification thickness a≤18mm, the straightness ≤5mm / 2m; when the order specification thickness 18mm<a≤25mm, the straightness ≤8mm / 2m; wherein, the order specification width b is 1800~2000mm.

[0009] Furthermore, the amount of pressure reduction at the entrance of the rough straightening process of the flattened plate processing is -4mm to -8mm.

[0010] Furthermore, when the straightness does not meet the requirements, it also includes tempering heat treatment of the steel plate and re-using it as the hot-rolled material for subsequent operation steps; the temperature of the tempering heat treatment is 550°C; the insulation time of the tempering heat treatment is 1.8amin; wherein a is the order specification thickness, in mm.

[0011] Furthermore, the thickness of the hot-rolled material is 230 mm; and the center segregation and center porosity of the slab of the hot-rolled material do not exceed C1.5.

[0012] Furthermore, before the hot rolled material is cooled, the hot rolled material is sequentially subjected to dephosphorization treatment, rough rolling treatment, finishing rolling treatment and coiling treatment; wherein the finishing rolling treatment temperature is 830-850°C; and the finishing rolling treatment reduction rate is not less than 50%.

[0013] Furthermore, the rough rolling process uses a rough rolling mill with flat rolls; and the finish rolling process uses a finish rolling mill with CVC rolls.

[0014] Furthermore, between the finishing rolling process and the coiling process, the finished rolled material is also subjected to laminar cooling until the coiling temperature during the coiling process is 560-630°C; wherein the upper and lower water ratio of the laminar cooling is set to 1:1.1.

[0015] Furthermore, the hot-rolled material is obtained by sequentially performing top and bottom combined blowing converter primary refining, LF refining and CC casting on the raw materials to obtain the hot-rolled material.

[0016] Furthermore, the process of cooling to below 60° C. is specifically to take the hot-rolled material out of the warehouse for 24 hours to be cooled, and then naturally cool it to below 60° C.

[0017] The beneficial effects achieved by the present invention are:

[0018] The metallographic surface of the 460MPa strength grade steel provided by the present invention has a 30-50μm decarburized layer structure, the main microstructures are ferrite, pearlite and bainite, the grains are uniform, the yield strength of the steel plate is less than 500MPa, the plate shape is straight, and the quality stability is high.

[0019] The manufacturing method of 460MPa strength grade steel provided by the present invention enhances the hardenability of the 460MPa strength grade steel by introducing B element and Cr element into the hot-rolled material and controlling the elements 0.0015wt%≤B≤0.0025wt% and Cr≤0.30wt%. Combined with the flattening and cutting plate processing process of controlling the straightness according to the thickness of the order specification, the 460MPa strength grade steel with good plate straightness, good warping control of laser cutting materials and high forming stability is stably produced. The manufacturing method has low cost and is suitable for large-scale promotion and application. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0021] Figure 1 The material microstructure diagram of the product obtained in Example 1;

[0022] Figure 2 This is the material microstructure diagram of the product prepared in Comparative Example 1.

[0023] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] It should be noted that, in the absence of conflict, the following embodiments and features in the embodiments can be combined with each other. It should also be understood that the terms used in the embodiments of the present invention are intended to describe specific embodiments rather than to limit the scope of protection of the present invention.

[0026] Unless otherwise defined, all technical and scientific terms used in the present invention are consistent with the prior art knowledge of those skilled in the art and the description of the present invention. The present invention can also be implemented using any methods, devices and materials in the prior art that are similar or equivalent to the methods, devices and materials described in the embodiments of the present invention.

[0027] When the embodiments give numerical ranges, it should be understood that unless otherwise specified in the present invention, both endpoints of each numerical range and any value between the two endpoints can be selected. The test methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturers. The materials or reagents required in the following embodiments are commercially available unless otherwise specified.

[0028] In order to solve the problems of poor quality stability and high production cost of 460MPa strength grade steel produced by the prior art, the present invention provides a 460MPa strength grade steel, the chemical composition mass percentage of the 460MPa strength grade steel is 0.05wt%≤C≤0.08wt%, 0.15wt%≤Si≤0.30wt%, 1.10wt%≤Mn≤1.30wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt% ≤Als≤0.045wt%, 0.025wt%≤Ti≤0.038wt%, 0.015wt%≤Nb≤0.030wt%, N≤0.0055wt%, 0.0015wt%≤B≤0.0025wt%, Cr≤0.30wt%, and the rest are iron and other inevitable impurities; and the metallographic surface layer of the 460MPa strength grade steel has a 30-50μm decarburized layer structure, and the main microstructures are ferrite, pearlite and bainite.

[0029] The metallographic surface of the 460MPa strength grade steel provided by the present invention has a 30-50μm decarburized layer structure, the main microstructures are ferrite, pearlite and bainite, the grains are uniform, the yield strength of the steel plate is less than 500MPa, the plate shape is straight, and the quality stability is high.

[0030] The present invention also provides a method for manufacturing 460MPa strength grade steel, comprising the steps of: providing a hot-rolled material; the chemical composition mass percentage of the hot-rolled material is 0.05wt%≤C≤0.08wt%, 0.15wt%≤Si≤0.30wt%, 1.10wt%≤Mn≤1.30wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt%≤Als≤0.045wt%, 0.025wt%≤Ti≤0.038wt%, 0.015wt%≤Nb≤0.030wt%, N≤0.0055wt%, 0.0015wt%≤B≤0.0025wt%, Cr≤0.30wt%, and the rest is iron and other inevitable impurities. Specifically, B and Cr elements improve the hardenability of the material, but experiments have found that when the B element exceeds 30ppm, the toughness of the material will be seriously deteriorated; when the Cr element is around 0.20wt%, it can improve surface oxides, etc., and finally the composition is determined to be 0.0015wt%≤B≤0.0025wt%, and when Cr≤0.30wt%, 460MPa strength grade steel with good plate flatness, good warping control of laser cutting materials, and high forming stability can be stably produced.

[0031] When the hot-rolled material is cooled to below 60°C, it is flattened and cut into plates according to the order specification thickness to obtain 460MPa strength grade steel.

[0032] When the order specification thickness a≤18mm, the straightness ≤5mm / 2m; when the order specification thickness 18mm<a≤25mm, the straightness ≤8mm / 2m; among which, the order specification width b is 1800~2000mm.

[0033] The manufacturing method of 460MPa strength grade steel provided by the present invention, by introducing B element and Cr element into hot-rolled material and controlling 0.0015wt%≤B≤0.0025wt%, Cr≤0.30wt%, preferably, Cr: 0.20wt%, enhances the hardenability of the 460MPa strength grade steel and improves the surface oxide; combined with the flattening plate processing process of controlling the straightness according to the order specification thickness, realizes the efficient and stable production of 460MPa strength grade steel with good plate straightness and high quality stability; and the manufacturing method has low cost and is suitable for large-scale promotion and application.

[0034] Furthermore, the pressure reduction of the rough straightening entrance of the flattening process is -4mm to -8mm. When the pressure reduction of the rough straightening entrance of the flattening process is -4mm to -8mm, the internal stress of the steel plate can be effectively released to improve the stability of the 460MPa strength grade steel.

[0035] Furthermore, when the flatness does not meet the requirements, it also includes tempering heat treatment of the steel plate and reusing it as hot-rolled material for subsequent operation steps; the temperature of the tempering heat treatment is 550°C; the holding time of the tempering heat treatment is 1.8amin; where a is the order specification thickness, in mm. Specifically, when the flatness of the steel plate does not meet the above requirements, the steel plate that does not meet the flatness requirements should be tempered heat treated at 550°C for 1.8amin, and after being tempered out of the furnace, it should be rolled on the cooling bed and naturally cooled to below 60°C, and then it should be cut and flattened according to the order specification thickness.

[0036] Furthermore, the thickness of the hot-rolled material is 230 mm; and the center segregation and center porosity of the slab of the hot-rolled material do not exceed C1.5.

[0037] Furthermore, before the hot rolled material is cooled, the hot rolled material is sequentially subjected to dephosphorization, rough rolling, finishing rolling and coiling treatments; wherein the finishing rolling temperature is 830-850°C; and the finishing rolling reduction ratio is not less than 50%.

[0038] Furthermore, the rough rolling process uses a rough rolling mill with flat rolls; and the finishing rolling process uses a finishing mill with CVC rolls.

[0039] Furthermore, between the finishing and coiling processes, the finished rolled material is subjected to laminar cooling until the coiling temperature is 560-630°C during the coiling process; wherein the upper and lower water ratio of the laminar cooling is set to 1:1.1. Specifically, when the upper and lower water ratio of the laminar cooling is set to 1:1.1, uniform cooling of the upper and lower surfaces of the rolled material can be ensured.

[0040] Furthermore, the hot-rolled material is obtained by sequentially performing top and bottom combined blowing converter primary refining, LF refining and CC casting on the raw materials to obtain the hot-rolled material. Specifically, LF refining is slag deoxidation, adjusting the composition of molten steel and controlling the temperature of molten steel, and finally forming molten steel with qualified composition, high cleanliness and appropriate temperature, and CC casting is to form a slab with good surface and internal quality.

[0041] Furthermore, the process of cooling to below 60°C is specifically to take the hot-rolled material out of the warehouse for cooling for 24 hours, and then naturally cool it to below 60°C.

[0042] For further understanding of the present invention, examples are given below:

[0043] Example 1

[0044] (1) Composition of molten steel in the tundish: C: 0.075wt%, Si: 0.183wt%, Mn: 1.25wt%, P: 0.0112wt%, S: 0.0032wt%, Als: 0.0296wt%, Ti: 0.0285wt%, Nb: 0.0185wt%, Cr: 0.255wt%, N: 0.0055wt%, B: 0.0018wt%, and the rest are iron and unavoidable elements.

[0045] (2) Rolling process: Finishing rolling temperature is 830℃~850℃, coiling temperature is 570℃, laminar water ratio is 1:1.1 and laminar water height is set. The thickness of hot rolled material is 230mm, the temperature out of continuous casting furnace is 1210℃, and the total heating time is 262min. After the slab is heated, controlled rolling is carried out, and two-stage rolling is adopted. The rough rolling mill adopts flat rolls and the finishing mill adopts CVC rolls.

[0046] (3) Rolling is controlled according to the hot rolling process. The rolled steel coil is shipped out for 24 hours to be cooled. When the steel coil is naturally cooled to below 60°C, it is processed for flattening and cutting. The production specification of the order thickness is 8mm, and the pressure reduction at the entrance of the rough straightening is reduced to -4mm. The straightness of the steel plate is controlled not to exceed 5mm / 2m. If the straightness of the steel plate exceeds 5mm / 2m, it is reprocessed by heat treatment and tempering process.

[0047] (4) The straightness of the steel plate exceeds 5mm / 2m, and the steel plate is tempered. The tempering process is: temperature 550℃, holding time 36min, and then the steel plate is rolled on the cooling bed and naturally cooled to room temperature, and the straightness is 2mm / 2m.

[0048] Comparative Example 1

[0049] (1) Composition of molten steel in the tundish: C: 0.075wt%, Si: 0.153wt%, Mn: 1.32wt%, P: 0.0132wt%, S: 0.0022wt%, Als: 0.0326wt%, Ti: 0.0525wt%, Nb: 0.0225wt%, N: 0.0062wt%, and the rest are iron and unavoidable elements.

[0050] (2) Rolling process: Finishing rolling temperature is 850℃~870℃, coiling temperature is 600℃, laminar water ratio is 1:1.1 and laminar water height is set. The thickness of the ingot is 230mm, the temperature of the continuous casting ingot heating furnace is 1215℃, and the total heating time is 246min. After the slab is heated, controlled rolling is carried out, and two-stage rolling is adopted. The rough rolling mill adopts flat rolls and the finishing mill adopts CVC rolls.

[0051] (3) Rolling is controlled according to the hot rolling process. The rolled steel coil is placed in the hot coil warehouse for more than 48 hours. The steel coil is naturally cooled to below 60°C for flattening and cutting. The pressure reduction at the entrance of the rough straightening is reduced to -5mm, and the straightness of the steel plate is 8-15mm / 2m.

[0052] Analysis example 1

[0053] (1) The mechanical properties of the products obtained in Example 1 and Comparative Example 1 were compared and analyzed; the mechanical properties of the products obtained in Example 1 and Comparative Example 1 are shown in Table 1.

[0054] Table 1 Comparative analysis of mechanical properties of products obtained from Examples 1-2 and Comparative Examples 1-2

[0055]

[0056] According to Table 1, the yield and tensile mechanical properties of the material in Example 1 are relatively lower by about 30 MPa than those of the material in Comparative Example 1, and the elongation is increased by 4%. The material has good processing and forming properties.

[0057] (2) The metallographic structures of Example 1 and Comparative Example 1 were observed microscopically, and the microstructure diagrams of the materials were as follows: Figure 1 , Figure 2 shown.

[0058] from Figure 1 It can be seen that the top layer is 30-50um decarburized layer; the material microstructure is ferrite, pearlite and bainite, and the finishing and coiling temperature refines the material grain size. The addition of B element and the reduction of Ti element achieve the structural strengthening instead of partial analysis strengthening.

[0059] from Figure 2 It can be seen that the material microstructure is ferrite, pearlite and bainite; according to Figure 1 and Figure 2 It can be seen that: Figure 1 The topmost 30-50μm decarburized layer has a microstructure of ferrite, pearlite and bainite, with a finer grain size and good toughness. By using the hardenability characteristics of B and Cr elements, the addition of B and Cr elements and the reduction of Ti elements, the organization is strengthened instead of precipitation strengthening, and the mechanical properties of the material are more stable.

[0060] In summary, the above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A 460MPa strength grade steel, characterized in that: The chemical composition mass percentage of the 460MPa strength grade steel is 0.05wt%≤C≤0.08wt%, 0.15wt%≤Si≤0.30wt%, 1.10wt%≤Mn≤1.30wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt%≤Als≤0.045wt%, 0.025wt%≤Ti≤0.038wt%, 0.015wt%≤Nb≤0.030wt%, N≤0.0055wt%, 0.0015wt%≤B≤0.0025wt%, Cr≤0.30wt%, and the rest is iron and other unavoidable impurities; The surface layer of the metallographic structure of the 460MPa strength grade steel has a 30-50μm decarburized layer structure, and the main microstructures are ferrite, pearlite and bainite.

2. A method for manufacturing 460MPa strength grade steel, characterized in that: Includes steps: A hot-rolled material is provided; the chemical composition of the hot-rolled material is 0.05wt%≤C≤0.08wt%, 0.15wt%≤Si≤0.30wt%, 1.10wt%≤Mn≤1.30wt%, P≤0.02wt%, S≤0.005wt%, 0.018wt%≤Als≤0.045wt%, 0.025wt%≤Ti≤0.038wt%, 0.015wt%≤Nb≤0.030wt%, N≤0.0055wt%, 0.0015wt%≤B≤0.0025wt%, Cr≤0.30wt%, and the rest is iron and other inevitable impurities; When the hot-rolled material is cooled to below 60°C, it is cut into plates according to the order specifications to obtain 460MPa strength grade steel; When the order specification thickness a≤18mm, the straightness ≤5mm / 2m; when the order specification thickness 18mm<a≤25mm, the straightness ≤8mm / 2m; wherein, the order specification width b is 1800~2000mm.

3. The manufacturing method according to claim 2, characterized in that: The rough straightening entrance pressure reduction amount of the flattened plate processing is -4mm to -8mm.

4. The manufacturing method according to claim 2, characterized in that: When the straightness does not meet the requirement, the steel plate is subjected to tempering heat treatment and used as the hot-rolled material for subsequent operation steps; The temperature of the tempering heat treatment is 550°C; the insulation time of the tempering heat treatment is 1.8amin; wherein a is the order specification thickness, in mm.

5. The manufacturing method according to claim 2, characterized in that: The thickness of the hot-rolled material is 230 mm; and the center segregation and center porosity of the slab of the hot-rolled material do not exceed C1.

5.

6. The manufacturing method according to claim 2, characterized in that: The hot rolled material is subjected to dephosphorization treatment, rough rolling treatment, finish rolling treatment and coiling treatment in sequence before the hot rolled material is cooled; Wherein, the temperature of the finish rolling treatment is 830-850°C; and the reduction rate of the finish rolling treatment is not less than 50%.

7. The manufacturing method according to claim 6, characterized in that: The rough rolling process uses a rough rolling mill with flat rolls; the finish rolling process uses a finish rolling mill with CVC rolls.

8. The manufacturing method according to claim 6, characterized in that: The finishing process and the coiling process also include laminar cooling of the rolled material after the finishing process until the coiling temperature during the coiling process is 560-630°C; Wherein, the upper and lower water ratio of the laminar cooling is set to 1:1.

1.

9. The manufacturing method according to claim 2, characterized in that: The hot-rolled material is obtained by sequentially performing top-bottom combined blowing converter primary refining, LF refining and CC casting on the raw materials to obtain the hot-rolled material.

10. The manufacturing method according to claim 2, characterized in that: The process of cooling to below 60° C. specifically includes taking the hot-rolled material out of the warehouse for cooling for 24 hours, and then naturally cooling it to below 60° C.

Citation Information

Patent Citations

  • F+P+B type low-yield-ratio and high-strength medium steel plate and production method thereof

    CN103014520A

  • Railway steel plate with high strength and low yield ratio and good toughness and manufacturing method thereof

    CN110343966A

  • Hot rolled steel plate with yield strength being 700 MPa and manufacturing method of hot rolled steel plate

    CN111440984A

  • Production method of high-toughness bridge structure steel plate

    CN114182174A

  • High-strength marine steel plate with thickness smaller than or equal to 12 mm and manufacturing method thereof

    CN117604398A