Thermally conductive sheet
By using high-reflectivity adhesives and thermally conductive fillers in thermal conductive sheets, combined with graphite materials and grinding processes, the problem of increased thermal resistance in semiconductor equipment is solved and more efficient heat dissipation is achieved.
Patent Information
- Application Number
- CN202380026041.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-29
AI Technical Summary
In the semiconductor field, with the miniaturization and performance improvement of equipment, the heat density increases, and it is difficult for existing thermal conductive sheets to effectively reduce the thermal resistance value, especially the problem that the thermal resistance value may not be reduced after the surface roughness is reduced.
A thermally conductive sheet containing adhesive and thermally conductive filler is used. The reflectivity of its surface is above 0.30% and has no fluidity. The thermally conductive filler is oriented along the thickness direction and contains graphite material, and the adhesion force is improved through grinding to reduce the thermal resistance value.
The thermal resistance value is fully reduced, the adhesion and thermal conductivity of the thermal conductive sheet are improved, and effective heat dissipation in highly integrated semiconductor equipment is ensured.
Smart Images

Figure BDA0005031455840000071 
Figure BDA0005031455840000261 
Figure BDA0005031455840000271
Abstract
Description
Technical Field
[0001] The invention relates to a heat conducting sheet. Background Art
[0002] In electronic devices such as computers, automobile parts, and mobile phones, heat sinks and other heat dissipation bodies are usually used to release the heat generated by heat generating bodies such as semiconductor components and mechanical parts. In order to improve the heat conduction efficiency of the heat sink, it is known that a thermal conductive sheet is arranged between the heat generating body and the heat sink. When the thermal conductive sheet is arranged inside the electronic device, it is usually compressed for use, so it needs to be highly flexible. In order to further improve the heat dissipation, it is necessary to increase the thermal conductivity.
[0003] In order to further improve the conduction efficiency, the heat conducting sheet is required to have the ability to follow the heating element and the heat dissipating element. Therefore, a phase change type heat conducting sheet, which softens or melts by heating and is called a phase change sheet, has been studied. For example, Patent Document 1 discloses a heat sink, which contains at least silicone oil introduced with an alkyl group, α-olefin and a heat conductive filler, is putty-like at room temperature, and softens and flows by heating.
[0004] In addition, a thermally conductive sheet filled with a large amount of CPAO is also known. For example, Patent Document 2 discloses a thermosetting resin composition containing CPAO and a thermosetting resin and a sheet-shaped molded product thereof.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2004-331835
[0008] Patent Document 2: Japanese Patent Application Publication No. 2010-185052 Summary of the invention
[0009] Problems to be solved by the invention
[0010] However, for example, in the semiconductor field, with the miniaturization of equipment, the improvement of semiconductor performance, and the high integration of semiconductors, the heat density inside the equipment has become greater than before. Therefore, the release of heat generated inside the equipment also needs to be further improved. In view of such needs, attempts are being made to improve the efficiency of heat dissipation based on thermal conductive sheets. As a means of this, for example, it is possible to consider increasing thermal conductivity, reducing contact thermal resistance, and reducing substantial thickness.
[0011] Here, from the perspective of increasing the thermal conductivity of the thermally conductive sheet, a technique is used to orient the graphite material with high thermal conductivity in the thickness direction from the heating element toward the heat sink. In addition, from the perspective of reducing the contact thermal resistance, the surface roughness is sometimes reduced. However, if the surface roughness is reduced to a certain level, it is difficult to further reduce the surface roughness, and there is also the problem that the thermal resistance value may not be reduced by simply reducing the surface roughness.
[0012] Therefore, an object of the present invention is to provide a thermally conductive sheet used between a heat sink and a heat generator, which can sufficiently reduce the thermal resistance value.
[0013] Means of solving the problem
[0014] The present inventors have conducted intensive studies and have found that the above-mentioned problems can be solved by using a thermally conductive sheet including a binder and a thermally conductive filler and having a reflectivity of at least one surface of 0.30% or more, thereby completing the present invention.
[0015] That is, the present invention provides the following [1] to
[12] .
[0016] [1] A thermally conductive sheet comprising an adhesive and a thermally conductive filler dispersed in the adhesive, and used by being sandwiched between a heat generating body and a heat dissipating body,
[0017] The reflectivity of the surface of the thermally conductive sheet in contact with the heat generating body or the heat dissipating body is 0.30% or more.
[0018] [2] The thermally conductive sheet according to [1], which has no fluidity at 0 to 100°C.
[0019] [3] The thermally conductive sheet according to [1] or [2], wherein the thermally conductive filler includes an anisotropic filler oriented in a thickness direction of the thermally conductive sheet.
[0020] [4] The thermally conductive sheet according to any one of [1] to [3], wherein the thermally conductive filler includes a graphite material.
[0021] [5] The thermally conductive sheet according to any one of [1] to [4], wherein the reflectivity is 0.45% or more.
[0022] [6] The thermally conductive sheet according to any one of [1] to [5], wherein the binder contains cross-linked silicone.
[0023] [7] The thermally conductive sheet according to any one of [1] to [6], comprising a phase change material.
[0024] [8] The thermally conductive sheet according to [7], wherein the content of the phase change material is 2 to 30 parts by mass based on 100 parts by mass of the binder.
[0025] [9] The thermally conductive sheet according to [7] or [8], wherein the phase change material is alkyl silicone.
[0026]
[10] The thermally conductive sheet according to any one of [1] to [9], wherein the surface having a reflectivity of 0.30% or more is a cut surface.
[0027]
[11] The thermally conductive sheet according to any one of [1] to
[10] , wherein the thermally conductive sheet has an E hardness of 10 to 80.
[0028]
[12] The method for producing a thermally conductive sheet according to any one of [1] to
[11] , comprising a step of grinding a surface of a molded body including a binder and a thermally conductive filler dispersed in the binder.
[0029] Effects of the Invention
[0030] According to the present invention, a thermally conductive sheet capable of sufficiently reducing thermal resistance can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is a schematic diagram of a thermal resistance measuring instrument. DETAILED DESCRIPTION
[0032] [Thermal conductive sheet]
[0033] Hereinafter, a thermally conductive sheet according to an embodiment of the present invention will be described in detail.
[0034] The thermally conductive sheet of the present invention comprises a binder and a thermally conductive filler dispersed in the binder, and is a thermally conductive sheet used to be sandwiched between a heating element and a heat dissipating element.
[0035] <Reflectivity>
[0036] When the thermally conductive sheet of the present invention is sandwiched between a heating element and a radiator, the reflectivity of the surface in contact with the heating element or the radiator (hereinafter, also referred to as "reflectivity") is 0.30% or more. When the reflectivity is less than 0.30%, the thermal resistance of the thermally conductive sheet increases, or the adhesion of the thermally conductive sheet to the radiator or the heating element is impaired, a gap is generated between the heating element or the radiator and the thermally conductive sheet, and the thermally conductive sheet cannot fully exert its thermal conductivity.
[0037] In the present invention, the reflectivity of at least one of the surface in contact with the heating element and the surface in contact with the heat sink of the thermal conductive sheet is 0.30% or more, and preferably both surfaces are 0.30% or more. When both surfaces are 0.30% or more, the thermal conductive sheet can be closely attached to both the heat sink and the heating element, and the thermal resistance value of the thermal conductive sheet can be further reduced.
[0038] In the present invention, from the perspective of improving adhesion and more effectively reducing thermal resistance, the reflectivity is preferably 0.45% or more, more preferably 0.50% or more, and further preferably 0.55% or more. The principle of improved thermal conductivity when the reflectivity increases is still uncertain, but it is speculated that it is not only due to the improved smoothness of the surface of the thermal conductive sheet, but also due to the different grinding easiness of the resin and the thermal conductive filler, so that their ratio changes, the anisotropic filler arranged in a manner of inverted surface increases, and the side (long axis side) of the anisotropic filler arranged in a manner of inverted surface is also ground, so that the adhesion with the heating element or the heat sink becomes greater and the thermal resistance value becomes smaller.
[0039] The upper limit of the reflectivity is not particularly limited, but is practically, for example, 4.0% or less, preferably 3.5% or less, and more preferably 2.0% or less.
[0040] In addition, the reflectance can be obtained by the measuring method described in the Examples mentioned later.
[0041] <Liquidity>
[0042] The thermally conductive sheet of the present invention preferably has no fluidity at 0 to 100°C. Here, having no fluidity means that even when the thermally conductive sheet is heated from 0°C to 100°C, the components constituting the thermally conductive sheet will not flow out to the outside of the thermally conductive sheet, and the thermally conductive sheet can maintain its shape even when heated to 100°C. In this case, the thermally conductive sheet is sometimes heated and slightly deformed, but it essentially remains elastically deformed and can return to its original shape after cooling. If the thermally conductive sheet has such physical properties, when the thermally conductive sheet is sandwiched between a heat sink and a heating element for use, the components of the thermally conductive sheet will not flow out due to the heat released by the heating element, and the shape of the thermally conductive sheet can be substantially maintained. Therefore, good thermal conductivity can be exerted.
[0043] It should be noted that, as described later, when the thermally conductive sheet includes a phase change material, the shape of the thermally conductive sheet can be maintained even when the thermally conductive sheet is heated to a temperature higher than the melting point of the phase change material. That is, the phase change material itself may melt, but the melted phase change material does not flow out to the outside.
[0044] <Adhesive>
[0045] The adhesive used in the thermal conductive sheet of the present invention is a polymer compound such as an elastomer and rubber. It is preferred to use an adhesive formed by curing a liquid polymer composition (curable polymer composition) composed of a mixed system such as a main agent and a curing agent. The curable polymer composition may, for example, contain uncrosslinked rubber and a crosslinking agent, or may contain monomers, prepolymers, and a curing agent. In addition, the above-mentioned curing reaction may be room temperature curing or thermal curing. The adhesive formed by the curable polymer composition is preferably a crosslinked matrix having a crosslinked structure. In addition, the adhesive is preferably an example of a silicone matrix.
[0046] (Silicone Matrix)
[0047] The silicone matrix is preferably silicone that has no fluidity at room temperature (23° C.) and high temperature (80° C.) Since the silicone matrix has no fluidity, the thermal conductive sheet can maintain its shape at room temperature and high temperature.
[0048] In addition, as the silicone matrix of the present invention, for example, silicone rubber can be used. By using silicone rubber, compression deformation becomes easy and it is easy to assemble between the heating element and the heat sink. In addition, since a certain compression property can be given to the thermal conductive sheet, reliability can be improved.
[0049] The organosilicon used in the organosilicon matrix may be either a condensation reaction type or an addition reaction type, but the addition reaction type is preferred from the viewpoints of being easy to highly fill with thermally conductive fillers and being able to easily adjust the curing temperature using a catalyst or the like. The organosilicon matrix can be obtained, for example, by curing a curable organosilicon composition. The curable organosilicon composition can be composed, for example, of a main agent and a curing agent.
[0050] When the curable silicone composition is of an addition reaction type, it preferably contains an alkenyl group-containing organopolysiloxane as a main agent and a hydrogen organopolysiloxane as a curing agent from the viewpoint of facilitating high filling of a thermally conductive filler.
[0051] It should be noted that the curable silicone composition is preferably in a liquid state before curing. The curable silicone composition is in a liquid state before curing, so that it is easy to highly fill the thermal conductive filler. It should be noted that in this specification, liquid means liquid at room temperature (23° C.) and 1 atmosphere.
[0052] In addition, in order to ensure the shape retention of the thermally conductive sheet, the silicone matrix preferably uses a crosslinked silicone, and more preferably a three-dimensional crosslinked silicone matrix. For this purpose, for example, in the case of an addition reaction type, a curable silicone composition containing an alkenyl-containing organopolysiloxane having at least 3 alkenyl groups per molecule or a hydrogen organopolysiloxane having at least 3 hydrogen atoms added to silicon atoms can be cured.
[0053] The content of the silicone matrix may be, for example, about 5 to 50 mass %, preferably 8 to 35 mass %, and more preferably 12 to 25 mass %, based on the total amount of the thermally conductive sheet.
[0054] (Phase Change Materials)
[0055] In the thermally conductive sheet, the adhesive component preferably contains a phase change material. By containing a phase change material, the thermally conductive sheet can improve flexibility when heated, and can easily greatly improve the adhesion to the heating element or the heat sink. In addition, it is easy to increase the reflectivity of the surface of the thermally conductive sheet.
[0056] It should be noted that the thermally conductive sheet with improved adhesion is beneficial in the following applications. For example, in miniaturized and highly integrated semiconductors, the substrate is thin, so as the substrate becomes thinner, it is easy for the substrate to warp due to heat. On the other hand, the thermally conductive sheet usually has resilience, so by having a certain degree of thickness, it is easy to absorb thickness changes, and even if the substrate warps, it can be used without gaps. However, when the thickness of the thermally conductive sheet is reduced as described above, there is still a problem that it is difficult to absorb thickness changes when used in compression. Therefore, it is necessary to improve the adhesion to the heat sink or the heating element so that even if the substrate warps, it can fill the space between the heat sink and the heating element without gaps.
[0057] Phase change material is a material that changes from solid to liquid by heating. Phase change material can be a compound that is liquid at room temperature (23°C) or melted by heating to a certain temperature (for example, a temperature higher than 23°C and lower than 80°C). From the perspective of easy improvement of flexibility when heated, it is preferably solid at room temperature and 1 atmosphere. Therefore, the melting point of the phase change material is preferably higher than room temperature (23°C), more preferably above 30°C, and further preferably above 35°C.
[0058] From the viewpoint of being able to melt when heated at a high temperature (eg, 80° C.), the melting point of the phase change material is preferably 80° C. or lower, more preferably 70° C. or lower, further preferably 60° C. or lower, and further preferably 50° C. or lower.
[0059] The melting point of the phase change material is the temperature of the endothermic peak of the DTA curve measured by thermogravimetric differential thermal analysis (TGDTA) at a heating rate of 1°C / min. When the alkyl silicone is a mixture, the melting point is regarded as the maximum endothermic peak in the above temperature range.
[0060] Specific examples of phase change materials include liquid paraffin, paraffin, vaseline, poly-α-olefin (PAO), alkyl silicone, polyethylene wax, polypropylene wax, etc. It should be noted that vaseline is a semisolid hydrocarbon compound, which is a mixture of various hydrocarbon compounds such as isoparaffin, cycloparaffin, and cycloparaffin. In addition, as vaseline, for example, white vaseline defined in the Japanese Pharmacopoeia can be exemplified.
[0061] Among them, from the perspective of effectively improving the reflectivity of the surface of the thermally conductive sheet, paraffin wax, vaseline, poly-α-olefin (PAO), alkyl silicone, polyethylene wax, and polypropylene wax are preferred, and poly-α-olefin (PAO) and alkyl silicone are more preferred.
[0062] When poly-α-olefin (PAO) is used as a phase change material, crystallizable poly-α-olefin (CPAO) having crystallinity is more preferred. Poly-α-olefin is a polymer of α-olefin. The type of α-olefin is not particularly limited, and it may be a straight chain or a branched chain, and may also have a cyclic structure. Poly-α-olefin is, for example, a polymer of α-olefin having 2 to 30 carbon atoms, preferably 6 to 20 carbon atoms. Crystallizable poly-α-olefin, for example, can be made into a side chain crystallizable poly-α-olefin by increasing the number of carbon atoms of α-olefin.
[0063] The poly-α-olefin may be a polymer of a single α-olefin or a copolymer of two or more α-olefins.
[0064] Examples of the alkyl silicone include compounds having a polysiloxane skeleton in the main chain and an alkyl group. The alkyl group is an alkyl group bonded to a silicon atom, and preferably includes an alkyl group having 8 or more carbon atoms.
[0065] Among them, the alkyl silicone is preferably an alkyl silicone represented by the following formula (1).
[0066]
[0067] Here, R represents an alkyl group having 8 or more carbon atoms, and m and n are integers such that m:n is in the range of 100:0 to 50:50. The total of m and n is 20 or more and 1000 or less.
[0068] The alkyl group having 8 or more carbon atoms may be a linear alkyl group or a branched alkyl group, and is preferably a linear alkyl group.
[0069] Here, the number of carbon atoms in the alkyl group is preferably in the range of 8 to 26, and more preferably in the range of 12 to 22. When R is an alkyl group having 8 or more carbon atoms, the melting point of the alkyl silicone can be prevented from being too low. On the other hand, when R is an alkyl group having 26 or less carbon atoms, an alkyl silicone having a melting point of 80° C. or less is easily obtained.
[0070] R is not particularly limited, and is preferably dodecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl, nonadecyl, eicosyl, heneicosyl, docosyl, or the like, and more preferably octadecyl.
[0071] In addition, when m:n is 100:0, alkyl silicone becomes close to the so-called hard resin at a temperature below the melting point, and the closer m:n is to 50:50, the more it becomes like wax. In other words, by using an appropriate amount of alkyl silicone with m:n of 100:0, the thermal conductive sheet becomes hard to a certain extent, and the handling property is easily improved.
[0072] The alkyl silicone is particularly preferably polyoctadecylmethylsiloxane (R=18, m:n=100:0).
[0073] The alkyl silicone may be a compound other than the compound represented by the above formula (1), and may be, for example, an alkyl silicone having a substituent other than an alkyl group.
[0074] By using poly-α-olefin (PAO) and alkyl silicone as the above substances, the reflectivity of the surface of the thermally conductive sheet can be more effectively improved.
[0075] In addition, the phase change material may be contained alone or in combination of two or more.
[0076] The content of the phase change material is preferably 1 to 45 parts by mass, more preferably 2 to 30 parts by mass, and further preferably 5 to 20 parts by mass relative to 100 parts by mass of the adhesive. By making the content of the phase change material above the above lower limit, the reflectivity of the surface of the thermal conductive sheet can be effectively improved. In addition, by making the content of the phase change material below the above upper limit, the content ratio of the adhesive component can be made above a certain value, thereby improving the adhesion of the thermal conductive sheet, thereby effectively improving the reflectivity.
[0077] <Thermal conductive filler>
[0078] In the thermally conductive sheet of the present invention, the thermally conductive filler may be dispersed in the binder and retained in the binder.
[0079] The thermally conductive filler may be an anisotropic filler or a non-anisotropic filler, or both. The thermally conductive filler preferably contains at least an anisotropic filler, and more preferably contains both an anisotropic filler and a non-anisotropic filler. The thermally conductive sheet can easily improve thermal conductivity by containing an anisotropic filler.
[0080] The anisotropic filler is preferably oriented in one direction, specifically, preferably oriented in the thickness direction of the thermally conductive sheet. By orienting the anisotropic filler in the thickness direction, the thermal conductivity in the thickness direction can be easily improved.
[0081] It should be noted that when anisotropic fillers are oriented in the thickness direction, their major axis direction does not need to be strictly parallel to the thickness direction, and even if the major axis direction is somewhat inclined relative to the thickness direction, it is considered to be oriented in the thickness direction. Specifically, materials with a major axis direction inclined less than about 20° are also considered to be anisotropic fillers oriented in the thickness direction. If such anisotropic fillers are the majority in the thermal conductive sheet (for example, more than 60%, preferably more than 80% relative to the total amount of anisotropic fillers), they are considered to be oriented in the thickness direction.
[0082] In the above description, an example in which the anisotropic filler is oriented in the thickness direction is described as a premise, but the same is true for the case in which the anisotropic filler is oriented in other directions.
[0083] The thermally conductive sheet preferably contains a graphite material. By including a graphite material, it is easy to further improve thermal conductivity. In addition, if a graphite material is included, the reflectivity tends to be lower than that of a thermally conductive sheet without a graphite material. However, in the present invention, for a thermally conductive sheet containing a graphite material, by setting the reflectivity to a certain value or more as described above, it is also easy to improve the adhesion and thermal conductivity. The graphite material can be an anisotropic filler or a non-anisotropic material, preferably an anisotropic filler.
[0084] Relative to 100 parts by mass of the adhesive, the content of the thermally conductive filler is preferably 150 to 3000 parts by mass, more preferably 200 to 2000 parts by mass, and further preferably 300 to 1000 parts by mass. By making the thermally conductive filler more than 150 parts by mass, a certain thermal conductivity can be imparted to the thermally conductive sheet. In addition, by setting it to less than 3000 parts by mass, the reflectivity of the thermally conductive sheet can be made to be above a certain value. In addition, the proportion of the adhesive in the thermally conductive sheet can be made to be above a certain value, the adhesion of the thermally conductive sheet is increased, and the thermal resistance value can be reduced.
[0085] (Anisotropic filler)
[0086] Anisotropic fillers are fillers with anisotropic shapes and are fillers that can be oriented. As anisotropic fillers, fiber materials, flaky materials, etc. can be cited. The aspect ratio of the anisotropic filler is high, specifically, the aspect ratio exceeds 2, and the aspect ratio is preferably 5 or more. By making the aspect ratio greater than 2, it is easy to orient the anisotropic filler in one direction such as the thickness direction, and it is easy to improve the thermal conductivity of the thermal conductive sheet in one direction such as the thickness direction. In addition, the upper limit of the aspect ratio is not particularly limited, and is 100 in practical use.
[0087] It should be noted that the aspect ratio refers to the ratio of the length in the long axis direction of the anisotropic filler to the length in the short axis direction. In fibrous materials, it refers to the fiber length / fiber diameter, and in flaky materials, it refers to the length in the long axis direction / thickness of the flaky material.
[0088] The content of the anisotropic filler in the thermally conductive sheet is preferably 10 to 500 parts by mass, more preferably 30 to 300 parts by mass, and even more preferably 50 to 250 parts by mass based on 100 parts by mass of the binder.
[0089] By setting the content of the anisotropic filler to 10 parts by mass or more, it is easy to improve thermal conductivity. In addition, by setting it to 500 parts by mass or less, the viscosity of the mixed composition described later is easy to become appropriate, and the orientation of the anisotropic filler becomes good. Furthermore, the dispersibility of the anisotropic filler in the adhesive also becomes good.
[0090] When the anisotropic filler is a fiber material, the average fiber length is preferably 10 to 500 μm, more preferably 20 to 350 μm, and even more preferably 50 to 300 μm. When the average fiber length is 10 μm or more, the anisotropic fillers are in proper contact with each other inside the thermally conductive sheet, thereby ensuring a heat transfer path and improving the thermal conductivity of the thermally conductive sheet.
[0091] On the other hand, when the average fiber length is set to 500 μm or less, the volume of the anisotropic filler becomes low, and a high filling in the binder component can be achieved.
[0092] In addition, the average fiber length of the fiber material is preferably shorter than the thickness of the thermally conductive sheet. By being shorter than the thickness, the fiber material is prevented from protruding more than necessary from the surface of the thermally conductive sheet.
[0093] The above average fiber length can be calculated by observing the anisotropic filler with a microscope. More specifically, for example, the fiber lengths of 50 arbitrary anisotropic fillers can be measured using an electron microscope or an optical microscope, and the average value (arithmetic mean) can be taken as the average fiber length.
[0094] In addition, when the anisotropic filler is a flaky material, the average particle size is preferably 10 to 400 μm, more preferably 15 to 300 μm, and further preferably 20 to 200 μm. By making the average particle size 10 μm or more, the anisotropic fillers in the thermally conductive sheet are easily in contact with each other, ensuring the heat transfer path, and the thermal conductivity of the thermally conductive sheet becomes good. On the other hand, if the average particle size is 400 μm or less, the volume of the thermally conductive sheet becomes low, and the anisotropic filler can be highly filled in the adhesive component.
[0095] It should be noted that the average particle size of the flaky material can be calculated by observing the anisotropic filler with a microscope and taking the major diameter as the diameter. More specifically, for example, an electron microscope or an optical microscope can be used to measure the major diameters of 50 arbitrary anisotropic fillers and the average value (arithmetic mean) thereof can be taken as the average particle size.
[0096] The anisotropic filler may be a known material having thermal conductivity, and may have diamagnetic properties when oriented by magnetic field orientation as described below. On the other hand, the anisotropic filler may not have diamagnetic properties when oriented by flow orientation or when not oriented.
[0097] Specific examples of anisotropic fillers include carbon materials represented by carbon fibers or flaky carbon powders, metal materials represented by metal fibers or metal oxides, boron nitride or metal nitrides, metal carbides, metal hydroxides, poly(p-phenylene benzoxazole) fibers, etc. Among them, carbon materials are preferred because of their small specific gravity and good dispersibility in the binder component, and graphite materials with high thermal conductivity are more preferred. Graphite materials have antimagnetism because the graphite planes are aligned in a specified direction.
[0098] In addition, boron nitride is also preferred as an anisotropic filler. Boron nitride is not particularly limited, and is preferably used in the form of a flaky material. The flaky boron nitride may be agglomerated or non-agglomerated, and preferably a part or all of it is non-agglomerated. It should be noted that boron nitride and the like also have antimagnetism because the crystal planes are aligned in a specified direction.
[0099] In addition, the anisotropic filler is not particularly limited, and the thermal conductivity along the direction having anisotropy (i.e., the long axis direction) is generally 30 W / m·K or more, preferably 60 W / m·K or more, more preferably 100 W / m·K or more, and further preferably 200 W / m·K or more. The upper limit of the thermal conductivity of the anisotropic filler is not particularly limited, and is, for example, 2000 W / m·K or less. The thermal conductivity can be measured by a laser flash method or the like.
[0100] Anisotropic fillers can be used alone or in combination of two or more. For example, as anisotropic fillers, anisotropic fillers having at least two different average particle diameters or average fiber lengths can be used. It is believed that if anisotropic fillers of different sizes are used, the smaller anisotropic fillers enter between the relatively larger anisotropic fillers, thereby filling the anisotropic fillers into the adhesive component at a high density and improving the heat conduction efficiency.
[0101] The carbon fiber used as the anisotropic filler is preferably graphitized carbon fiber. In addition, the flaky carbon powder is preferably flaky graphite powder. As the anisotropic filler, it is preferred to use graphitized carbon fiber and flaky graphite powder in combination.
[0102] The crystal planes of graphite of graphitized carbon fiber are connected in the fiber axis direction, and have high thermal conductivity in the fiber axis direction. Therefore, by making the fiber axis direction consistent with the specified direction, the thermal conductivity in a specific direction can be improved. In addition, in flaky graphite powder, the crystal planes of graphite are connected in the in-plane direction of the flaky surface, and have high thermal conductivity in the in-plane direction. Therefore, by making the flaky surface consistent with the specified direction, the thermal conductivity in a specific direction can be improved. Graphitized carbon fiber and flaky graphite powder preferably have a high degree of graphitization.
[0103] Furthermore, if flaky graphite powder is added, the scale surface of the flaky graphite powder near the surface is polished along the polished surface during the polishing process, thereby reducing thermal resistance and improving reflectivity.
[0104] As the graphite materials such as the above-mentioned graphitized carbon fiber and flaky graphite powder, the material formed by graphitizing the following raw materials can be used. For example, condensed polycyclic hydrocarbon compounds such as naphthalene, PAN (polyacrylonitrile), condensed heterocyclic compounds such as asphalt, etc. can be listed, and graphitized mesophase asphalt, polyimide, and polybenzoxazole with high graphitization degree are particularly preferably used. For example, by using mesophase asphalt, in the spinning process described later, the asphalt is oriented along the fiber axis direction due to its anisotropy, and a graphitized carbon fiber with excellent thermal conductivity in the fiber axis direction can be obtained.
[0105] There is no particular restriction on the use of mesophase pitch in graphitized carbon fibers as long as they can be spun. Mesophase pitch can be used alone or in combination with other raw materials. However, from the perspectives of high thermal conductivity, spinnability, and quality stability, it is most preferred to use mesophase pitch alone, i.e., graphitized carbon fibers with a mesophase pitch content of 100%.
[0106] Graphitized carbon fiber can be obtained by graphitizing after being spun, infusible and carbonized in sequence, crushed or cut into a predetermined particle size, or graphitized after being pulverized or cut after being carbonized. In the case of pulverizing or cutting before graphitization, polycondensation reaction and cyclization reaction are easily carried out in the surface newly exposed to the surface due to pulverization when graphitization is carried out, so the degree of graphitization can be increased to obtain graphitized carbon fiber with further improved thermal conductivity. On the other hand, in the case of graphitizing the carbon fiber after spinning, the carbon fiber after graphitization is rigid and therefore easy to pulverize, and a carbon fiber powder with a narrow fiber length distribution can be obtained by pulverizing in a short time.
[0107] The average fiber length of the graphitized carbon fiber is preferably 10 to 500 μm, more preferably 20 to 350 μm, and further preferably 50 to 300 μm, as described above. In addition, the aspect ratio of the graphitized carbon fiber is more than 2, preferably 5 or more, as described above. The thermal conductivity of the graphitized carbon fiber is not particularly limited, and the thermal conductivity in the fiber axis direction is preferably 400 W / m·K or more, and more preferably 800 W / m·K or more.
[0108] When the thermally conductive sheet contains an anisotropic filler, the anisotropic filler may be exposed on the surface of the sheet or not, preferably exposed. The surface of the thermally conductive sheet can be a non-adhesive surface because the anisotropic filler is exposed. The thermally conductive sheet becomes the main surface of the sheet, and the anisotropic filler can be exposed on only one of the two surfaces of the sheet, or on both surfaces. Since the surface of the sheet is non-adhesive, the thermally conductive sheet can slide when assembled in an electronic device, etc., and the assembly property is improved.
[0109] (Non-anisotropic filler)
[0110] Non-anisotropic fillers are materials that impart thermal conductivity to the thermally conductive sheet alone or together with anisotropic fillers. Non-anisotropic fillers can further improve thermal conductivity by being used in combination with anisotropic fillers oriented in one direction, especially in the gaps between the oriented anisotropic fillers. Non-anisotropic fillers are fillers that are substantially non-anisotropic in shape, and are fillers that will not be oriented in a predetermined direction even in an environment where anisotropic fillers are oriented in a predetermined direction, such as under the generation of magnetic lines of force described later or under the action of shear forces.
[0111] The aspect ratio of the non-anisotropic filler is 2 or less, preferably 1.5 or less. When used in combination with an anisotropic filler, the non-anisotropic filler with a low aspect ratio is easily arranged in the gap between the anisotropic fillers, and the thermal conductivity is easily improved. In addition, by making the aspect ratio less than 2, the viscosity of the mixed composition described later can be prevented from rising, and high filling can be achieved.
[0112] Specific examples of the anisotropic filler include metals, metal oxides, metal nitrides, metal hydroxides, carbon materials, oxides other than metals, nitrides, carbides, etc. In addition, the shape of the anisotropic filler includes spherical shapes, irregular powders, etc.
[0113] Among the non-anisotropic fillers, examples of metals include aluminum, copper, nickel, etc., examples of metal oxides include aluminum oxide represented by alumina, magnesium oxide, zinc oxide, etc., and examples of metal nitrides include aluminum nitride, etc. Examples of metal hydroxides include aluminum hydroxide. Furthermore, examples of carbon materials include spherical graphite, etc. Examples of oxides, nitrides, and carbides other than metals include quartz, boron nitride, silicon carbide, etc.
[0114] Among them, alumina and aluminum are preferred, and aluminum is more preferred, because they have high thermal conductivity and can easily obtain spherical products.
[0115] As the non-anisotropic filler, the above-mentioned non-anisotropic fillers may be used alone or in combination of two or more.
[0116] The average particle size of the non-anisotropic filler is, for example, 0.1 to 200 μm. For example, when used in combination with an anisotropic filler, the average particle size of the non-anisotropic filler is preferably 0.1 to 50 μm, more preferably 0.5 to 35 μm, and further preferably 1 to 15 μm. By making the average particle size 50 μm or less, even if used in combination with an anisotropic filler, it is not easy to cause adverse conditions such as disturbing the orientation of the anisotropic filler. In addition, by making the average particle size 0.1 μm or more, the specific surface area of the non-anisotropic filler will not become larger than necessary, and even if a large amount is added, the viscosity of the mixed composition is not easy to increase, and it is easy to highly fill the non-anisotropic filler.
[0117] As the non-anisotropic filler, for example, a non-anisotropic filler having at least two different average particle diameters can be used.
[0118] In addition, when a non-anisotropic filler is used alone as a thermally conductive filler, the above-mentioned average particle size is preferably 0.1 to 200 μm, more preferably 0.5 to 100 μm, and further preferably 1 to 70 μm. In addition, in this case, from the perspective of improving the thermal conductivity of the thermally conductive sheet, it is preferred to use two or more non-anisotropic fillers with different average particle sizes in combination, and it is preferred to use a small-particle thermally conductive filler with an average particle size of 0.1 μm to 5 μm and a large-particle thermally conductive filler with an average particle size of more than 5 μm and less than 200 μm. In the case of using a small-particle thermally conductive filler and a large-particle thermally conductive filler, their mass ratio (large-particle thermally conductive filler / small-particle thermally conductive filler) is preferably 0.1 to 10, more preferably 0.3 to 7, and further preferably 1 to 5.
[0119] The average particle size of the anisotropic filler can be measured by observation using an electron microscope, etc. More specifically, for example, the particle sizes of 50 arbitrary anisotropic fillers can be measured using an electron microscope or an optical microscope, and the average value (arithmetic mean) can be taken as the average particle size.
[0120] The content of the non-anisotropic filler is preferably 50 to 2500 parts by mass, more preferably 100 to 1500 parts by mass, and further preferably 200 to 750 parts by mass relative to 100 parts by mass of the adhesive. By setting it to 50 parts by mass or more, the thermal conductivity of the thermally conductive sheet can be improved. On the other hand, by setting it to 1500 parts by mass or less, the non-anisotropic filler is appropriately dispersed in the adhesive component, and the effect of improving the thermal conductivity corresponding to the content can be obtained. In addition, it is also possible to prevent the viscosity of the mixed composition from rising above the necessary level.
[0121] (additive)
[0122] Various additives may be further added to the thermally conductive sheet of the present invention within the range that the function of the thermally conductive sheet is not impaired. As additives, for example, one or more selected from dispersants, coupling agents, adhesives, flame retardants, antioxidants, colorants, anti-settling agents, etc. may be mentioned. In addition, as described later, when a polymer composition such as a curable silicone composition is cured, a curing catalyst that promotes curing may be added as an additive. As a curing catalyst, in the case of a curable silicone composition, a platinum catalyst may be mentioned.
[0123] In addition, as described later, a compatible substance may be added to the mixed composition. The compatible substance may volatilize during the process of manufacturing the thermally conductive sheet and not remain in the thermally conductive sheet, or at least a part of the mixed compatible substance may remain.
[0124] [Physical properties and other characteristics of thermal conductive sheets]
[0125] The surface of the thermal conductive sheet with a reflectivity of 0.30% or more is preferably a cut surface. That is, in the present invention, the surface of the thermal conductive sheet that contacts the heat sink or the heating element is preferably a cut surface. By making such a surface a cut surface, the reflectivity can be effectively improved. The thermal conductive sheet can have one surface as a cut surface, or both surfaces as cut surfaces.
[0126] It should be noted that, as described later, the cut surface refers to a surface formed by cutting with a shear blade, laser, etc. After being cut, the cut surface may be further subjected to surface treatment such as grinding.
[0127] (Sealing force)
[0128] The adhesion of the thermally conductive sheet of the present invention is preferably 0.1 MPa or more, more preferably 0.45 MPa or more, and further preferably 1.0 MPa or more. By making the adhesion above the lower limit, the adhesion of the thermally conductive sheet to the heating element or the heat sink becomes sufficient, and it is not easy to produce a gap with the heating element or the heat sink, so excellent thermal conductivity can be obtained. In addition, there is no particular limit to the upper limit of the adhesion. Considering that it is easy to correct the position of the thermally conductive sheet after the thermally conductive sheet is configured once between the heating element and the heat sink, it is preferably 8 MPa or less, more preferably 5 MPa or less, and further preferably 3 MPa or less.
[0129] In addition, the adhesion can be obtained by the measurement method described in the Examples.
[0130] (Thermal resistance)
[0131] The thermal resistance value of the thermally conductive sheet of the present invention is preferably 0.18°C / W or less, more preferably 0.14°C / W or less, and further preferably 0.106°C / W or less. If the thermal resistance value is below the above upper limit value, the efficiency of heat transfer from the heating element to the heat sink via the thermally conductive sheet is improved, and excellent thermal conductivity can be obtained. In the present invention, the lower the thermal resistance value, the better, as long as it is 0°C / W or more, but in practical use, for example, it is 0.01°C / W or more, preferably 0.05°C / W or more.
[0132] It should be noted that the thermal resistance value can be obtained by the measurement method described in the Examples.
[0133] (E hardness)
[0134] The thermally conductive sheet of the present invention preferably has an E-type hardness (hereinafter also referred to as "E hardness") specified in JIS K6253 of 10 to 80, more preferably 20 to 70, and even more preferably 30 to 65. When the E hardness is equal to or greater than the lower limit, the thermally conductive sheet can be easily polished in the step (B) described below, and the reflectivity of the surface of the thermally conductive sheet can easily reach 0.30% or more. In addition, when the E hardness is equal to or less than the upper limit, a certain degree of softness can be imparted to the thermally conductive sheet, and the adhesion of the thermally conductive sheet can be easily improved.
[0135] (thickness)
[0136] The thickness of the thermally conductive sheet of the present invention is not particularly limited and can be appropriately set according to the shape and application of the electronic device on which the thermally conductive sheet is mounted, and is preferably 0.05 to 5 mm, more preferably 0.1 to 3 mm, and even more preferably 0.15 to 2 mm.
[0137] [Method for manufacturing thermally conductive sheet]
[0138] The thermally conductive sheet of the present invention can be produced, for example, by a method comprising the following steps (A) and (B).
[0139] Step (A): a step of obtaining a molded body comprising a binder and a thermally conductive filler dispersed in the binder;
[0140] Step (B): a step of polishing the surface of the molded body.
[0141] Hereinafter, each step will be described in more detail.
[0142] <Process (A)>
[0143] In step (A), it is preferred to obtain an oriented molded body in which the anisotropic filler is oriented in one direction in the thickness direction of the thermally conductive sheet, cut the oriented molded body into a sheet, and obtain a sheet-like molded body. Then, it is preferred to grind the sheet-like molded body in step (B).
[0144] Alternatively, the molded article may be obtained by mixing at least a polymer composition, a phase change material, and a thermally conductive filler to obtain a mixed composition, and curing the mixed composition. Preferably, a compatible substance is further mixed into the mixed composition.
[0145] Hereinafter, preferred embodiments of the step (A) will be described in detail.
[0146] As described above, the mixed composition for obtaining the molded body is preferably obtained by mixing a polymer composition, a phase change material, a thermally conductive filler and a compatible substance. The compatible substance is a substance that dissolves in the phase change material and is compatible with the polymer composition such as the curable silicone composition. The phase change material may have low compatibility with the polymer composition such as the curable silicone composition, but by using the compatible substance, the phase change material can be uniformly mixed in the polymer composition. Therefore, in the adhesive such as the silicone matrix obtained by curing the polymer composition, the compatible substance is also uniformly mixed.
[0147] The mixing method and mixing order of the above-mentioned components are not particularly limited as long as the above-mentioned components can be mixed to obtain a mixed composition. The polymer composition, phase change material, thermal conductive filler, compatible substance and other components optionally added as needed can be appropriately mixed in any order to obtain a mixed composition.
[0148] However, the phase change material is preferably dissolved in a compatible substance and then mixed with the polymer composition (more specifically, the main agent, curing agent, etc. constituting the polymer composition) and other components.
[0149] At this time, the mixture of the phase change material and the compatible substance, the polymer composition (or the main agent and the curing agent), the thermal conductive filler and other components optionally added as needed may be mixed in any order to obtain a mixed composition.
[0150] In this way, if the phase change material is dissolved in the compatible substance in advance in step (A), the phase change material can be mixed more uniformly in the binder.
[0151] It should be noted that, when the phase change material is dissolved in the compatible substance, it can be heated appropriately. At this time, the heating temperature is preferably heated to a temperature higher than the melting point of the phase change material, for example, it can be heated to above 40°C for dissolution. In addition, the upper limit of the heating temperature can be set to a temperature at which the polymer composition is substantially not cured during the mixing process when the main agent and the curing agent are mixed.
[0152] (Compatible substances)
[0153] The compatible substance is preferably a substance that dissolves in the phase change material and is compatible with the polymer composition such as the curable silicone composition. The compatible substance may be a component that is volatilized by heating during curing.
[0154] As the compatible substance, an alkoxysilane compound is preferably used. By using the alkoxysilane compound, bubbles and the like are not observed on the surface of the thermally conductive sheet obtained by curing, and the appearance is good.
[0155] The alkoxysilane compound used as the compatible substance is a compound having a structure in which 1 to 3 of the 4 bonds possessed by a silicon atom (Si) are bonded to an alkoxy group and the remaining bonds are bonded to an organic substituent.
[0156] Examples of the alkoxy group of the alkoxysilane compound include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a pentyloxy group, and a hexyloxy group. The alkoxysilane compound may be contained in the polymer composition in the form of a dimer.
[0157] Among the alkoxysilane compounds, alkoxysilane compounds having at least one of a methoxy group and an ethoxy group are preferred from the perspective of ease of availability. From the perspective of compatibility with the polymer composition, solubility, etc., the number of alkoxy groups possessed by the alkoxysilane compound is preferably 2 or 3, more preferably 3. Specifically, the alkoxysilane compound is preferably at least one selected from a trimethoxysilane compound, a triethoxysilane compound, a dimethoxysilane compound, and a diethoxysilane compound.
[0158] As the functional group contained in the organic substituent possessed by the alkoxysilane compound, for example, acryloyl, alkyl, carboxyl, vinyl, methacryloyl, aromatic, amino, isocyanate, isocyanurate, epoxy, hydroxyl and mercapto can be cited. Here, when a platinum catalyst is used as a curing catalyst for the polymer composition, it is preferred to select and use an alkoxysilane compound that is not likely to affect the curing reaction of the organopolysiloxane. Specifically, when an addition reaction type organopolysiloxane using a platinum catalyst is used, the organic substituent of the alkoxysilane compound preferably does not contain an amino, isocyanate, isocyanurate, hydroxyl or mercapto.
[0159] The alkoxysilane compound preferably includes an alkylalkoxysilane compound having an alkyl group bonded to a silicon atom, that is, an alkoxysilane compound having an alkyl group as an organic substituent. Therefore, dialkyldialkoxysilane compounds and alkyltrialkoxysilane compounds are preferred, and alkyltrialkoxysilane compounds are preferred.
[0160] The number of carbon atoms of the alkyl group bonded to the silicon atom may be, for example, 1 to 16. In trialkoxysilane compounds such as trimethoxysilane compounds and triethoxysilane compounds, the number of carbon atoms of the alkyl group is preferably 6 or more, more preferably 8 or more, and the number of carbon atoms is preferably 12 or less, more preferably 10 or less.
[0161] On the other hand, in dialkoxysilane compounds such as dimethoxysilane compounds and triethoxysilane compounds, the alkyl group may have 1 or more carbon atoms, and preferably 10 or less, more preferably 6 or less, and even more preferably 4 or less carbon atoms.
[0162] As the alkyl-containing alkoxysilane compound, for example, methyltrimethoxysilane, dimethyldimethoxysilane, diethyldimethoxysilane, trimethylmethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, ethyltrimethoxysilane, n-propyltrimethoxysilane, di-n-propyldimethoxysilane, di-n-propyldiethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, isobutyltrimethoxysilane, isobutyltriethoxysilane, n-hexyltrimethoxysilane, n-hexyltriethoxysilane, methylcyclohexyldimethoxysilane, methylcyclohexyldiethoxysilane, n-octyltrimethoxysilane, n-octyltriethoxysilane, n-decyltrimethoxysilane, and n-decyltriethoxysilane.
[0163] Among the alkyl group-containing alkoxysilane compounds, n-decyltrimethoxysilane, dimethyldimethoxysilane, and n-octyltriethoxysilane are more preferred, and n-decyltrimethoxysilane and n-octyltriethoxysilane are still more preferred.
[0164] The alkoxysiloxane compound used as the compatibilizing material has two or more siloxane bonds and has a structure in which an alkoxy group is bonded to at least one silicon atom. The alkoxysiloxane compound has a structure in which an organic substituent is bonded to at least one silicon atom among the silicon atoms constituting the siloxane bonds.
[0165] Examples of the alkoxy group and organic substituent of the alkoxysiloxane compound include those exemplified in the above description of the alkoxysilane compound, and it is preferred that the alkoxy group and organic substituent of the alkoxysiloxane compound be at least an alkyl group.
[0166] Examples of the alkoxysiloxane compound include methylmethoxysiloxane oligomer, methylphenylmethoxysiloxane oligomer, methylepoxymethoxysiloxane oligomer, methylmercaptomethoxysiloxane oligomer, and methacryloylmethoxysiloxane oligomer.
[0167] The alkoxysiloxane compound may be used alone or in combination of two or more.
[0168] As the hydrocarbon solvent used as the compatible substance, an aromatic hydrocarbon solvent can be mentioned. Among them, from the perspective of compatibility with the polymer composition, an aromatic hydrocarbon solvent is preferred. As the aromatic hydrocarbon solvent, an aromatic hydrocarbon solvent having about 6 to 10 carbon atoms can be mentioned, for example, toluene, xylene, mesitylene, ethylbenzene, propylbenzene, butylbenzene, tert-butylbenzene, etc. can be mentioned, preferably toluene, xylene, etc.
[0169] The content of the compatible substance is preferably 10 to 50 parts by mass, more preferably 15 to 40 parts by mass, and further preferably 20 to 35 parts by mass, relative to 100 parts by mass of the polymer composition (when silicone is used, it is a curable silicone composition). When the content of the compatible substance is above the above lower limit, the thermal conductive filler is easily dispersed in the polymer composition. In addition, if the content of the compatible substance is below the above upper limit, an effect commensurate with the amount of the compatible substance used can be obtained.
[0170] In step (A), as described above, it is preferred that the mixed composition is formed into an oriented molded body. The mixed composition is preferably cured to form an oriented molded body. More specifically, the oriented molded body can be obtained by a magnetic field orientation method or a flow orientation method, among which the magnetic field orientation method is preferred.
[0171] (Magnetic field orientation method)
[0172] In the magnetic field orientation method, a mixed composition including a polymer composition such as a liquid curable silicone composition that becomes a silicone matrix after curing and a thermally conductive filler containing at least an anisotropic filler is injected into the interior of a mold, etc., and then placed in a magnetic field to orient the anisotropic filler along the magnetic field, and then the polymer composition is cured to obtain an oriented molded body. As the oriented molded body, it is preferred to form a block-shaped oriented molded body.
[0173] In addition, a release film may be arranged inside the mold at the portion in contact with the mixed composition. The release film may be, for example, a resin film with good release properties or a resin film treated with a release agent on one side. By using the release film, the oriented molded body can be easily released from the mold.
[0174] In order to carry out magnetic field orientation, the viscosity of the mixed composition used in the magnetic field orientation method is preferably 10 to 300 Pa·s. By setting it to 10 Pa·s or more, anisotropic fillers and non-anisotropic fillers are not easy to settle. In addition, by setting it to 300 Pa·s or less, the fluidity becomes good, the anisotropic filler is properly oriented in the magnetic field, and the undesirable situation that the orientation takes too much time will not occur. It should be noted that the viscosity refers to the viscosity measured at a rotation speed of 10 rpm at 25°C using a rotational viscometer (Brookfield viscometer DV-E, rotor SC4-14).
[0175] However, when an anisotropic filler or a non-anisotropic filler that is difficult to settle is used, or when an additive such as an anti-settling agent is used in combination, the viscosity of the mixed composition may be less than 10 Pa·s.
[0176] In the magnetic field orientation manufacturing method, as a magnetic field line generating source for applying magnetic field lines, superconducting magnets, permanent magnets, electromagnets, etc. can be listed, but from the perspective of being able to generate a magnetic field with a high magnetic flux density, superconducting magnets are preferred. The magnetic flux density of the magnetic field generated from these magnetic field line generating sources is preferably 1 to 30 Tesla. If the magnetic flux density is set to more than 1 Tesla, the above-mentioned anisotropic filler composed of carbon materials, etc. can be easily oriented. In addition, by setting it to less than 30 Tesla, actual manufacturing can be performed.
[0177] The curing of a polymer composition such as a curable silicone composition can be performed by heating, for example, at a temperature of about 50 to 150° C. The heating time is, for example, about 10 minutes to 3 hours.
[0178] (Flow Orientation Method)
[0179] In the flow orientation method, a shear force is applied to the mixed composition to produce a pre-sheet in which the anisotropic filler is oriented in the surface direction, a plurality of sheets are laminated to produce a laminated block, and the laminated block is made into an oriented molded body.
[0180] More specifically, in the flow orientation method, first, as described above, a mixed composition containing at least a polymer composition and a thermally conductive filler containing at least an anisotropic filler is prepared. Here, the polymer compound used in the polymer composition may include a polymer compound that is liquid at room temperature (23° C.) or a polymer compound that is solid at room temperature.
[0181] In order to apply shear force when the mixed composition is stretched into a sheet, the mixed composition should have a relatively high viscosity. Specifically, the viscosity of the mixed composition is preferably 3 to 50 Pa·s. In order to obtain the above viscosity, a solvent is preferably added to the mixed composition.
[0182] Next, the mixed composition is stretched flatly while applying shear force to form a sheet (prepared sheet). By applying shear force, the anisotropic filler can be oriented in the shear direction. As a means of forming the sheet, for example, the mixed composition can be applied on the substrate film by a coating applicator such as a rod coater or a scraper, or by extrusion molding, spraying from a nozzle, etc., and then, it is dried as needed, or the mixed composition is semi-cured. The thickness of the spare sheet is preferably about 50 to 250 μm. In the spare sheet, the anisotropic filler is oriented in one direction along the surface direction of the sheet.
[0183] Next, after overlapping and laminating multiple spare sheets in the same orientation direction, the mixed composition is cured by heating, ultraviolet irradiation, etc. as needed, and the spare sheets are bonded to each other by heat pressing, etc., thereby forming a laminated block, and the laminated block is made into an oriented molded body.
[0184] Next, the oriented molded body obtained above is cut perpendicularly to the orientation direction of the anisotropic filler by slicing or the like to obtain a sheet-like molded body. Slicing can be performed, for example, by a shear blade, laser, or the like.
[0185] <Process (B)>
[0186] In step (B), the molded product such as the sheet-like molded product obtained in step (A) is ground. The molded product is usually a sheet-like molded product as described above, and one or both surfaces of the sheet-like molded product may be ground.
[0187] The surface can be polished using, for example, polishing paper, polishing film, polishing cloth, polishing tape, etc. In the present production method, by polishing the surface of the sheet-like molded body, the reflectivity of the surface in contact with the heat sink or heating element can be made 0.30% or more.
[0188] As the properties of the grinding paper, it is preferred that the average particle size (D50) of the abrasive contained therein is 0.1 to 100 μm, and more preferably 9 to 60 μm. By using grinding paper with an average particle size of 0.1 μm or more, the reflectivity of the sheet surface can be made to be 0.30% or more. In addition, by using grinding paper with an average particle size of 100 μm or less, damage that causes practical problems on the surface of the thermal conductive sheet is prevented. In addition, based on the same reasons as above, the particle size of the abrasive as grinding paper, for example, is preferably #120 to 20000, more preferably #300 to 15000, and further preferably #320 to 6000.
[0189] The grinding method may be, in addition to grinding by continuously contacting the surface of the thermal conductive sheet with grinding paper in the same straight line direction, grinding by reciprocating a certain distance, grinding by rotating in the same direction, or grinding by contacting in various directions.
[0190] In addition, regarding the degree of polishing, for example, it can be performed while observing the surface state. For example, in the case of reciprocating polishing, 10 to 500 reciprocations are preferred, 30 to 300 times are more preferred, and 55 to 150 times are further preferred. Specifically, it is preferred to polish until the reflectivity of the surface of the thermal conductive sheet reaches 0.30% or more.
[0191] The surface of the thermally conductive sheet is preferably ground in two grinding steps. In this case, the average particle size of the grinding paper used in the first grinding step is preferably 3 to 40 μm larger than the average particle size of the grinding paper used in the second grinding step, more preferably 5 to 30 μm larger, and further preferably 10 to 25 μm larger.
[0192] In addition, it is preferred that the particle size of the grinding paper is different in the first grinding step and the second grinding step. The particle size of the grinding paper is more preferably larger in the first grinding step than in the second grinding step. The particle size of the grinding paper in the first grinding step is preferably larger than that of the grinding paper in the second grinding step by #500 to 8000, more preferably larger by #800 to 5000, and further preferably larger by #1000 to 3500.
[0193] Furthermore, the number of polishing times in the first polishing step is preferably 3 to 120 times more than the number of polishing times in the second polishing step, more preferably 5 to 100 times more, and even more preferably 8 to 80 times more.
[0194] As described above, if the polishing step is performed in two steps, relatively coarse polishing is performed in the first step and fine polishing is performed in the second step, so that the reflectivity of the surface can be easily made to be 0.30% or more.
[0195] [How to use the thermal conductive sheet]
[0196] The thermally conductive sheet of the present invention can be used inside electronic devices, etc. Specifically, the thermally conductive sheet is interposed between the heating element and the heat sink, and is used to conduct heat from the heating element to the heat sink. Specifically, the thermally conductive sheet is interposed between the heating element and the heat sink, and conducts the heat generated by the heating element to move it to the heat sink, so that the heat is dissipated from the heat sink. Here, as the heating element, various electronic components such as CPU, power semiconductor, power supply, etc. used inside the electronic device can be listed. In addition, as the heat sink, radiator, heat pump, metal housing of electronic equipment, etc. can be listed. The two surfaces of the thermally conductive sheet are respectively in close contact with the heating element and the heat sink, and can be used after being compressed.
[0197] Example
[0198] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.
[0199] [physical properties]
[0200] Various physical properties of thermal conductivity were measured by the following methods.
[0201] <Reflectivity>
[0202] The reflectance was measured using the following measuring equipment and under the following measuring conditions.
[0203] ·Measurement equipment: "UV-1900i" manufactured by Shimadzu Corporation
[0204] Measurement conditions: The regular reflection of the test piece prepared in each example and comparative example was measured when the light source was 550 nm, the incident angle was 5 degrees, and the reflectance when the standard mirror (the same plate was silver-plated) was designated as 100%.
[0205] <E Hardness>
[0206] The thermally conductive sheets obtained in the examples and comparative examples were stacked to a thickness of 10 mm to prepare test pieces, and the E hardness of the test pieces was measured using an E-type hardness tester in accordance with JIS K 6253, which is Japanese Industrial Standards.
[0207] <Thermal resistance value>
[0208] Thermal resistance, use Figure 1 The thermal resistance measuring instrument shown is measured by the method shown below.
[0209] Specifically, for each sample, a test piece S with a size of 30 mm × 30 mm and a thickness of 1 mm was prepared for this test. Then, each test piece S was attached to a copper block 22 with a measuring surface of 25.4 mm × 25.4 mm and a side covered with a heat insulating material 21, and clamped with an upper copper block 23. A load was applied through a load sensor 26, and the thickness was set to 90% of the original thickness. Here, the lower copper block 22 was in contact with a heater 24. In addition, the upper copper block 23 was covered with a heat insulating material 21 and connected to a radiator 25 with a fan. Next, the heater 24 was heated at a heat output of 25 W, and 10 minutes after the temperature became roughly stable, the temperature (θ j0 ), the temperature of the copper block 22 below (θ j1 ), and the heat generation (Q) of the heater, the thermal resistance value of each sample was calculated by the following formula (1).
[0210] Thermal resistance = (θ j1 -θ j0 ) / Q···Formula (1)
[0211] In formula (1), θ j1 is the temperature of the copper block 22 below, θ j0 is the temperature of the upper copper block 23, and Q is the calorific value.
[0212] <Close fit>
[0213] The adhesion (tensile shear strength) was measured in accordance with the tensile shear test of JIS K6850:1999.
[0214] The thermally conductive sheet (20 mm long, 20 mm wide, 0.2 mm thick) produced by the methods of each embodiment and comparative example is sandwiched between two aluminum sheets (30 mm long, 100 mm wide, 0.012 mm thick). At this time, the front ends of the aluminum sheets are arranged so as to overlap each other with a length of 25 mm × 25 mm. Then, the test sample is produced by crimping at a temperature of 80°C and a pressure of 20 psi for 3 minutes. The test sample is naturally cooled to 25°C, and a tensile test is carried out using a tensile testing machine (produced by Toyo Seiki Seisaku-sho, Ltd.) at room temperature of 25°C and a tensile speed of 500 mm / min to measure the adhesion (tensile shear strength).
[0215] <Surface roughness (arithmetic mean height Sa)>
[0216] In Examples 1, 5, 9, and Comparative Example 7, the surface roughness (arithmetic mean height Sa) was measured by the following method, and the influence of the surface roughness was evaluated.
[0217] The surface properties of the thermally conductive sheets of each example and comparative example were analyzed using a laser microscope (VK-X150 manufactured by Keyence Corporation) in accordance with ISO 25178. Specifically, the surface profile of a two-dimensional region with a surface area of 1000 μm × 1000 μm was measured by a laser method at a lens magnification of 10 times. The average value of three measurements of the same sample was taken as the arithmetic mean height (Sa).
[0218] [Example 1]
[0219] First, the following materials (1) to (5) were mixed according to the formulation described in Table 1 to obtain a mixed composition. In order to obtain the mixed composition, the component (3) was dissolved in the component (2) and then mixed with the other components.
[0220] (1) Curable silicone composition: alkenyl-containing organopolysiloxane and hydrogen organopolysiloxane (total 100 parts by mass)
[0221] (2) Compatible material: 32 parts by mass of n-decyltrimethoxysilane
[0222] (3) Phase change material 1: 18 parts by weight of polyoctadecylmethylsiloxane (melting point 50° C.)
[0223] (4) Anisotropic filler: Carbon fiber 1 (graphitized carbon fiber with an average fiber length of 100 μm, aspect ratio of 10, and thermal conductivity of 500 W / m·K in the fiber axis direction) 187 parts by mass, Carbon fiber 2 (graphitized carbon fiber with an average fiber length of 150 μm, aspect ratio of 15, and thermal conductivity of 500 W / m·K in the fiber axis direction) 12 parts by mass, Flake graphite powder (average particle size of 130 μm, aspect ratio of 10, thermal conductivity of 550 W / m·K) 23 parts by mass
[0224] (5) Non-anisotropic filler: 35 parts by mass of alumina (spherical, average particle size 3 μm, aspect ratio 1.0), 285 parts by mass of aluminum powder (irregular shape, average particle size 3 μm)
[0225] Next, the mixed composition is injected into a mold set to be thicker than the thermal conductive sheet, and an 8T magnetic field is applied in the thickness direction to orient the carbon fibers in the thickness direction. The mixture is then heated at 80°C for 60 minutes to solidify the matrix and obtain a block-shaped oriented molded body.
[0226] Next, the block-shaped oriented compact was sliced into sheets having a thickness of 1 mm and 0.2 mm using a shear knife to obtain a sheet-shaped compact.
[0227] Next, the two surfaces of the sheet-like molded body were reciprocated 25 times using coarse-mesh grinding paper A (grain size #800) with an average particle size (D50) of 20 μm, and then further reciprocated 10 times using coarse-mesh grinding paper B (grain size #4000) with an average particle size (D50) of 3 μm, and then heated at 150°C for 2 hours to obtain a thermally conductive sheet.
[0228] [Examples 2 to 5]
[0229] A thermally conductive sheet was obtained by the same method as in Example 1 except that the formulation of the mixed composition was changed as shown in Table 1.
[0230] It should be noted that the phase change material 2 is as follows.
[0231] Phase change material 2: side chain crystalline poly-α-olefin (CPAO, melting point 42°C)
[0232] Table 1
[0233]
[0234] [Examples 6 to 17]
[0235] A thermally conductive sheet was obtained by the same method as in Example 1 except that the formulation of the mixed composition and the number of reciprocating grinding were changed as shown in Tables 2 and 3.
[0236] Table 2
[0237]
[0238] Table 3
[0239]
[0240] [Comparative Examples 1 to 7]
[0241] A thermally conductive sheet was obtained by the same method as in Example 1 except that the formulation of the mixed composition and the number of reciprocating grinding were changed as shown in Table 4.
[0242] Table 4
[0243]
[0244] From the above examples, it can be seen that the thermally conductive sheet that meets the requirements of the present invention has high adhesion to the heating element and the heat sink, low thermal resistance, and thus good thermal conductivity. In addition, the adhesion to the polished surface of the material containing the phase change material is significantly improved.
[0245] In contrast, the thermally conductive sheet produced in the comparative example lacked the above-mentioned adhesion, had a high thermal resistance value, and could not obtain good thermal conductivity.
[0246] In addition, the measurement and examination results about the surface roughness (arithmetic mean height Sa) are as follows.
[0247] The thickness of Example 1 is 6.9 μm, that of Example 5 is 5.5 μm, that of Example 9 is 5.6 μm, and that of Comparative Example 7 is 10.1 μm.
[0248] Here, when Example 1 is compared with Comparative Example 7, it can be seen that when Sa is reduced, the thermal resistance value is also reduced, but when Example 1 is compared with Examples 5 and 9, it can be seen that even if Sa is reduced, the thermal resistance value is not necessarily reduced. In addition, in the comparison between Example 5 and Example 9, although Sa is the same, the thermal resistance value is 0.125°C / W in Example 5 and 0.100°C / W in Example 9, with a difference of 0.025°C / W.
[0249] On the other hand, regarding the thermally conductive sheets produced in Examples 1, 5, 9, and Comparative Example 7, a correlation between the reflectivity and the thermal resistance value was observed.
[0250] From the above results, it can be seen that in the region where the thermal resistance value is extremely small, the thermal resistance value will not necessarily be reduced simply by reducing the surface roughness.
[0251] Explanation of symbols
[0252] 21 Insulation materials
[0253] 22 Copper block below
[0254] 23 Copper block above
[0255] 24 Heater
[0256] 25 Radiator
[0257] 26 Load Sensor
[0258] S test piece
[0259] θ j0 The temperature of the upper copper block
[0260] θ j1 The temperature of the copper block below
Claims
1. A thermally conductive sheet comprising an adhesive and a thermally conductive filler dispersed in the adhesive, and being sandwiched between a heating element and a heat dissipating element for use, The reflectivity of the surface of the thermally conductive sheet in contact with the heat generating body or the heat dissipating body is 0.30% or more. 2 . The thermally conductive sheet according to claim 1 , which has no fluidity at 0 to 100° C. 3 . The thermally conductive sheet according to claim 1 , wherein the thermally conductive filler includes an anisotropic filler oriented in a thickness direction of the thermally conductive sheet. 4 . The thermally conductive sheet according to claim 1 , wherein the thermally conductive filler comprises a graphite material. 5 . The thermally conductive sheet according to claim 1 , wherein the reflectivity is 0.45% or more. 6 . The thermally conductive sheet according to claim 1 , wherein the adhesive comprises cross-linked silicone. 7 . The thermally conductive sheet according to claim 1 , comprising a phase change material. 8 . The thermally conductive sheet according to claim 7 , wherein a content of the phase change material is 2 to 30 parts by mass based on 100 parts by mass of the binder. 9 . The thermally conductive sheet according to claim 7 , wherein the phase change material is alkyl silicone. 10 . The thermally conductive sheet according to claim 1 , wherein the surface having a reflectivity of 0.30% or more is a cut surface. 11 . The thermally conductive sheet according to claim 1 , wherein the thermally conductive sheet has an E hardness of 10 to 80. 12 . The method for producing a thermally conductive sheet according to claim 1 , comprising a step of polishing a surface of a molded body including a binder and a thermally conductive filler dispersed in the binder.