Cylindrical nonaqueous electrolyte secondary battery
By winding the positive electrode and the negative electrode through a separator in a cylindrical non-aqueous electrolyte secondary battery, and providing multiple leads at the exposed parts of the current collector, the problem of electrode warpage and roundness that is difficult to improve is solved, and high performance is achieved. Battery design for increased capacity and long-term reliability.
Patent Information
- Application Number
- CN202380022812.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-15
- Publication Date
- 2024-10-29
AI Technical Summary
In existing cylindrical non-aqueous electrolyte secondary batteries, the negative electrode lead arrangement makes it difficult to improve electrode warpage and roundness, affecting its high capacity and long-term reliability.
By winding the long positive and negative electrodes through the separator, protruding parts of the positive and negative electrode leads are provided, and a plurality of current collector exposed parts are arranged at the current collector exposed parts of the positive and negative electrodes to ensure the fixation and non-contamination of the leads. Fix the exposed parts to reduce the warping of the electrodes, and increase the density of the electrodes through the arrangement of spacers and insulating tape.
It achieves high capacity and high output of the electrode, while improving the long-term reliability of the battery and reducing the risk of electrode warping and active material falling off.
Smart Images

Figure CN118872142A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a cylindrical nonaqueous electrolyte secondary battery. Background Art
[0002] Non-aqueous electrolyte secondary batteries, especially lithium-ion secondary batteries, are used as the main power source for mobile devices such as mobile communication devices and portable electronic devices because they can easily achieve high energy density and obtain high voltage. Furthermore, in recent years, non-aqueous electrolyte secondary batteries have been installed in automobiles and power storage systems, and high capacity, high output, and long-term aging resistance are desired.
[0003] In addition, it is known that for the requirement of high output, if leads are set at both ends of the long side direction of the negative electrode in the nonaqueous electrolyte secondary battery, low resistance can be achieved. Furthermore, the high capacity of nonaqueous electrolyte secondary batteries is in development. If there is a structure with a negative electrode lead in the central part of the electrode body, it is believed that the shape of the electrode body is easy to become a distorted shape and it is difficult to improve the roundness of the electrode body. And, for this reason, the maximum diameter of the electrode body increases, and when the electrode body is inserted into a shell of a given size, the electrode body is easy to interfere with the shell, and it is believed that it is difficult to carry out high capacity.
[0004] In this context, the cylindrical non-aqueous electrolyte secondary battery described in Patent Document 1 sets both the positive electrode lead and the negative electrode lead at a location corresponding to a position between 1 / 3 and 2 / 3 of the radius of the electrode body. In this way, the battery has low resistance by shortening the current collection path, and the roundness of the electrode body is also improved, thereby achieving high capacity. Furthermore, in the cylindrical non-aqueous electrolyte secondary battery, a double-sided mixture uncoated portion and a single-sided mixture uncoated portion are continuously formed at a position in the positive electrode corresponding to a position between 1 / 3 and 2 / 3 of the radius of the electrode body. In this way, the positive electrode side opposite to the negative electrode mixture uncoated portion of the portion where the negative electrode lead is installed can be reliably made an uncoated portion, thereby preventing lithium precipitation.
[0005] Prior Art Literature
[0006] Patent Literature
[0007] Patent Document 1: U.S. Patent Application Publication No. 2021 / 023044 Summary of the invention
[0008] The cylindrical non-aqueous electrolyte secondary battery described in Patent Document 1 is easy to achieve high capacity and high output because both the positive electrode lead and the negative electrode lead are fixed at a position corresponding to the position between 1 / 3 and 2 / 3 of the radius of the electrode body. However, in the cylindrical non-aqueous electrolyte secondary battery described in Patent Document 1, the uncoated portion of the positive electrode mixture on one side is asymmetrically shaped across the positive electrode collector, so it is easy to warp in the long side direction of the positive electrode during rolling. When the insulating tape is pasted on the exposed portion of the positive electrode collector, the insulating tape is easy to be pasted when the positive electrode is bent, and the short-circuit prevention effect of the insulating tape may be reduced, and the positive electrode is easy to break. Furthermore, for the single-sided positive electrode mixture coating portion, since the positive electrode mixture layer does not exist on one side, it is difficult to compress during rolling compared to the positive electrode mixture double-sided coating portion, and it is difficult to make the positive electrode mixture layer high density. Therefore, if charge and discharge are repeated, the active material is likely to fall off at the boundary between the double-sided coating portion and the single-sided coating portion, and the reliability during long-term use is difficult to improve. Therefore, the purpose of the present disclosure is to provide a cylindrical non-aqueous electrolyte secondary battery that is easy to achieve high capacity and high output, and can suppress the warping of the electrode, and the reliability during long-term use is also easy to improve.
[0009] In order to solve the above-mentioned problems, the cylindrical non-aqueous electrolyte secondary battery involved in the present disclosure comprises: an electrode body, which is obtained by winding a long positive electrode and a long negative electrode via a separator, the positive electrode including a positive electrode collector and a positive electrode mixture layer arranged on both sides of the positive electrode collector, and the negative electrode including a negative electrode collector and a negative electrode mixture layer arranged on both sides of the negative electrode collector; a positive electrode lead, which is fixed to the positive electrode collector and includes a protrusion protruding from a first side in the height direction of the electrode body; and a negative electrode lead, which is fixed to the negative electrode collector and includes a protrusion protruding from a second side in the height direction of the electrode body, the positive electrode has two or more two-sided positive electrode collector exposure portions in approximately the same area in the long side direction of the positive electrode on both sides of the positive electrode first side and the positive electrode second side, the positive electrode collector is exposed in the two-sided positive electrode collector exposure portions, and the two or more two-sided positive electrode collector exposure portions are arranged at a point from the starting end and the ending end of the winding. The two sides have portions separated by a gap in the long side direction of the positive electrode, and are arranged at a gap from each other in the long side direction of the positive electrode, more than two positive electrode collector exposure portions on both sides include a lead fixed exposure portion to which a positive electrode lead is fixed and a lead non-fixed exposure portion to which a positive electrode lead is not fixed, the negative electrode has more than two negative electrode mixture layer forming portions on both sides where a negative electrode mixture layer exists in approximately the same area in the long side direction of the negative electrode on both sides of the negative electrode first side and the negative electrode second side, and has at least one negative electrode collector exposure portion on both sides where a negative electrode collector is exposed in approximately the same area in the long side direction of the negative electrode on both sides of the negative electrode first side and the negative electrode second side, the negative electrode collector exposure portions on both sides are opposite to the positive electrode collector exposure portions on both sides via spacers, the negative electrode lead is fixed to the negative electrode collector exposure portions on both sides, and at least a portion of the positive electrode lead is arranged at a position overlapping in the height direction at a negative electrode lead opposing position in the positive electrode where the negative electrode lead is opposite to the negative electrode lead via the spacer.
[0010] It should be noted that the above-mentioned "approximately the same" requirement is met under the same circumstances, and in the comparison of the same circumstances, the above-mentioned "approximately the same" requirement is also met when the difference is smaller than the case where the size is only different from the tolerance (the maximum error generated in manufacturing). In addition, in the comparison with the same situation, the above-mentioned "approximately the same" requirement is also met when the difference is smaller than the case where the size is twice the size of the difference tolerance (the maximum error generated in manufacturing). This difference makes it easy to achieve high capacity and high output, and can suppress the warping of the electrode and improve the reliability during long-term use.
[0011] According to the cylindrical nonaqueous electrolyte secondary battery of the present disclosure, it is easy to achieve high capacity and high output, and warping of the electrode can be suppressed, and reliability during long-term use can be easily improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1It is a cross-sectional view in the axial direction of a cylindrical nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure.
[0013] Figure 2 It is a perspective view of an electrode body of the nonaqueous electrolyte secondary battery.
[0014] Figure 3A It is a plan view showing the outer surface of the rolled positive electrode, the positive electrode lead, and the insulating tape in the positive electrode that has been unfolded into a long strip.
[0015] Figure 3B It is a plan view showing the inner surface of the rolled positive electrode, the positive electrode lead, and the insulating tape in the positive electrode that has been unfolded into a long strip.
[0016] Figure 3C It is a plan view showing the outer surface of the rolled negative electrode, the negative electrode lead, and the insulating tape in the negative electrode that has been unfolded into a long strip.
[0017] Figure 3D It is a plan view showing the inner surface of the negative electrode rolled into a long strip, the negative electrode lead, and the insulating tape.
[0018] Figure 4A It is a plan view showing the outer surface of the rolled positive electrode, the positive electrode lead, and the insulating tape of the cylindrical lithium ion secondary battery of Example 2, which is unfolded into a long strip.
[0019] Figure 4B It is a plan view showing the inner surface of the rolled positive electrode, the positive electrode lead, and the insulating tape in the cylindrical lithium ion secondary battery of Example 2, which is unfolded into a long strip.
[0020] Figure 4C It is a plan view showing the outer surface of the rolled negative electrode, the negative electrode lead, the negative electrode lead at the winding end side, and the insulating tape in the rolled negative electrode of the cylindrical lithium ion secondary battery of Example 2.
[0021] Figure 4D It is a plan view showing the inner surface of the rolled negative electrode, the negative electrode lead, the negative electrode winding end side negative electrode lead, and the insulating tape in the cylindrical lithium ion secondary battery of Example 2, which is unfolded into a long strip.
[0022] Figure 5A It is a plan view showing the outer surface of the rolled positive electrode, the positive electrode lead, and the insulating tape of the cylindrical lithium ion secondary battery of Comparative Example 1, which is unfolded into a long strip.
[0023] Figure 5B It is a plan view showing the inner surface of the rolled positive electrode, the positive electrode lead, and the insulating tape of the cylindrical lithium ion secondary battery of Comparative Example 1, which is unfolded into a long strip.
[0024] Figure 5CIt is a plan view showing the outer surface of the rolled negative electrode, the negative electrode lead, and the insulating tape of the cylindrical lithium ion secondary battery of Comparative Example 1, which is unfolded into a long strip.
[0025] Figure 5D It is a plan view showing the inner surface of the rolled negative electrode, the negative electrode lead, and the insulating tape of the cylindrical lithium ion secondary battery of Comparative Example 1, which is unfolded into a long strip.
[0026] Fig. 6A It is a plan view showing the outer surface of the rolled positive electrode, the positive electrode lead, and the insulating tape of the cylindrical lithium ion secondary battery of Comparative Example 2, which is unfolded into a long strip.
[0027] Figure 6B It is a plan view showing the inner surface of the rolled positive electrode, the positive electrode lead, and the insulating tape of the cylindrical lithium ion secondary battery of Comparative Example 2, which is unfolded into a long strip.
[0028] Figure 6C It is a plan view showing the outer surface of the rolled negative electrode, the negative electrode lead inside the rolled negative electrode, the negative electrode lead at the winding end side, and the insulating tape of the cylindrical lithium ion secondary battery of Comparative Example 2, which is unfolded into a long strip.
[0029] Fig.6D It is a plan view showing the inner surface of the rolled negative electrode, the negative electrode lead on the inner side of the rolled negative electrode, the negative electrode lead on the winding end side, and the insulating tape of the cylindrical lithium ion secondary battery of Comparative Example 2, which is unfolded into a long strip.
[0030] Fig. 7A It is a plan view showing the outer surface of the rolled positive electrode, the positive electrode lead, and the insulating tape of the cylindrical lithium ion secondary battery of Comparative Example 3, which is unfolded into a long strip.
[0031] Figure 7B It is a plan view showing the inner surface of the rolled positive electrode, the positive electrode lead, and the insulating tape of the cylindrical lithium ion secondary battery of Comparative Example 3, which is unfolded into a long strip.
[0032] Figure 7C It is a plan view showing the outer surface of the rolled negative electrode, the negative electrode lead on the winding end side, and the insulating tape in the cylindrical lithium ion secondary battery of Comparative Example 3, which is unfolded into a long strip.
[0033] Fig.7D It is a plan view showing the inner surface of the rolled negative electrode, the negative electrode lead on the winding end side, and the insulating tape in the cylindrical lithium ion secondary battery of Comparative Example 3, which is unfolded into a long strip.
[0034] Fig. 8A It is a plan view showing the outer surface of the rolled positive electrode, three positive electrode leads, and an insulating tape in a cylindrical nonaqueous electrolyte secondary battery according to a modified example, which is unfolded into a long strip.
[0035] Figure 8B It is a plan view showing the inner surface of a rolled positive electrode, three positive electrode leads, and an insulating tape in a cylindrical nonaqueous electrolyte secondary battery according to a modified example, which is unfolded into a long strip.
[0036] Figure 8C It is a plan view showing the outer surface of the rolled negative electrode, three negative electrode leads, and an insulating tape in a cylindrical nonaqueous electrolyte secondary battery according to a modified example, which is unfolded into a long strip.
[0037] Fig.8D It is a plan view showing the inner surface of a negative electrode rolled into a strip shape, three negative electrode leads, and an insulating tape in a cylindrical nonaqueous electrolyte secondary battery according to a modification. DETAILED DESCRIPTION
[0038] Hereinafter, an embodiment of the cylindrical non-aqueous electrolyte secondary battery involved in the present disclosure will be described in detail with reference to the accompanying drawings. It is initially assumed that the characteristic parts of the embodiments and modified examples described below can be appropriately combined to construct a new embodiment. In addition, in the following embodiments, the same structure in the drawings is marked with the same figure mark, and repeated descriptions are omitted. In addition, many drawings are schematic diagrams, and the dimension ratios of the vertical, horizontal, height, etc. in each component may not be consistent between different drawings. Furthermore, in this specification, the sealing body 17 side of the cylindrical non-aqueous electrolyte secondary battery 10 in the axial direction is set to "up", and the bottom 68 side of the outer can 16 in the axial direction is set to "down". In addition, in this specification, when only the "height direction" is mentioned, the height direction refers to the height direction of the electrode body (winding body) 14. In addition, in the following Figures 3A to 8D In the expanded diagram of the electrodes (negative electrode, positive electrode), the area indicated by the oblique lines is the mixture layer formation area. In addition, in the following description, the technical idea of the present disclosure is described by taking the case where the cylindrical non-aqueous electrolyte secondary battery is a cylindrical lithium-ion secondary battery as an example, but the cylindrical non-aqueous electrolyte secondary battery of the present disclosure is not limited to a cylindrical lithium-ion secondary battery. Furthermore, for the structural elements described below that are not recorded in the independent claims representing the highest concept, they are arbitrary structural elements and are not necessary structural elements.
[0039] Figure 1 is a cross-sectional view in the axial direction of a cylindrical nonaqueous electrolyte secondary battery 10 according to one embodiment of the present disclosure. Figure 2 FIG. 1 is a perspective view of the electrode body 14 of the cylindrical nonaqueous electrolyte secondary battery 10. Figure 1As shown in the figure, the cylindrical non-aqueous electrolyte secondary battery (hereinafter, simply referred to as a battery) 10 includes a wound electrode body 14, a non-aqueous electrolyte (not shown), a bottomed cylindrical metal outer can 16 that accommodates the electrode body 14 and the non-aqueous electrolyte, and a sealing body 17 that seals the opening of the outer can 16. Figure 2 As shown, the electrode body 14 has a wound structure in which a long positive electrode 11 and a long negative electrode 12 are wound with two long separators 13 interposed therebetween.
[0040] The negative electrode 12 is formed to be one size larger than the positive electrode 11 in order to prevent lithium precipitation. That is, the negative electrode 12 is formed to be longer than the positive electrode 11 in the long side direction and the width direction (short side direction). In addition, the two separators 13 are formed to be at least one size larger than the positive electrode 11, for example, arranged to sandwich the positive electrode 11. The negative electrode 12 may also constitute the winding start end of the electrode body 14. However, generally speaking, the separator 13 extends beyond the winding start side end of the negative electrode 12, and the winding start side end of the separator 13 becomes the winding start end of the electrode body 14.
[0041] The non-aqueous electrolyte includes a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. Non-aqueous solvents, for example, esters, ethers, nitriles, amides, and mixed solvents of two or more thereof may also be used. The non-aqueous solvent may also contain a halogen replacement obtained by replacing at least a portion of the hydrogen atoms of these solvents with halogen atoms such as fluorine. It should be noted that the non-aqueous electrolyte is not limited to a liquid electrolyte, and may also be a solid electrolyte using a gel-like polymer. The electrolyte salt used is a lithium salt such as LiPF6.
[0042] The positive electrode 11 has a positive electrode current collector 41 (see Figure 3A , Figure 3B ) and the positive electrode mixture layer 42 formed on both sides of the positive electrode current collector 41 (see Figure 3A , Figure 3B ). The positive electrode current collector 41 can be made of a metal foil such as aluminum or aluminum alloy that is stable within the potential range of the positive electrode 11, or a thin film in which the metal is arranged on the surface. The positive electrode mixture layer 42 includes a positive electrode active material, a conductive agent, and a binder. The positive electrode 11 can be made, for example, by applying a positive electrode mixture slurry including a positive electrode active material, a conductive agent, and a binder on the positive electrode current collector 41, drying the coating, and then compressing it to form the positive electrode mixture layer 42 on both sides of the positive electrode current collector 41.
[0043] The positive electrode active material is composed of a lithium-containing metal composite oxide as a main component. Examples of the metal elements contained in the lithium-containing metal composite oxide include Ni, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, and W. An example of a preferred lithium-containing metal composite oxide is a composite oxide containing at least one of Ni, Co, Mn, and Al.
[0044] As the conductive agent included in the positive electrode mixture layer 42, carbon materials such as carbon black, acetylene black, Ketjen black, graphite, and carbon nanotubes can be exemplified. As the binder included in the positive electrode mixture layer 42, fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide resin, acrylic resin, and polyolefin resin can be exemplified. These resins and cellulose derivatives such as carboxymethyl cellulose (CMC) or its salts, polyethylene oxide (PEO), etc. can also be used simultaneously.
[0045] The negative electrode 12 has a negative electrode current collector 51 (see Figure 3C , Figure 3D ) and the negative electrode mixture layer 52 formed on both sides of the negative electrode current collector 51 (see Figure 3C , Figure 3D ). The negative electrode current collector 51 can be made of a metal foil such as copper or copper alloy that is stable within the potential range of the negative electrode 12, or a thin film in which the metal is arranged on the surface. The negative electrode mixture layer 52 includes a negative electrode active material and a binder. The negative electrode 12 can be made, for example, by applying a negative electrode mixture slurry including a negative electrode active material and a binder on the negative electrode current collector 51, drying the coating, and then compressing the coating to form the negative electrode mixture layer 52 on both sides of the negative electrode current collector 51.
[0046] Generally speaking, the negative electrode active material can use a carbon material that can reversibly absorb and release lithium ions. Preferred carbon materials are natural graphites such as flaky graphite, block graphite, and earthy graphite, block artificial graphite, and artificial graphites such as graphitized mesophase carbon microbeads. The negative electrode mixture layer 52 may also contain a Si material containing silicon (Si) as the negative electrode active material. In addition, in this case, the negative electrode mixture layer 52 may also contain SiO x Silicon oxide represented by (0.5≤x≤1.6). In addition, as the negative electrode active material, a metal that alloys with lithium other than Si, an alloy containing the metal, a compound containing the metal, etc. may be used.
[0047] The binder included in the negative electrode mixture layer 52 may be fluororesin, PAN, polyimide resin, acrylic resin, polyolefin resin, etc., as in the case of the positive electrode 11, preferably styrene-butadiene rubber (SBR) or its modified product. The negative electrode mixture layer 52 may include, for example, CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol, etc. in addition to SBR.
[0048] For the spacer 13, a porous sheet having ion permeability and insulation is used. Specific examples of the porous sheet include microporous films, woven fabrics, nonwoven fabrics, etc. As the material of the spacer 13, polyolefin resins such as polyethylene and polypropylene, cellulose, etc. are preferred. The spacer 13 may also be either a single-layer structure or a laminated structure. A heat-resistant layer may also be formed on the surface of the spacer 13.
[0049] like Figure 1 As shown in the figure, the positive electrode lead 20 is joined to the positive electrode 11, and the negative electrode lead 21 is joined to the negative electrode 12. The battery 10 has an insulating plate 18 above the electrode body 14 and an insulating plate 19 below the electrode body 14. The positive electrode lead 20 passes through the through hole of the insulating plate 18 and extends to the sealing body 17 side, and the negative electrode lead 21 passes through the through hole of the insulating plate 19 and extends to the bottom 68 side of the outer can 16. The positive electrode lead 20 is connected to the lower surface of the sealing plate 23 of the sealing body 17 by welding or the like. The terminal cap 27 constituting the top plate of the sealing body 17 is electrically connected to the sealing plate 23, and the terminal cap 27 serves as a positive terminal. Furthermore, the negative electrode lead 21 is connected to the inner surface of the bottom 68 of the metal outer can 16 by welding or the like, and the outer can 16 serves as a negative terminal.
[0050] In the present embodiment, the positive lead 20 is electrically connected to the middle part of the positive current collector 41, such as the middle part in the winding direction. In addition, the negative lead 21 is electrically connected to the middle part of the negative current collector 51, such as the middle part in the winding direction, and the end of the winding end side of the negative current collector 51 in the winding direction is made to abut against the inner surface of the outer can 16. In this way, by electrically connecting both the middle part of the long side direction and the end part of the winding end side of the negative electrode 12 to the negative terminal, the current collection path for current flow is shortened and the resistance is reduced. However, the negative lead electrically connected to the middle part of the long side direction of the negative current collector 51, such as the middle part, may be electrically connected to the outer can, and the negative lead on the winding end side electrically connected to the end part of the winding end side of the negative current collector 51 in the long side direction may be electrically connected to the outer can. Alternatively, the outermost peripheral surface in the winding direction of the electrode body may be formed by a separator, and one negative electrode lead electrically connected to an intermediate portion such as the center portion in the longitudinal direction of the negative electrode current collector 51 may be electrically connected to the outer can.
[0051] The battery 10 further includes a resin gasket 28 disposed between the outer can 16 and the sealing body 17. The sealing body 17 is fixed to the opening of the outer can 16 by riveting via the gasket 28. Thus, the internal space of the battery 10 is sealed. The gasket 28 is sandwiched between the outer can 16 and the sealing body 17 to insulate the sealing body 17 from the outer can 16. The gasket 28 has the function of a sealing material for maintaining the airtightness inside the battery and the function of an insulating material for insulating the outer can 16 from the sealing body 17.
[0052] The outer can 16 accommodates the electrode body 14 and the non-aqueous electrolyte, and has a shoulder 38, a groove 34, a cylindrical portion 30, and a bottom 68. The groove 34 can be formed, for example, by spinning a portion of the side surface of the outer can 16 radially inwardly to form an annular depression radially inwardly. The shoulder 38 is formed by bending and curving the upper end of the outer can 16 inwardly toward the peripheral edge 45 of the sealing body 17 when the sealing body 17 is riveted and fixed to the outer can 16.
[0053] The sealing body 17 has a structure in which a sealing plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a terminal cap 27 are stacked in order from the electrode body 14 side. The components constituting the sealing body 17 have, for example, a disc shape or a ring shape, and the components except the insulating member 25 are electrically connected to each other. The sealing plate 23 has at least one through hole 23a. In addition, the lower valve body 24 and the upper valve body 26 are connected at their respective central portions, and an insulating member 25 is sandwiched between their respective peripheral portions.
[0054] If the battery 10 generates abnormal heat and the internal pressure of the battery 10 increases, the lower valve body 24 will deform and break by pushing the upper valve body 26 toward the terminal cap 27, and the current path between the lower valve body 24 and the upper valve body 26 will be cut off. If the internal pressure rises further, the upper valve body 26 will break, and gas will be discharged from the through hole 27a of the terminal cap 27. By discharging this gas, the internal pressure of the battery 10 can be prevented from excessively rising and causing the battery 10 to rupture, and the safety of the battery 10 can be improved.
[0055] Figure 3A 1 is a top view showing the rolled outer surface 11a of the positive electrode 11, the positive electrode lead 20 and the insulating tape 60, which are unfolded into a long strip. Figure 3B 1 is a top view showing the inner surface 11b of the rolled positive electrode 11, the positive electrode lead 20 and the insulating tape 60 in the rolled positive electrode 11. Figure 3C 1 is a top view showing the rolled outer surface 12a of the negative electrode 12 which is unfolded into a long strip, the negative electrode lead 21 and the insulating tape 70. Figure 3D It is a plan view showing the inner surface 12 b of the roll of the negative electrode 12 that has been unrolled into a long strip, the negative electrode lead 21 , and the insulating tape 70 .
[0056] The outer surface 11a of the positive electrode 11 constitutes the first positive electrode surface, and the inner surface 11b of the positive electrode 11 constitutes the second positive electrode surface. In addition, the outer surface 12a of the negative electrode 12 constitutes the first negative electrode surface, and the inner surface 12b of the negative electrode 12 constitutes the second negative electrode surface. Figure 3A as well as Figure 3B In FIG. 1 , the α direction indicates the long side direction of the positive electrode when the positive electrode 11 is unfolded into a strip shape, and the β direction indicates the width direction of the positive electrode when the positive electrode 11 is unfolded into a strip shape. Figure 3C as well as Figure 3D In the figure, the γ direction indicates the long side direction of the negative electrode when the negative electrode 12 is developed into a strip shape, and the δ direction indicates the width direction of the negative electrode when the negative electrode 12 is developed into a strip shape.
[0057] like Figure 3A as well as Figure 3B As shown in FIG. 1 , the positive electrode 11 has a longitudinal direction ( Figure 3A , Figure 3B The two positive electrode collector exposure portions 45a and 45b on both sides of the positive electrode 11 are provided at locations spaced apart in the α direction at both ends of the winding start end of the positive electrode 11 and the winding end end of the positive electrode 11, and are spaced apart from each other in the α direction. The two positive electrode collector exposure portions 45a and 45b on both sides have: a lead fixing exposure portion 45a for fixing the positive electrode lead 20; and a lead non-fixing exposure portion 45b spaced apart from the positive electrode lead 20 in the α direction.
[0058] The two exposed portions 45a and 45b of the positive electrode current collector on both sides are respectively present in the middle region when the long strip positive electrode 11 is divided into three regions of equal length in the α direction. In other words, when the coordinate (position) of the winding start end of the positive electrode 11 is defined as 0 (reference position) in the α direction, and the coordinate (position) of the winding end is defined as 1, the two exposed portions 45a and 45b of the positive electrode current collector on both sides are respectively present at positions from 1 / 3 to 2 / 3 in the α direction. In addition, the positive electrode lead 20 is fixed at a position located at 1 / 3 to 2 / 3 of the radius of the electrode body 14.
[0059] The negative electrode 12 has a long side direction ( Figure 3C , Figure 3DThe negative electrode current collector exposed portion 55a on both sides where the negative electrode current collector 51 is exposed is provided in substantially the same region in the γ direction (shown in the γ direction) of the roll outer surface 12a and the roll inner surface 12b. The negative electrode current collector exposed portion 55a on both sides is provided between the two negative electrode mixture layer forming portions 56a and 56b on both sides in the γ direction that exist in substantially the same region in the γ direction. The negative electrode current collector exposed portion 55a on both sides is opposite to the positive electrode current collector exposed portions 45a and 45b on both sides via the separator 13.
[0060] More specifically, in the present embodiment, the lead non-fixed exposed portion 45b is located at a position closer to the winding start side than the lead fixed exposed portion 45a. Moreover, the lead non-fixed exposed portion 47b located outside the roll among the lead non-fixed exposed portion 45b is opposite to the negative electrode current collector exposed portion 57b located inside the roll among the negative electrode current collector exposed portions 55a on both sides, with the separator 13 interposed therebetween. In addition, the positive lead 20 is fixed to the lead fixed exposed portion 48b located inside the roll among the lead fixed exposed portion 45a, and the negative lead 21 is fixed to the negative electrode current collector exposed portion 57a located outside the roll among the negative electrode current collector exposed portions 55a on both sides. Moreover, the lead fixed exposed portion 48b located inside the roll is opposite to the negative electrode current collector exposed portion 57a located outside the roll among the negative electrode current collector exposed portions 55a on both sides.
[0061] The positive electrode lead 20 and the negative electrode lead 21 are opposed to each other and arranged at a distance in the height direction, and the positive electrode lead 20 and the negative electrode lead 21 are fixed at different height positions of the electrode body 14. Furthermore, the positive electrode lead 20 protrudes to the first side in the height direction (one side in the height direction), and the negative electrode lead 21 protrudes to the second side in the height direction (the other side in the height direction). Therefore, in the present embodiment, the positive electrode lead 20 does not overlap with the negative electrode lead 21 in the radial direction of the electrode body 14 via the separator 13. More specifically, in the present embodiment, when the overlap amount in the height direction of the positive electrode lead 20 with the positive electrode 11 is set to A [mm], the overlap amount in the height direction of the negative electrode lead 21 with the negative electrode 12 is set to B [mm], and the negative electrode width of the negative electrode 12 is set to C [mm], (A + B) < C is established. In addition, it is more preferable that A < (C / 2) and B < (C / 2) are established.
[0062] At least a portion of the positive electrode lead 20 is disposed at a position overlapping with a negative electrode lead facing position in the positive electrode 11 that faces the negative electrode lead 21 via the separator 13 in the height direction of the electrode body 14. In other words, at least a portion of the positive electrode lead 20 and at least a portion of the negative electrode lead 21 are located within the same winding direction range of the electrode body 14. In this way, since the range of the winding direction of the electrode body where the flat-plate-shaped electrode leads 20 and 21 are located can be limited to a local range, the roundness of the electrode body 14 can be improved, and as a result, the capacity of the battery 10 can be improved. The negative electrode lead 21 is fixed at a position located at 1 / 3 to 2 / 3 of the radius of the electrode body 14, similarly to the positive electrode lead 20.
[0063] It should be noted that, in the present embodiment, the positive electrode lead 20 is described as being spaced apart from the negative electrode lead 21 in the height direction, but at least a portion of the positive electrode lead may overlap with the negative electrode lead in the radial direction of the electrode body via a spacer. Furthermore, although the positive electrode lead 20 and the negative electrode lead 21 are fixed at a position located at 1 / 3-2 / 3 of the radius of the electrode body 14, the positive electrode lead and the negative electrode lead may not be fixed at a position located at 1 / 3-2 / 3 of the radius of the electrode body 14.
[0064] like Figure 3C as well as Figure 3D As shown in the figure, in the present embodiment, the outer surface 12a of the negative electrode 12 has an outermost negative electrode collector exposed portion 58 where the negative electrode collector 51 is exposed at the end of the winding end side in the γ direction, and the inner surface 12b of the negative electrode 12 also has an outermost negative electrode collector exposed portion 59 where the negative electrode collector 51 is exposed at the end of the winding end side in the γ direction. The length of the outermost negative electrode collector exposed portion 58 in the γ direction is longer than the length of the negative electrode collector exposed portion 59 in the γ direction. The outermost negative electrode collector exposed portion 58 includes a portion located on the outermost peripheral surface of the electrode body 14. The outermost negative electrode collector exposed portion 58 is in contact with the inner peripheral surface of the outer can 16 of the battery 10 to be electrically connected to the inner peripheral surface of the outer can 16. As a result, the current collection path can be shortened and the resistance of the battery 10 can be reduced.
[0065] like Figure 3A as well as Figure 3B As shown in FIG. 1 , an insulating tape 60 is attached to each of the positive electrode current collector exposed portions 45a and 45b on both sides of the roll outer surface 11a and the roll inner surface 11b so as to cover the positive electrode mixture layer 42 on both sides in the α direction. Figure 3C as well as Figure 3DAs shown, the insulating tape 70 is also pasted on the exposed negative electrode collector portion 57a on the outside of the roll to which the negative electrode lead 21 is fixed, at least in a state of covering the negative electrode lead. Furthermore, the insulating tape 70 may be pasted in a state of covering the negative electrode mixture layer 52 on both sides of the γ direction. In addition, the insulating tape may be pasted on the exposed negative electrode collector portion 57b on the inside of the roll, or may be pasted to cover the boundary between the negative electrode mixture layer and the exposed negative electrode collector portion other than this. The insulating tapes 60 and 70 are provided for the purpose of preventing short circuits and preventing the active material from falling off. The insulating tapes 60 and 70 may be formed, for example, by using a tape having a base material composed of a polyimide film and an adhesive material composed of silicon, but as long as it is an insulating tape that can be pasted, it may be formed of any material.
[0066] (Example 1)
[0067] <Production of positive electrode>
[0068] will have Figure 3A , Figure 3B The positive electrode has an expanded shape and has Figure 3C as well as Figure 3D The cylindrical lithium ion secondary battery having the negative electrode in the developed shape shown in FIG. 1 is a cylindrical lithium ion secondary battery of Example 1. In more detail, a lithium nickel cobalt composite oxide (LiNi 0.82 Co 0.15 Al 0.03 O2) particles, acetylene black as a conductive agent and polyvinylidene fluoride (PVdF) as a binder were added to N-methyl-2-pyrrolidone (NMP) at a mass ratio of 100:1.0:0.9 and kneaded to prepare a positive electrode slurry.
[0069] On one side of a positive electrode collector made of aluminum foil with a thickness of 15 μm, the positive electrode slurry is intermittently applied at a given interval and then dried, and the solvent (NMP) used in the preparation of the slurry is removed to form an exposed portion of the positive electrode collector with a width of 8 mm (positive electrode mixture uncoated portion). Next, the positive electrode slurry is intermittently applied on the reverse side through the positive electrode collector and then dried, and the solvent (NMP) used in the preparation of the slurry is removed to form an exposed portion of the positive electrode collector with a width of 8 mm (positive electrode mixture uncoated portion). At this time, the positions of the uncoated portions on both sides of the positive electrode collector are adjusted to be the same. Then, it is rolled using a roller press so that the thickness of the positive electrode mixture coating portion is 0.125 mm, and cut into a width of 63 mm and a length of 930 mm to obtain a positive electrode.
[0070] The obtained positive electrode has two exposed portions of the collector on both sides (uncoated portions of the positive electrode mixture on both sides) at a position 286mm-298mm from the end of the winding start side of the positive electrode in the long side direction of the positive electrode and a position 327mm-345mm from the end of the winding start side of the positive electrode in the long side direction of the positive electrode. The welding position in the width direction of the positive lead with a width of 4mm and a thickness of 0.15mm is a position 334mm-338mm from the end of the winding start side of the positive electrode, which is included in the uncoated portions of the positive electrode mixture on both sides of the positive electrode. The welding position in the positive electrode width direction of the positive electrode lead is a position 30mm opposite to the positive electrode collector in the positive electrode width direction, and the positive electrode lead is configured to protrude 18mm from the positive electrode. The positive electrode lead is ultrasonically welded to the inner surface of the positive electrode roll. A polyimide tape (insulating tape) with a width of 21 mm was attached to the positive electrode mixture non-coated area including the positive electrode lead welding area so as to cover the positive electrode mixture layer forming area (positive electrode mixture coated area) by 1.5 mm on one side.
[0071] <Production of negative electrode>
[0072] 100 parts by mass of graphite powder, 1 part by mass of carboxymethyl cellulose (CMC) as a binder, 1 part by mass of styrene-butadiene rubber (SBR) and water are mixed to prepare a negative electrode slurry. After intermittently coating the negative electrode slurry on one side of a negative electrode collector made of copper foil with a thickness of 8 μm, the negative electrode slurry is dried, and the solvent (water) used in the preparation of the slurry is removed so that an 88 mm negative electrode mixture uncoated portion is formed at other locations across a 7 mm wide collector exposed portion (mixture uncoated portion) and a mixture layer (mixture coated portion). Next, after intermittently coating the negative electrode slurry on the reverse side across the negative electrode collector, the negative electrode mixture uncoated portion is dried and the solvent (water) used in the preparation of the slurry is removed so that a 25 mm negative electrode mixture uncoated portion is formed at other locations across a 7 mm mixture uncoated portion and a mixture coated portion. At this time, the 7 mm negative electrode mixture uncoated portion is adjusted to be in the same position in the long side direction of the negative electrode on both sides of the negative electrode collector. Then, the sheet was rolled using a roll press so that the thickness of the negative electrode mixture coating portions on both surfaces was 0.154 mm, and cut into pieces with a width of 64 mm and a length of 966 mm to obtain a negative electrode.
[0073] The negative electrode has a 2mm uncoated portion of the mixture on both sides of the front and back at the end of the winding start side, and further has a negative electrode mixture uncoated portion on both sides at a position of 326mm-333mm in the long side direction of the negative electrode from the winding start end of the negative electrode. In addition, the negative electrode also has an 86mm uncoated portion on the outer surface of the roll at the end of the winding end side, and a 23mm uncoated portion of the negative electrode mixture on the inner surface of the roll at the end of the winding end side. Next, a negative electrode lead with a width of 4mm and a thickness of 0.15mm is set. The welding position of the negative electrode lead is a position of 327.5mm-331.5mm in the long side direction of the negative electrode from the winding start end of the negative electrode, and is included in the uncoated portion of the negative electrode mixture on both sides of the negative electrode. On the other hand, the welding position of the negative electrode lead in the negative electrode width direction is a position 30mm opposite to the negative electrode collector in the negative electrode width direction, and the negative electrode lead is configured to protrude 12mm from the bottom side of the outer can in the height direction of the negative electrode. The negative electrode lead was ultrasonically welded to the outer surface of the negative electrode roll, and a polyethylene tape (insulating tape) with a width of 6 mm was attached to the negative electrode mixture uncoated portion including the negative electrode lead welding portion so as to completely cover the negative electrode lead.
[0074] <Preparation of Electrolyte>
[0075] Vinylene carbonate is mixed into a mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC) and ethyl methyl carbonate in a volume ratio of 15:10:75 (25°C, 1 atmosphere), and LiPF6 is dissolved therein to become 3% by mass at a concentration of 1.4 mol / L, thereby obtaining a non-aqueous electrolyte.
[0076] <Battery Assembly>
[0077] The positive electrode and the negative electrode are wound with a separator composed of a polyethylene microporous film to produce an electrode body. In the electrode body, the uncoated portion of the negative electrode mixture provided at the negative electrode is opposed to the insulating tape completely pasted to the uncoated portion of the mixture of the positive electrode through the separator. The length of the separator is adjusted so that the outermost periphery of the electrode body is composed of copper foil of the exposed portion of the negative electrode collector throughout the entire periphery. Insulating plates made of polypropylene are respectively arranged on the upper and lower surfaces of the electrode body. After the above-mentioned electrode body is inserted into a bottomed cylindrical outer can, the negative electrode lead is ultrasonically welded to the bottom surface of the bottomed cylindrical outer can, and the positive electrode lead is laser welded to the sealing body, and then the aforementioned non-aqueous electrolyte is injected into the outer can. Then, the sealing body is riveted and fixed using an insulating gasket, thereby producing a cylindrical lithium-ion secondary battery with a diameter of 21mm, a height of 70mm, and a design capacity of 4400mAh.
[0078] (Example 2)
[0079] Figure 4A1 is a plan view showing the rolled outer surface 11a of the positive electrode 11 unfolded into a long strip, the positive electrode lead 20 and the insulating tape 60 of the cylindrical lithium ion secondary battery of Example 2. Figure 4B 1 is a top view showing the inner surface 11b of the rolled positive electrode 11, the positive electrode lead 20 and the insulating tape 60 in the rolled positive electrode 11. Figure 4C 1 is a plan view showing the rolled outer surface 12a, the negative electrode lead 21, the winding end side negative electrode lead 125 and the insulating tape 70 of the cylindrical lithium ion secondary battery of Example 2, which is unfolded into a long strip shape. Figure 4D It is a plan view showing the inner surface 12 b of the negative electrode 12 that has been unrolled into a long strip, the negative electrode lead 21 , the negative electrode lead 125 on the winding end side, and the polyethylene tape (insulating tape 70 ).
[0080] like Figure 4A to Figure 4D As shown, the cylindrical lithium ion secondary battery of Example 2 is different from the cylindrical lithium ion secondary battery of Example 1 in that it has a negative electrode lead 125 with a width of 3 mm and a thickness of 0.15 mm fixed at a position 959 mm from the winding start end of the negative electrode 12 in the long side direction of the negative electrode, in addition to the negative electrode lead 21 disposed at a position of 326 mm to 333 mm on both sides of the negative electrode 12 where the negative electrode mixture is not applied. The cylindrical lithium ion secondary battery of Example 2 has the same structure as the cylindrical lithium ion secondary battery of Example 1 except for this. The negative electrode lead 21 and the negative electrode lead 125 on the winding end side are respectively opposed to the negative electrode collector by 30 mm in the negative electrode width direction. Furthermore, the negative electrode lead 121 and the negative electrode lead 125 on the winding end side are respectively protruded 19 mm from the negative electrode 112 to the bottom plate side of the outer can.
[0081] (Comparative Example 1)
[0082] Figure 5A 3 is a top view showing the rolled outer surface 311a of the positive electrode 311 unfolded into a strip shape, the positive electrode lead 320 and the insulating tape 360 of the cylindrical lithium ion secondary battery of Comparative Example 1. Figure 5B 3 is a top view showing the inner surface 311b of the rolled positive electrode 311, the positive electrode lead 320 and the insulating tape 360. Figure 5C 1 is a plan view showing the rolled outer surface 12 a of the negative electrode 12 unfolded into a strip shape, the negative electrode lead 21 , and the insulating tape 70 of the cylindrical lithium ion secondary battery of Comparative Example 1. Figure 5D FIG. 1 is a top view showing the inner surface 12 b of the rolled negative electrode 12, the negative electrode lead 21, and the insulating tape 70 in the rolled negative electrode 12. Figure 5A as well as Figure 5B As shown, the positive electrode 311 includes a positive electrode current collector 341 and a positive electrode mixture layer 342 .
[0083] Reference Figure 5A to Figure 5D , after intermittently applying the positive electrode slurry on one side of a positive electrode collector made of aluminum foil with a thickness of 15 μm, it was dried, and the solvent (NMP) used in the preparation of the slurry was removed to form an uncoated portion of the positive electrode mixture with a width of 8 mm. Next, the positive electrode slurry was intermittently applied on the reverse side through the positive electrode collector and dried, and the solvent (NMP) used in the preparation of the slurry was removed to form an uncoated portion of the positive electrode mixture with a width of 26 mm. Then, the positive electrode mixture was rolled using a roller press so that the thickness of the coated portion was 0.125 mm, and it was cut into a width of 63 mm and a length of 930 mm to obtain a positive electrode.
[0084] The inner surface 311b of the positive electrode 311 has a positive electrode mixture uncoated portion at a position 327mm-345mm from the start end of the winding in the long side direction of the positive electrode. On the other hand, the outer surface 311a of the positive electrode 311 has a positive electrode mixture uncoated portion at a position 286mm-345mm from the start end of the winding in the long side direction of the positive electrode. In addition, the welding position in the width direction of the positive electrode lead with a width of 4mm and a thickness of 0.15mm is set to a position 334mm-338mm from the start end of the winding in the long side direction of the positive electrode, and is set to a position included in the positive electrode mixture uncoated portion on both sides.
[0085] The welding position of the positive electrode lead 320 in the positive electrode width direction is at a position 30 mm opposite to the positive electrode collector in the positive electrode width direction, and the positive electrode lead 320 is configured to protrude 18 mm from the positive electrode. The positive electrode lead 320 is ultrasonically welded to the inner surface 311b of the roll of the positive electrode 311. A polyimide tape (insulating tape 360) with a width of 21 mm is pasted on the inner surface 311b of the roll so that the positive electrode mixture coating portion is covered by 1.5 mm on one side. On the other hand, a polyimide tape (insulating tape 360) with a width of 62 mm is pasted on the surface arranged on the periphery of the electrode body so that the entire area of the uncoated portion of the positive electrode mixture and the single-sided coating portion of the positive electrode mixture are covered by 1.5 mm. The structure of the cylindrical lithium ion secondary battery of Comparative Example 1 other than these is the same as the structure of the cylindrical lithium ion secondary battery of Example 1.
[0086] (Comparative Example 2)
[0087] Fig. 6A 4 is a top view showing the rolled outer surface 411a of the positive electrode 411 unfolded into a strip shape, the positive electrode lead 420 and the insulating tape 460 of the cylindrical lithium ion secondary battery of Comparative Example 2. Figure 6B 4 is a top view showing the inner surface 411b of the rolled positive electrode 411, the positive electrode lead 420 and the insulating tape 460 in the positive electrode 411 which is unfolded into a long strip. Figure 6C4 is a top view showing the rolled outer surface 412a of the negative electrode 412 which is unfolded into a long strip, the negative electrode lead 421 at the winding start side, the negative electrode lead 425 at the winding end side, and the insulating tape 470 of the cylindrical lithium ion secondary battery of Comparative Example 2, Fig.6D 4 is a top view showing the inner surface 412b of the negative electrode 412 that has been unrolled into a long strip, the negative electrode lead 421 at the start of winding, the negative electrode lead 425 at the end of winding, and the insulating tape 470. Fig. 6A as well as Figure 6B As shown in FIG. 4 , the positive electrode 411 includes a positive electrode current collector 441 and a positive electrode mixture layer 442. Figure 6C as well as Fig.6D As shown, the negative electrode 412 includes a negative electrode current collector 451 and a negative electrode mixture layer 452 .
[0088] Reference Figure 6A to Figure 6D , after intermittently applying the positive electrode slurry to one side of a positive electrode collector made of aluminum foil with a thickness of 15 μm, the positive electrode slurry is dried, and the solvent (NMP) used in the preparation of the slurry is removed to form an uncoated portion of the positive electrode mixture with a width of 8 mm. Next, after intermittently applying the positive electrode slurry to the reverse side through the positive electrode collector, the positive electrode slurry is dried, and the solvent (NMP) used in the preparation of the slurry is removed to form an uncoated portion of the positive electrode mixture with a width of 26 mm. Then, the positive electrode 411 is obtained by rolling using a roller press so that the thickness of the coated portion of the positive electrode mixture is 0.125 mm, and cutting into a width of 63 mm and a length of 910 mm.
[0089] The outer surface 411a and the inner surface 411b of the positive electrode 411 both have a positive electrode mixture uncoated portion at a position 327 mm to 345 mm from the start of winding in the long side direction of the positive electrode. Furthermore, the welding position in the width direction of the positive electrode lead having a width of 4 mm and a thickness of 0.15 mm is set at a position 334 mm to 338 mm from the start of winding in the long side direction of the positive electrode, and is set as a position included in the positive electrode mixture uncoated portion on both sides.
[0090] The positive electrode lead 420 is welded at a position 60 mm opposite to the positive electrode collector in the positive electrode width direction, and the positive electrode lead 420 is arranged to protrude 18 mm from the positive electrode. The positive electrode lead 420 is ultrasonically welded to the inner surface 411b of the roll of the positive electrode 411. A polyimide tape (insulating tape 460) with a width of 21 mm is attached to the inner surface 411b of the roll so that the positive electrode mixture coating portion is covered by 1.5 mm on one side.
[0091] Reference Figure 6A to Figure 6D, after intermittently applying the negative electrode slurry to one side of a negative electrode collector made of copper foil with a thickness of 8 μm, the negative electrode slurry is dried and the solvent (water) used in the preparation of the slurry is removed to form a 98 mm uncoated portion of the negative electrode mixture. Next, after intermittently applying the negative electrode slurry to the reverse side through the negative electrode collector, the negative electrode slurry is dried and the solvent (water) used in the preparation of the slurry is removed to form a 35 mm uncoated portion of the negative electrode mixture. Then, the negative electrode 412 is produced by rolling using a roller press so that the thickness of the negative electrode mixture coating on both sides is 0.154 mm, and then cut into a width of 64 mm and a length of 956 mm.
[0092] The negative electrode 412 has an uncoated portion with a length of 12 mm in the long side direction of the negative electrode on both the front and back surfaces at the end of the winding start side. In addition, the negative electrode 412 has an uncoated portion with a length of 86 mm in the long side direction of the negative electrode on the outer peripheral side of the end of the winding end side, and has a negative electrode mixture uncoated portion with a length of 23 mm in the long side direction of the negative electrode on the inner peripheral side of the end of the winding end side.
[0093] A negative electrode lead 421 on the winding start side and a negative electrode lead 425 on the winding end side are fixed to the negative electrode 412. The welding position of the negative electrode lead 421 on the winding start side in the negative electrode long side direction is a position 2mm-5mm away from the winding start end in the negative electrode long side direction, and is a position included in the uncoated part of the negative electrode mixture on both sides. The welding position of the negative electrode lead 421 on the winding start side in the negative electrode width direction is a position 60mm opposite to the negative electrode collector in the negative electrode width direction, and the negative electrode lead 421 on the winding start side is configured to protrude 10mm from the negative electrode 412. The negative electrode lead 421 on the winding start side is ultrasonically welded to the outer surface of the negative electrode 412. A polyethylene tape (insulating tape 470) with a width of 8mm is pasted on the uncoated part of the negative electrode mixture including the welding position of the negative electrode lead on the winding start side so that the negative electrode lead 421 on the winding start side is completely covered.
[0094] The welding position of the negative electrode lead 425 on the winding end side in the negative electrode long side direction is 953 mm to 955 mm from the winding start end in the negative electrode long side direction. The welding position of the negative electrode lead 425 on the winding end side in the negative electrode width direction is 30 mm opposite to the negative electrode current collector in the negative electrode width direction, and the negative electrode lead 425 on the winding end side is arranged to protrude 19 mm from the negative electrode 412. The negative electrode lead 421 on the winding start side is ultrasonically welded to the outer surface of the negative electrode 412.
[0095] (Comparative Example 3)
[0096] Fig. 7A A plan view showing the rolled outer surface 411a of the positive electrode 411 unfolded into a strip shape, the positive electrode lead 420 and the insulating tape 460 of the cylindrical lithium ion secondary battery of Comparative Example 3, Figure 7B4 is a top view showing the inner surface 411b of the rolled positive electrode 411, the positive electrode lead 420 and the insulating tape 460 in the positive electrode 411 which is unfolded into a long strip. Figure 7C FIG. 1 is a top view showing the rolled outer surface 512 a of the negative electrode 512 which is unfolded into a strip shape, the negative electrode lead 525 at the winding end side, and the insulating tape 570 of the cylindrical lithium ion secondary battery of Comparative Example 3. Fig.7D FIG. 5 is a top view showing the inner surface 512b of the negative electrode 512 that has been unrolled into a long strip, the negative electrode lead 525 at the winding end, and the insulating tape 570. Figure 7C as well as Fig.7D As shown, the negative electrode 512 includes a negative electrode current collector 551 and a negative electrode mixture layer 552 .
[0097] Reference Figure 7A to Figure 7D , the negative electrode slurry is intermittently applied to one side of a negative electrode collector made of copper foil with a thickness of 8μm, and then dried, and then the solvent (water) used in the preparation of the slurry is removed to form an 88mm uncoated portion of the negative electrode mixture. Next, the negative electrode slurry is intermittently applied to the reverse side through the negative electrode collector and then dried, and then the solvent (water) used in the preparation of the slurry is removed to form a 25mm uncoated portion of the negative electrode mixture. Then, the negative electrode mixture is rolled using a roller press so that the thickness of the coated portion of the negative electrode mixture on both sides is 0.154mm, and it is cut into a width of 64mm and a length of 946mm, thereby forming a negative electrode 512.
[0098] The negative electrode 512 has an uncoated portion with a length of 2 mm in the long side direction of the negative electrode on both the front and back sides at the end of the winding start side. Furthermore, the negative electrode 512 has an uncoated portion with a length of 86 mm in the long side direction of the negative electrode on the outer circumference of the end of the winding end side, and has a negative electrode mixture uncoated portion with a length of 23 mm in the long side direction of the negative electrode on the inner circumference of the end of the winding end side. A winding end side negative electrode lead 525 with a width of 4 mm and a thickness of 0.15 mm is fixed to the negative electrode 512.
[0099] The welding position of the negative electrode lead 525 on the winding end side in the negative electrode long side direction is a position 938mm-942mm away from the winding start end in the negative electrode long side direction. The welding position of the negative electrode lead 525 on the winding end side in the negative electrode width direction is a position 30mm opposite to the negative electrode collector in the negative electrode width direction, and the negative electrode lead 525 on the winding end side is configured to protrude 19mm from the negative electrode 512. The negative electrode lead 525 on the winding end side is ultrasonically welded to the outer surface of the negative electrode 412. A polyethylene tape (insulating tape 470) with a width of 8mm is pasted on the uncoated portion of the negative electrode mixture including the welding position of the negative electrode lead on the winding start side so that the negative electrode lead 425 on the winding end side is completely covered.
[0100] [1 kHz impedance measurement]
[0101] Using each of the cylindrical lithium ion secondary batteries of Examples 1 and 2 and Comparative Examples 1 to 3, impedance was measured at a frequency of 1 kHz in an environment of 25°C.
[0102] [Electrode body roundness measurement]
[0103] For each of the cylindrical lithium ion secondary batteries of Examples 1 and 2 and Comparative Examples 1 to 3, the maximum diameter and the minimum diameter of the electrode body were measured with a caliper to calculate the circularity.
[0104] [Measurement of positive electrode warpage]
[0105] For the cylindrical lithium-ion secondary batteries of Examples 1 and 2, the positions 5 cm on both sides of the center of the two uncoated portions of the mixture on both sides between the 1 / 3 to 2 / 3 positions of the positive electrode were fixed, and the warping amount at both ends of the long side direction of the positive electrode was measured. For the cylindrical lithium-ion secondary battery of Comparative Example 1, the uncoated portion of the single-sided positive electrode mixture at the 1 / 3 to 2 / 3 position of the positive electrode was set as the top, and the positions 5 cm on both sides from the center were fixed to measure the warping amount at both ends of the long side direction of the positive electrode. For the cylindrical lithium-ion secondary batteries of Comparative Examples 2 and 3, the position of 10 vm was fixed in the winding direction of the positive electrode and the warping amount of the plate was measured with a caliper.
[0106] [Positive electrode mixture drop test]
[0107] For the cylindrical lithium-ion secondary batteries of Examples 1, 2 and Comparative Example 1, the values are measured at the part that includes all the uncoated parts of the positive electrode mixture, and for Comparative Examples 2 and 3, the values are measured at the coated parts of the positive electrode mixture on both sides. The positive electrode is cut into 120 mm long and aligned with a round bar of 6 mm in diameter, including all the uncoated parts of the positive electrode mixture. A tensile force of 10 N is applied to the positive electrode, and the positive electrode is reciprocated 3 times at a speed of 10 mm / sec in the direction from the start of winding to the end of winding, and then from the end of winding to the start of winding, to confirm whether the positive electrode mixture has fallen off.
[0108] Table 1 shows the measurement results of each test.
[0109] [Table 1]
[0110]
[0111] [Summary of each measurement result]
[0112] <Impedance(1kHz)>
[0113] Comparison Example 2 in which negative electrode leads were arranged at the winding start end and winding end end of the negative electrode, respectively, was compared with Comparison Example 3 in which negative electrode leads were provided only at the winding end end of the negative electrode, and it was confirmed that the resistance of the negative electrode collector could be reduced, and the impedance of the battery could be reduced from 20 mΩ to 12 mΩ and 8 mΩ. On the other hand, Examples 1 and 2 and Comparison Example 1 electrically connected the winding end end of the negative electrode to the outer can and fixed the negative electrode lead between 1 / 3 and 2 / 3 of the radius of the electrode body, and thus, in comparison with Comparison Example 2 in which two negative electrode leads were fixed to the winding start end and winding end end of the negative electrode, respectively, it was confirmed that the impedance of the battery could be reduced from 12 mΩ to 8 mΩ, and further to 4 mΩ.
[0114] This is considered to be because, when the negative electrode lead is fixed to between 1 / 3 and 2 / 3 of the radius of the electrode body, the current collection path on the negative electrode side can be shortened compared to the case where the negative electrode lead is fixed to the end of the winding start side of the negative electrode. It should be noted that it can be confirmed that when the winding end side negative electrode lead of Example 2 is used and electrically connected to the outer can, as a structure in which the winding end side end of the negative electrode is electrically connected to the outer can, a resistance reduction effect substantially equivalent to the structure in which the negative electrode current collector is in contact with the inner circumferential surface of the outer can in Example 1 can be obtained.
[0115] <Electrode body roundness>
[0116] In Examples 1 and 2 and Comparative Examples 1 and 3, the roundness of the electrode body reached 98.5% because the negative electrode lead was not fixed at the end of the winding start side. Therefore, if the negative electrode lead was not fixed at the end of the winding start side, the average diameter of the electrode body could be made close to a fixed value, so it was confirmed that the capacity could be improved.
[0117] (First summary)
[0118] According to the measurement results of impedance and electrode body roundness, it can be confirmed that Examples 1, 2 and Comparative Example 1 can achieve low resistance of the battery and improve the roundness of the electrode body. Therefore, if the structures of Examples 1, 2 and Comparative Example 1 are adopted, the capacity of the non-aqueous electrolyte secondary battery can be increased.
[0119] <Positive electrode warping amount>
[0120] In Comparative Example 1, since there is a single-sided uncoated portion of the positive electrode mixture at a position between 1 / 3 and 2 / 3 of the radius of the positive electrode body, a 2 mm warp occurs in the width direction during rolling. In contrast, in Examples 1 and 2, since there is no single-sided uncoated portion of the positive electrode mixture at the same position of the positive electrode, it can be confirmed that no warping of the positive electrode occurs.
[0121] <Positive electrode mixture drop test>
[0122] The positive plates of Examples 1 and 2 and Comparative Examples 2 and 3 do not have a single-sided positive electrode mixture layer, and no mixture fell off in the positive electrode mixture shedding test. On the other hand, Comparative Example 1 confirmed that a portion of the positive electrode mixture fell off at the boundary between the single-sided positive electrode mixture coating portion and the double-sided mixture coating portion. Therefore, it is believed that Comparative Example 1 has a higher risk of falling off at the boundary between the double-sided coating portion and the single-sided coating portion.
[0123] (Second summary)
[0124] According to the results of the positive electrode warping and positive electrode mixture shedding tests, it can be confirmed that the batteries of Examples 1 and 2 can reduce the positive electrode warping and suppress the positive electrode mixture shedding in comparison with the battery of Comparative Example 1. Therefore, if the structures of Examples 1 and 2 are adopted, a non-aqueous electrolyte secondary battery with excellent long-term reliability can be produced in comparison with the case of adopting the structure of Comparative Example 1.
[0125] [Modifications]
[0126] The present disclosure is not limited to the above-mentioned embodiments and their variations, and various improvements and changes can be made within the scope of the matters described in the claims of the present application and their equivalents. For example, in the above-mentioned embodiments, the case where the battery has only one positive electrode lead 20 is described. However, the battery of the present disclosure may also have two or more positive electrode leads as described below.
[0127] Fig. 8A 1 is a plan view showing the rolled outer surface 211a of the positive electrode 211 unfolded into a strip shape, three positive electrode leads 20, 20, 20 and an insulating tape 60 of a cylindrical nonaqueous electrolyte secondary battery of a modified example. Figure 8B 2 is a top view showing the inner surface 211b of the rolled positive electrode 211, three positive electrode leads 20, 20, 20 and the insulating tape 60 in the rolled positive electrode 211. Figure 8C 1 is a top view showing the rolled outer surface 212a of the negative electrode 212 unfolded into a strip shape, three negative electrode leads 21, 21, 21 and the insulating tape 70 of the cylindrical nonaqueous electrolyte secondary battery of the modified example. Fig.8D 2 is a top view showing the inner surface 212b of the negative electrode 212 that has been unrolled into a long strip, three negative electrode leads 21, 21, 21, and the insulating tape 70. Fig. 8A as well as Figure 8B As shown in FIG. 2 , the positive electrode 211 includes a positive electrode current collector 241 and a positive electrode mixture layer 242. Figure 8C as well as Fig.8D As shown, the negative electrode 212 includes a negative electrode current collector 251 and a negative electrode mixture layer 252 .
[0128] like Figures 8A to 8DAs shown in the figure, the cylindrical non-aqueous electrolyte secondary battery can also have the following combination of N groups (N is a natural number greater than 2) spaced apart from each other in the winding direction of the electrode body: Figure 3A to Figure 3D The combination of the two double-sided positive electrode current collector exposed portions 45a, 45b, the positive electrode lead 20, the double-sided negative electrode current collector exposed portions 55a and the negative electrode lead 21, which have the relative positional relationship described in detail, is, for example, Figures 8A to 8D As shown in the figure, three sets of this combination may be provided. In this way, since the current collection paths in each of the positive electrode 211 and the negative electrode 212 can be shortened, the resistance of the cylindrical non-aqueous electrolyte secondary battery can be greatly reduced.
[0129] In the above description, each collector exposure portion is formed in a strip-shaped region from one end to the other end in the width direction of the electrode, but the electrode body may also include one or more collector exposure portions where the collector is not exposed in the entire width direction of the long strip electrode.
[0130] --Description of Reference Numerals-
[0131] Battery, 11, 111, 211 positive electrode, 11a, 211a roll outer surface, 11b, 211b roll inner surface, 12, 112, 212 negative electrode, 12a, 212a roll outer surface, 12b, 212b roll inner surface, 13 separator, 14 electrode body, 16 outer can, 17 sealing body, 20, 320 positive electrode lead, 21, 121 negative electrode lead, 41, 241 positive electrode collector, 42, 242 positive electrode mixture layer, 45a lead fixing exposed portion , 45b lead non-fixed exposed portion, 47b outer lead non-fixed exposed portion, 48b inner lead fixed exposed portion, 51, 251 negative electrode collector, 52, 252 negative electrode mixture layer, 55a both sides of negative electrode collector exposed portion, 56a both sides of negative electrode mixture layer forming portion, 57a outer side of negative electrode collector exposed portion, 57b inner side of negative electrode collector exposed portion, 58 outermost negative electrode collector exposed portion, 59 negative electrode collector exposed portion, 125 winding end side negative lead.
Claims
1. A cylindrical non-aqueous electrolyte secondary battery comprising: An electrode body, wherein a long positive electrode and a long negative electrode are wound with a separator, wherein the positive electrode comprises a positive electrode collector and positive electrode mixture layers arranged on both sides of the positive electrode collector, and the negative electrode comprises a negative electrode collector and negative electrode mixture layers arranged on both sides of the negative electrode collector; a positive electrode lead fixed to the positive electrode current collector and including a protrusion protruding from a first side in a height direction of the electrode body; and a negative electrode lead fixed to the negative electrode current collector and including a protrusion protruding from the second side in the height direction of the electrode body, The positive electrode has two or more double-sided positive electrode current collector exposed portions in substantially the same region in the long side direction of the positive electrode on both sides of the positive electrode first side and the positive electrode second side, and the positive electrode current collector is exposed in the double-sided positive electrode current collector exposed portions. The two or more double-sided positive electrode current collector exposed portions are provided at locations spaced apart from both sides of the winding start end and the winding end end in the longitudinal direction of the positive electrode, and are spaced apart from each other in the longitudinal direction of the positive electrode. The two or more positive electrode current collector exposed portions on both sides include: a lead-fixed exposed portion to which the positive electrode lead is fixed; and a lead-unfixed exposed portion to which the positive electrode lead is not fixed, The negative electrode has two or more two-sided negative electrode mixture layer forming portions where the negative electrode mixture layer exists in substantially the same region in the long side direction of the negative electrode on both sides of the negative electrode first surface and the negative electrode second surface, and has at least one two-sided negative electrode current collector exposed portion in substantially the same region in the long side direction of the negative electrode on both sides of the negative electrode first surface and the negative electrode second surface, wherein the negative electrode current collector is exposed in the two-sided negative electrode current collector exposed portions, The negative electrode current collector exposed portions on both sides are opposed to the positive electrode current collector exposed portions on both sides via the separator. The negative electrode lead is fixed to the exposed portions of the negative electrode current collectors on both sides. At least a portion of the positive electrode lead is disposed at a portion overlapping with a negative electrode lead facing position in the positive electrode that faces the negative electrode lead via the separator in the height direction.
2. The cylindrical nonaqueous electrolyte secondary battery according to claim 1, wherein: The positive electrode lead is disposed at a distance from the negative electrode lead in the height direction.
3. The cylindrical nonaqueous electrolyte secondary battery according to claim 1 or 2, wherein: The positive electrode has only two positive electrode current collector exposed portions on both sides. The positive electrode lead is fixed only at a position located between 1 / 3 and 2 / 3 of the radius of the electrode body, and the negative electrode lead is fixed only at a position located between 1 / 3 and 2 / 3 of the radius of the electrode body.
4. The cylindrical nonaqueous electrolyte secondary battery according to any one of claims 1 to 3, wherein The amount of overlap in the height direction of the positive lead with the positive electrode is set to A [mm], the amount of overlap in the height direction of the negative lead with the negative electrode is set to B [mm], and the negative electrode width of the negative electrode is set to C [mm]. At this time, (A+B)<C holds.
5. The cylindrical nonaqueous electrolyte secondary battery according to claim 4, wherein: The amount of overlap in the height direction of the positive lead with the positive electrode is set to A [mm], the amount of overlap in the height direction of the negative lead with the negative electrode is set to B [mm], and the negative electrode width of the negative electrode is set to C [mm]. At this time, A<(C / 2) holds, and B<(C / 2) holds.
6. The cylindrical nonaqueous electrolyte secondary battery according to any one of claims 1 to 5, wherein The outermost peripheral surface of the electrode body has an outermost negative electrode current collector exposed portion where the negative electrode current collector is exposed. At least a portion of the outermost negative electrode current collector exposed portion is in contact with the inner peripheral surface of the outer packaging can that houses the electrode assembly.
7. The cylindrical nonaqueous electrolyte secondary battery according to any one of claims 1 to 5, wherein The negative electrode has a winding end side negative electrode current collector exposed portion at the end portion on the winding end side where the negative electrode current collector is exposed. The cylindrical nonaqueous electrolyte secondary battery includes a winding-end-side negative electrode lead that electrically connects the negative electrode current collector exposed portion on the winding-end side and an outer can accommodating the electrode assembly.