Carrier-membrane layer integrated molecular sieve membrane prepared from clay as well as preparation method and application of carrier-membrane layer integrated molecular sieve membrane

The integrated molecular sieve membrane of carrier-film layer was prepared through clay, which solved the problem of uneven growth of molecular sieve membrane on the carrier surface, improved separation performance and economic performance, and reduced environmental pollution, achieving efficient and environmentally friendly separation effect.

CN118874232AActive Publication Date: 2024-11-01ANHUI POLYTECHNIC UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410915367.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The existing molecular sieve membrane preparation technology cannot ensure uniform and dense growth of the molecular sieve membrane on the support surface, resulting in low separation performance and high cost, and complex traditional methods and serious environmental pollution.

Method used

A carrier-film integrated molecular sieve membrane is prepared by clay. The molecular sieve membrane is prepared by preparing clay into a porous carrier precursor and converting the clay interface on the surface of the carrier precursor into a dense molecular sieve layer through high-temperature calcination to achieve non-solvent conversion.

Benefits of technology

It significantly improves the separation performance, reduces the cost of carrier preparation and roasting temperature, reduces the use of chemical reagents and pollutant emissions, and achieves the effect of energy saving and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874232A_ABST
    Figure CN118874232A_ABST
Patent Text Reader

Abstract

The invention provides a carrier-membrane layer integrated molecular sieve membrane prepared from clay as well as a preparation method and application of the carrier-membrane layer integrated molecular sieve membrane prepared from the clay, the clay is prepared into a porous carrier precursor, and then a clay interface on the surface of the carrier precursor is converted into a compact molecular sieve layer; and finally, carrying out high-temperature roasting to obtain the carrier-membrane layer integrated molecular sieve membrane with efficient separation performance. Compared with the prior art, the preparation method has the advantages that the cheap clay is used as a carrier raw material instead of a traditional chemical pure substance, so that the preparation cost of the carrier is reduced, and the roasting temperature of the carrier can be remarkably reduced; a compact clay layer on the surface of the carrier precursor is converted into the molecular sieve membrane by utilizing the characteristic that clay is easily converted into a molecular sieve, so that the compactness of the molecular sieve membrane can be improved; the clay is converted into the molecular sieve membrane by adopting a gas phase conversion method, so that the dosage of chemical reagents can be reduced, the emission of pollutants is reduced, and the effects of energy conservation and environmental protection are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of membrane separation, and in particular relates to a carrier-membrane layer integrated molecular sieve membrane prepared from clay, and a preparation method and application thereof. Background Art

[0002] Membrane separation technology has become one of the most commonly used separation technologies to solve major challenges in the fields of water resources, energy, and environment. Membrane materials are the core of membrane separation technology and have been widely used in microfiltration, nanofiltration, ultrafiltration, and other fields. However, the preparation of membrane materials with molecular-level difference separation performance is still a recognized problem.

[0003] Molecular sieve membranes are ideal membrane materials for separating small molecule mixtures because of their uniform, molecular-level pores. After decades of exploration and research, the quality of molecular sieve membranes has been greatly improved. However, the membrane defects in molecular sieve membranes provide non-selective channels for the transmission of substances, reducing the inherent separation performance of molecular sieve membranes. Therefore, it is crucial to reduce or eliminate membrane defects during the preparation of molecular sieve membranes.

[0004] Molecular sieve membranes are usually grown on the surface of porous carriers. The structure, morphology, and chemical properties of the carriers have a significant impact on the quality of molecular sieve membranes. Studies have shown that the preparation cost of the carrier accounts for more than 50% of the total cost of molecular sieve membranes.

[0005] Despite this, the existing molecular sieve membrane preparation technology still cannot ensure the uniform and dense growth of the molecular sieve membrane on the carrier surface, resulting in the molecular sieve membrane being not only more expensive than the organic membrane, but also having a much lower separation performance than the organic membrane.

[0006] The patent with publication number CN 115583657 A published on January 10, 2023 discloses a method for preparing an MFI molecular sieve membrane, including the following steps: S1, seed synthesis: the appropriately heated seed is formed on the carrier by grinding or ultrasonication to form a molecular sieve seed; S2, preparing a mixed sol solution: fresh condensed colloid particles are dispersed, added to water and an appropriate amount of viscous agent is added to form a mixed sol solution; S3, a mixed material is prepared; S4, high-temperature crystallization is performed; S5, molding, and an MFI molecular sieve membrane is obtained. The addition of an appropriate amount of viscous agent makes the mixed sol solution easier to mix and the mixed mixed sol solution is more suitable for crystallization. When the molecular sieve seed and the mixed sol solution are mixed to obtain a synthetic solution, a pore-forming agent is added to make the pore size of the prepared MFI molecular sieve membrane have better uniformity. However, the preparation method of the membrane prepared by hydrothermally coating the seed on the existing carrier is complicated.

[0007] Therefore, it is urgent to adopt new carriers and new technologies for preparing molecular sieve membranes to improve the separation selectivity and economic performance of molecular sieve membranes. Summary of the invention

[0008] The purpose of the present invention is to provide a carrier-membrane layer integrated molecular sieve membrane prepared from clay and a preparation method thereof, wherein clay is prepared into a porous carrier precursor, and then the clay interface on the surface of the carrier precursor is converted into a dense molecular sieve layer, and finally a carrier-membrane layer integrated molecular sieve membrane with high separation performance is obtained by high-temperature calcination. The carrier is prepared using cheap clay, and the molecular sieve membrane is prepared by non-solvent conversion, and the preparation method is simple.

[0009] Another object of the present invention is to provide an application of a carrier-membrane layer integrated molecular sieve membrane prepared from clay for separation of homogeneous systems, such as separation of mixed gases, separation of alcohol-water mixtures, separation of isomers of organic matter, etc.

[0010] The specific technical solutions of the present invention are as follows:

[0011] The method for preparing a carrier-membrane layer integrated molecular sieve membrane prepared from clay comprises the following steps:

[0012] 1) mixing clay, dispersant, pore former, flux, supplementary material and activator uniformly, forming, and obtaining a carrier precursor;

[0013] 2) placing the carrier precursor in a crystallization reactor, sealing it and performing crystallization synthesis;

[0014] 3) calcining the product of step 2) to form a carrier-membrane layer integrated molecular sieve membrane.

[0015] The clay in step 1) includes, but is not limited to, one or more of kaolin, montmorillonite, attapulgite, illite, diatomite, sepiolite, hydromica, glauconite, and chlorite;

[0016] The clay in step 1) may be pretreated, and the pretreatment includes high temperature heat treatment, acid solution treatment and / or alkaline solution treatment;

[0017] The high temperature heat treatment in step 1) is specifically as follows: heating the clay to 400-900°C, calcining for 0.5h-48h, with a heating and cooling rate of 0.1-30°C / min; high temperature heat treatment in air atmosphere.

[0018] The high temperature heat treatment in step 1) can also be: mixing clay and alkali and then calcining, the calcination conditions are: heating to 400-900°C, calcining for 0.5h-48h, and the heating and cooling rate is 0.1-30°C / min; the mixing mass ratio of the clay and the alkali is 1:0.01-30; the alkali is one or more of sodium hydroxide, potassium hydroxide, lithium hydroxide, cesium hydroxide, magnesium hydroxide or calcium hydroxide;

[0019] The acid solution treatment in step 1) is specifically as follows: adding clay to an acid solution and stirring at 30°C-200°C for 0.5h-24h; the acid solution is one or more of nitric acid, sulfuric acid, hydrochloric acid, and phosphoric acid solution, and the acid concentration is 0.1-10mol / L; the mass concentration of clay in the acid solution is 5-1000mg / mL;

[0020] The alkaline solution treatment in step 1) is specifically as follows: adding clay to an alkaline solution, stirring at 30°C-200°C for 0.5h-24h; the alkaline concentration is 0.1-20mol / L; the mass concentration of clay in the alkaline solution is 5-1000mg / mL; the alkaline solution is one or more of sodium hydroxide, potassium hydroxide, lithium hydroxide, and cesium hydroxide;

[0021] In step 1), the content of the dispersant in step 1) accounts for 0%-50% of the total mass of the carrier precursor; the dispersant includes but is not limited to one or more of water, methanol, ethanol, propanol, ethylene glycol, propylene glycol, butanediol, acetone, ether, tetrahydrofuran, dimethyl ether, N-methylpyrrolidone, N,N-dimethylformamide, and dimethyl sulfoxide;

[0022] The content of the pore-forming agent in step 1) accounts for 0%-40% of the total mass of the carrier precursor; the pore-forming agent includes one or more of a polymer material or an inorganic material; the polymer material includes but is not limited to methyl cellulose, carboxymethyl cellulose, starch, chitosan, urea, polyvinyl chloride, polystyrene, polymethyl methacrylate, polyvinyl butyral, polystyrene, polyethylene glycol, polyethylene, polyvinyl alcohol, polyethylene oxide, polypropylene oxide or one or more; the inorganic material includes but is not limited to one or more of sawdust, graphite, carbon powder, and carbon black;

[0023] The content of the flux in step 1) accounts for 0%-10% of the total mass of the carrier precursor; the flux includes but is not limited to one or more of silicon oxide, aluminum oxide, talc, and titanium dioxide;

[0024] The supplementary material in step 1) is a silicon source, an aluminum source or a phosphorus source supplemented to ensure the silicon-aluminum ratio, phosphorus-silicon ratio or phosphorus-aluminum ratio in the molecular sieve membrane. The silicon-aluminum ratio or phosphorus-aluminum ratio is different in different types of molecular sieves. Even if it is the same molecular sieve, its silicon-aluminum ratio can be adjusted as needed. The silicon source includes but is not limited to one or more of silicon dioxide, silica sol, silicate, and organosilicon. The aluminum source includes but is not limited to one or more of aluminum trioxide, aluminum sol, aluminate, aluminum chloride, aluminum sulfate, boehmite, pseudo-boehmite, aluminum nitrate, aluminum phosphate, and organoaluminum. The phosphorus source includes but is not limited to one or more of phosphoric acid, phosphorus trioxide, phosphorus trichloride, phosphorus pentasulfide, sodium tripolyphosphate, calcium phosphate, and organic phosphide;

[0025] The content of the activator in step 1) accounts for 0%-50% of the total mass of the carrier precursor; the activator includes but is not limited to one or more of ammonia, dimethylamine, trimethylamine, diethylamine, triethylamine, ammonium chloride, sodium chloride, ammonium iodide, ammonium fluoride, sodium fluoride, potassium fluoride, lithium fluoride, ammonium fluorosilicate, ammonium fluoroaluminate, aluminum fluorosilicate, sodium hydroxide, potassium hydroxide, lithium hydroxide, potassium carbonate, lithium carbonate, sodium carbonate, potassium bicarbonate, lithium bicarbonate, sodium bicarbonate, lithium phosphate, sodium phosphate, potassium phosphate, potassium hydrogen phosphate, lithium hydrogen phosphate, sodium hydrogen phosphate, potassium dihydrogen phosphate, lithium dihydrogen phosphate, sodium dihydrogen phosphate;

[0026] The mixing in step 1) refers to mixing the raw materials uniformly by crushing, stirring, ball milling, grinding or slurry refining;

[0027] The forming in step 1) includes forming by extrusion, pressing, injection molding or doctor blade coating;

[0028] The morphology of the carrier precursor in step 1) includes sheet, single tube, multi-channel or hollow fiber;

[0029] In step 2), the carrier precursor is placed in a crystallization kettle, and the crystallization kettle is sealed and transferred to a drying oven for crystallization synthesis, so that the clay interface on the surface of the carrier precursor is converted into a dense molecular sieve layer;

[0030] Step 2) Before placing the carrier precursor in the crystallization reactor, the seed crystal can be assembled first;

[0031] Step 2) Before the carrier precursor is placed in the crystallization reactor, a template can be assembled;

[0032] In step 2), the crystallization kettle may contain an alkaline solution, and the carrier precursor is placed above the alkaline solution in the crystallization kettle and does not contact the alkaline solution; the alkaline solution is one or more of ammonia water or organic amine solution, and the mass content of ammonia water or organic amine in the alkaline solution is 0%-99%;

[0033] The crystallization temperature in step 2) is 60°C-220°C, and the crystallization time is 3h-120h;

[0034] The step 3) is carried out in a muffle furnace, the calcination temperature is 300-1800°C, the calcination time is 0.5h-24h, the heating rate is 0.1-5°C / min, and the temperature can be kept at 200-500°C for 1h-4h during the heating process;

[0035] The molecular sieve membrane prepared in step 3) includes but is not limited to LTA, FAU, MFI, *BEA, TON, SAPO, and CHA.

[0036] Preferably, the preparation method of the LTA molecular sieve membrane is:

[0037] The kaolin is mixed with alkali and then calcined, and then mixed with water, pore-forming agent and activator, and after forming, it is directly transferred to a crystallization kettle for crystallization and calcination to obtain an LTA molecular sieve membrane;

[0038] Preferably, the preparation method of the *BEA molecular sieve membrane is: after bentonite, water, pore-forming agent and activator are mixed, the mixture is formed, and then the template is assembled; the mixture is then placed above the alkaline solution of the crystallization kettle without contacting the alkaline solution, and after crystallization, the mixture is calcined.

[0039] Preferably, the preparation method of the FAU molecular sieve membrane is: pre-treating sepiolite with an acid solution, then mixing it with a pore-forming agent, a supplement and an activator, forming it, assembling seed crystals, placing them above the alkaline solution of a crystallization kettle without contacting the alkaline solution, and calcining them after crystallization.

[0040] Alternatively, preferably, the preparation method of the FAU molecular sieve membrane is: pre-treating kaolin with an acid solution, mixing it with a pore former, a supplement and an activator, and then placing it above the alkaline solution of a crystallization kettle without contacting the alkaline solution, and calcining it after crystallization.

[0041] Preferably, the preparation method of the ZSM-5 molecular sieve membrane is: after mixing attapulgite, a dispersant and an activator, first assembling a template, and then placing it above the alkaline solution of a crystallization kettle without contacting the alkaline solution, and after crystallization, calcining.

[0042] The clay-prepared carrier-membrane layer integrated molecular sieve membrane provided by the present invention is prepared by the above method.

[0043] The application of the carrier-membrane layer integrated molecular sieve membrane prepared from clay provided by the present invention is used for separation of homogeneous systems, such as separation of mixed gases, separation of alcohol-water mixtures, separation of isomers of organic matter, etc. Preferably, it is used for separation of methanol and methyl tert-butyl ether, or for separation of water and ethanol; separation of p-xylene and other xylenes, separation of propanol and water, separation of oil and water, and battery separator, with ultra-high permeation selectivity.

[0044] The traditional molecular sieve membrane preparation process includes the preparation of carrier, preparation of synthetic solution, hydrothermal crystallization and high temperature calcination ( Figure 5 ). The entire process is long, the preparation process is complicated, and it consumes a lot of energy. In addition, the hydrothermal crystallization process requires an excessive amount of synthetic liquid, which can easily cause environmental pollution.

[0045] The present invention uses cheap clay to prepare a carrier-membrane integrated molecular sieve membrane, prepares the clay into a porous carrier precursor, then converts the clay interface on the surface of the carrier precursor into a dense molecular sieve layer, and finally obtains a carrier-membrane integrated molecular sieve membrane with high separation performance by high temperature calcination ( Figure 6 ).

[0046] Compared with the prior art, the present invention uses cheap clay instead of traditional pure chemical substances as carrier raw materials, which not only reduces the preparation cost of the carrier, but also can significantly reduce the calcination temperature of the carrier; the dense clay layer on the surface of the carrier precursor is converted into a molecular sieve membrane by utilizing the characteristic of clay that is easily converted into a molecular sieve, which can improve the density of the molecular sieve membrane; clay is converted into a molecular sieve membrane by a non-solvent conversion method, which can reduce the amount of chemical reagents used, reduce the emission of pollutants, and achieve energy-saving and environmental protection effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 This is a SEM image of the LTA molecular sieve membrane obtained in Example 1;

[0048] Figure 2 This is a SEM image of the *BEA molecular sieve membrane obtained in Example 2;

[0049] Figure 3 This is a SEM image of the FAU molecular sieve membrane obtained in Example 3;

[0050] Figure 4 This is a SEM image of the ZSM-5 molecular sieve membrane obtained in Example 4;

[0051] Figure 5 It is a schematic diagram of the process flow of the traditional preparation method;

[0052] Figure 6 Schematic diagram of the process flow of the preparation method of the invention. DETAILED DESCRIPTION

[0053] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0054] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0055] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0056] Example 1

[0057] The method for preparing a carrier-membrane layer integrated molecular sieve membrane prepared from clay comprises the following steps:

[0058] 1) 1000 g of kaolin (a type of clay, mainly containing kaolinite) and 50 g of sodium hydroxide were mixed and ground, and then calcined at 600° C. for 3 h. After cooling, the mixture was washed with water, filtered, and rinsed with deionized water to obtain pre-treated kaolin;

[0059] 2) 200 g of pre-treated kaolin, 50 g of water (dispersant), 20 g of polyethylene glycol (pore former), 10 g of ammonium fluoride (activator), and 20 g of sodium hydroxide (activator) were stirred and mixed for 20 min, and then extruded into a single-tube carrier precursor using an extruder;

[0060] 3) The tubular carrier precursor is transferred to a crystallization kettle, and then the crystallization kettle is sealed and transferred to a drying oven for crystallization at 100° C. for 72 hours;

[0061] 4) After the crystallization kettle is cooled, the tubular carrier precursor is taken out and placed in a muffle furnace with an air atmosphere at a heating rate of 0.3°C / min, kept at 200°C for 2h, and then heated to 800°C and calcined for 12h to obtain a carrier-membrane integrated LTA molecular sieve membrane.

[0062] Figure 1 This is a SEM image of the LTA molecular sieve membrane obtained in Example 1. As can be seen from the figure, a dense, flat, and defect-free LTA molecular sieve membrane is generated on the surface of the carrier.

[0063] The clay prepared in Example 1 was used to prepare a carrier-membrane layer integrated molecular sieve membrane for separating water and ethanol, specifically:

[0064] The LTA molecular sieve membrane prepared in step 4) was subjected to a pervaporation test. The molecular sieve membrane was fixed to a separation membrane pool, and a 75°C water / ethanol (10 / 90 wt%) mixture was introduced. The operating pressure was 0.1 MPa, and the permeation flux of the LTA molecular sieve membrane was 8.3 kg·m -2 ·h -1 , water / ethanol permeation selectivity is greater than 10000.

[0065] Example 2

[0066] The method for preparing a carrier-membrane layer integrated molecular sieve membrane prepared from clay comprises the following steps:

[0067] 1) 200 g of bentonite (a type of clay, mainly containing montmorillonite), 50 g of water (dispersant), 20 g of polyethylene glycol (pore-forming agent), and 30 g of potassium hydroxide (activator) were mixed and stirred for 20 min, and then extruded into a single-tube carrier precursor using an extruder;

[0068] 2) Immerse the carrier precursor in 1 mol / L tetraethylammonium bromide (template), immerse for 1 min and slowly pull out to obtain a carrier precursor coated with a template, add 10 mL of a 30% tetraethylammonium bromide solution to a crystallization kettle, and then transfer the tubular carrier precursor to the crystallization kettle so that it does not contact the solution, and then seal the crystallization kettle and transfer it to a drying oven at 120° C. for crystallization for 96 h;

[0069] 3) After the crystallization kettle is cooled, the tubular carrier precursor is taken out and placed in a muffle furnace at a heating and cooling rate of 0.3°C / min, wherein it is kept at 200°C for 2 hours, and then heated to 600°C for calcination for 12 hours to obtain a carrier-membrane layer integrated *BEA molecular sieve membrane.

[0070] Figure 2 This is a SEM image of the *BEA molecular sieve membrane obtained in Example 2. As can be seen from the figure, a dense, flat, defect-free *BEA molecular sieve membrane is formed on the surface of the carrier.

[0071] Example 3

[0072] The method for preparing a carrier-membrane layer integrated molecular sieve membrane prepared from clay comprises the following steps:

[0073] 1) adding 10 g of sepiolite to 100 mL of 10 mol / L nitric acid solution, stirring at 50° C. for 24 h, filtering after cooling and washing with deionized water to obtain pre-treated sepiolite;

[0074] 2) 2 g of pre-treated sepiolite, 0.2 g of carboxymethyl cellulose (pore former), 0.5 g of silicon dioxide (supplement), and 0.2 g of sodium hydroxide (activator) were mixed and stirred for 20 min, and then a sheet carrier precursor was prepared by a tabletting method;

[0075] 3) Assembling FAU molecular sieve seeds on the surface of the carrier precursor, specifically: dispersing FAU seeds with a particle size of 200 nm in anhydrous ethanol to prepare 5 g / L FAU seed suspension, then immersing the carrier precursor into the seed suspension, immersing for 30 seconds and slowly pulling out the carrier precursor for assembling FAU molecular sieve seeds, adding 10 mL of 10% ammonia solution by mass to the crystallization kettle, and then transferring the sheet carrier precursor to the crystallization kettle so that it does not contact with the solution, and then sealing the crystallization kettle and transferring it to a drying oven at 140° C. for crystallization for 36 hours;

[0076] 4) After the crystallization kettle is cooled, the tubular carrier precursor is taken out and placed in a muffle furnace at a heating and cooling rate of 0.3°C / min, wherein it is kept at 200°C for 2 hours, and then heated to 1000°C and calcined for 12 hours to obtain a carrier-membrane layer integrated FAU molecular sieve membrane.

[0077] Figure 3This is a SEM image of the FAU molecular sieve membrane obtained in Example 3. As can be seen from the figure, a dense, flat, and defect-free FAU molecular sieve membrane is generated on the surface of the carrier.

[0078] The clay prepared in Example 3 was used to prepare a carrier-membrane layer integrated molecular sieve membrane for separating methanol and methyl tert-butyl ether, specifically:

[0079] The FAU molecular sieve membrane prepared in step 4) was subjected to a pervaporation test. The permeation flux of the FAU molecular sieve membrane was 4.1 kg·m -2 ·h -1 , methanol / methyl tert-butyl ether permeation selectivity is greater than 10,000.

[0080] Example 4

[0081] The method for preparing a carrier-membrane layer integrated molecular sieve membrane prepared from clay comprises the following steps:

[0082] 1) 2 g of attapulgite (a type of clay, mainly containing attapulgite), 0.5 g of polyvinyl alcohol (dispersant), and 0.2 g of ammonium fluoride (activator) were mixed and ground for 30 min, and then pressed into a sheet-like carrier precursor using a tablet press;

[0083] 3) 0.5 mL of 0.5 mol / L tetrapropylammonium bromide (template) was uniformly added dropwise to the surface of the sheet carrier precursor to prepare a carrier precursor for assembling the template agent, 10 mL of 10% ammonia water was added to the crystallization kettle, and then the sheet carrier precursor was transferred to the crystallization kettle so that it did not contact with the solution, and then the crystallization kettle was sealed and transferred to a drying oven at 180° C. for crystallization for 24 h;

[0084] 4) After the crystallization kettle is cooled, the sheet-like carrier precursor is taken out and placed in a muffle furnace with a heating and cooling rate of 0.5°C / min, wherein it is kept at 200°C for 1 hour, and then heated to 500°C and calcined for 6 hours to obtain a carrier-membrane integrated ZSM-5 (a type of MFI) molecular sieve membrane.

[0085] Figure 4 This is a SEM image of the ZSM-5 molecular sieve membrane obtained in Example 4. As can be seen from the image, a dense, flat, and defect-free ZSM-5 molecular sieve membrane is formed on the surface of the carrier.

[0086] The clay prepared in Example 4 is used to prepare a carrier-membrane layer integrated molecular sieve membrane for separating p-xylene from other xylenes, specifically:

[0087] The permeability performance of the ZSM-5 molecular sieve membrane prepared in step 4) was tested. The permeability flux of the ZSM-5 molecular sieve membrane was 6.5 kg·m -2 ·h -1The permeation selectivity of p-xylene relative to other xylenes (m-xylene, o-xylene) is greater than 1000.

[0088] Example 5

[0089] The method for preparing a carrier-membrane layer integrated molecular sieve membrane prepared from clay comprises the following steps:

[0090] 1) Add 10 g of kaolin to 100 mL of 1 mol / L nitric acid solution, stir at 80° C. for 6 h, filter after cooling, and wash with deionized water to obtain pre-treated kaolin;

[0091] 2) 2 g of pre-treated kaolin, 0.5 g of methyl cellulose (pore former), 0.3 g of silica sol (supplement), and 0.5 g of potassium hydroxide (activator) were mixed and ground for 30 min, and then pressed into a sheet-like carrier precursor using a tablet press;

[0092] 3) Transfer the sheet-like carrier precursor to a crystallization kettle, add 5 mL of 40% tetramethylammonium hydroxide (organic amine solution) to the crystallization kettle, so that the carrier precursor is above the tetramethylammonium hydroxide and does not contact the solution, then seal the crystallization kettle and transfer it to a drying oven at 120° C. for crystallization for 12 hours;

[0093] 4) After the crystallization kettle is cooled, the sheet-like carrier precursor is taken out and placed in a muffle furnace with a heating and cooling rate of 2°C / min, wherein it is kept at 200°C for 1 hour, and then heated to 900°C and calcined for 18 hours to obtain a carrier-membrane layer integrated FAU molecular sieve membrane.

[0094] The clay prepared in Example 5 was used to prepare a carrier-membrane layer integrated molecular sieve membrane for separating methanol and methyl tert-butyl ether, specifically:

[0095] The FAU molecular sieve membrane prepared in step 4) was subjected to a pervaporation test. The permeation flux of the FAU molecular sieve membrane was 7.2 kg·m -2 ·h -1 , methanol / methyl tert-butyl ether permeation selectivity is greater than 10,000.

Claims

1. A method for preparing a carrier-membrane layer integrated molecular sieve membrane prepared from clay, characterized in that: The preparation method comprises the following steps: 1) mixing clay, dispersant, pore former, flux, supplementary material and activator uniformly, forming, and obtaining a carrier precursor; 2) placing the carrier precursor in a crystallization reactor, sealing it and performing crystallization synthesis; 3) calcining the product of step 2) to form a carrier-membrane layer integrated molecular sieve membrane.

2. The preparation method according to claim 1, characterized in that: The clay in step 1) includes, but is not limited to, one or more of kaolin, montmorillonite, attapulgite, illite, diatomite, sepiolite, hydromica, glauconite, and chlorite.

3. The preparation method according to claim 1 or 2, characterized in that: The clay in step 1) may be pretreated, and the pretreatment includes high temperature heat treatment, acid solution treatment and / or alkaline solution treatment.

4. The preparation method according to claim 1, characterized in that: The content of the dispersant in step 1) accounts for 0%-50% of the total mass of the carrier precursor; the dispersant includes but is not limited to one or more of water, methanol, ethanol, propanol, ethylene glycol, propylene glycol, butylene glycol, acetone, ether, tetrahydrofuran, dimethyl ether, N-methylpyrrolidone, N,N-dimethylformamide, and dimethyl sulfoxide; the content of the pore-forming agent in step 1) accounts for 0%-40% of the total mass of the carrier precursor; the pore-forming agent includes one or more of polymer materials or inorganic materials; the polymer materials include but are not limited to methyl cellulose, carboxymethyl cellulose, starch, chitosan, urea, polyvinyl chloride, polystyrene, polymethyl methacrylate, polyvinyl butyral, polystyrene, polyethylene glycol, polyethylene, polyvinyl alcohol, polyoxyethylene, and polyoxypropylene; the inorganic materials include but are not limited to one or more of sawdust, graphite, carbon powder, and carbon black.

5. The preparation method according to claim 1, characterized in that: The content of the flux in step 1) accounts for 0%-10% of the total mass of the carrier precursor; the flux includes but is not limited to one or more of silicon oxide, aluminum oxide, talc, and titanium dioxide; the supplementary material in step 1) is a silicon source, aluminum source or phosphorus source supplemented to ensure the silicon-aluminum ratio, phosphorus-silicon ratio or phosphorus-aluminum ratio in the molecular sieve membrane; the content of the activator in step 1) accounts for 0%-50% of the total mass of the carrier precursor; the activator includes but is not limited to ammonia water, dimethylamine, trimethylamine, diethylamine, triethylamine, ammonium chloride, sodium chloride, ammonium iodide, ammonium fluoride, sodium fluoride, potassium fluoride, lithium fluoride, ammonium fluorosilicate, ammonium fluoroaluminate, aluminum fluorosilicate, sodium hydroxide, potassium hydroxide, lithium hydroxide, potassium carbonate, lithium carbonate, sodium carbonate, potassium bicarbonate, lithium bicarbonate, sodium bicarbonate, lithium phosphate, sodium phosphate, potassium phosphate, potassium hydrogen phosphate, lithium hydrogen phosphate, sodium hydrogen phosphate, potassium dihydrogen phosphate, lithium dihydrogen phosphate, sodium dihydrogen phosphate One or more.

6. The preparation method according to claim 1, characterized in that: In step 2), the crystallization kettle contains an alkaline solution, and the carrier precursor is placed above the alkaline solution in the crystallization kettle without contacting the alkaline solution; the alkaline solution is one or more of ammonia water or organic amine solution, and the mass content of ammonia water or organic amine in the alkaline solution is 0%-99%.

7. The preparation method according to claim 1, characterized in that: The crystallization temperature in step 2) is 60°C-220°C, and the crystallization time is 3h-120h.

8. The preparation method according to claim 1, characterized in that: The calcination is carried out in a muffle furnace in step 3), the calcination temperature is 300-1800° C., the calcination time is 0.5h-24h, the heating and cooling rate is 0.1-5° C. / min, and the temperature is maintained at 200-500° C. for 1h-4h during the heating process.

9. A molecular sieve membrane with integrated carrier and membrane layer prepared by the clay prepared by the preparation method according to any one of claims 1 to 8.

10. An application of the clay according to claim 9 to prepare a carrier-membrane layer integrated molecular sieve membrane, characterized in that: Used for separation of homogeneous mixtures.

Citation Information

Patent Citations

  • ZSM-5 molecular sieve and preparation method thereof

    CN104843740A

  • Method for preparing NaA molecular sieve membrane by inner surface of asymmetric micro-pore ceramic

    CN106478079A

  • Hierarchical porous SAPO-34 / kaolin composite material and preparation method thereof

    CN106582804A

  • Preparation method for supported ultrathin two-dimensional molecular sieve membrane and application of supported ultrathin two-dimensional molecular sieve film

    CN109850913A

  • Preparation method of attapulgite-based NaA molecular sieve membrane support body

    CN112371081A