Glass panel unit, getter material, getter material composition, and method for manufacturing glass panel unit

By using zeolite crystals of 200 nm or larger particles and hydrogenation catalysts, an excellent getter material composition was prepared, which solved the problem of insufficient adsorption performance of glass panel units at low temperatures, and achieved efficient gas adsorption and heat in the low pressure range Insulation effect.

CN118874403APending Publication Date: 2024-11-01PANASONIC LIVING SPACE CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410833312.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2020-11-18
Filing Date
2021-04-26
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When the existing glass panel units are manufactured at low temperatures, the adsorption performance of the getter material is insufficient, especially in the low pressure range, and the particle size and activation temperature information of the zeolite are not fully utilized.

Method used

Using a getter material containing zeolite crystals of 200 nm or larger particles, a getter material composition with excellent gas adsorption properties is prepared by heating and activation of the zeolite during the manufacturing process, combining a hydrogenation catalyst and an appropriate solvent, and in a glass Used in panel units for efficient gas adsorption.

Benefits of technology

The gas adsorption capacity of glass panel units is significantly improved within the low pressure range, reducing manufacturing costs, simplifying the process flow, and improving thermal insulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874403A_ABST
    Figure CN118874403A_ABST
Patent Text Reader

Abstract

The problem to be overcome by the present disclosure is to provide a glass panel unit having a getter material that achieves sufficient adsorption performance in a low pressure range, and also to provide such a getter material. A glass panel unit 10 includes: a first glass plate 20; a second glass sheet 30 facing the first glass sheet 20; a frame member 40; evacuating the space 50; and a gas adsorbent 60. The frame member 40 sealingly bonds the first glass plate 20 and the second glass plate 30. The evacuated space 50 is surrounded by the first glass plate 20, the second glass plate 30, and the frame member 40. A gas adsorbent 60 is placed in the evacuated space 50. The gas adsorbent 60 contains a getter material. The getter material contains a plurality of particles of zeolite crystals. Particles having a particle size of 200 nm or more comprise more than half of the total weight of the plurality of particles. The plurality of particles have an activatable temperature equal to or lower than 400 DEG C.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of the PCT international application PCT / JP2021 / 016576 filed on April 26, 2021, which entered the Chinese national stage on November 3, 2022, and the Chinese patent application number is 202180032767.0, and the invention name is "Glass panel unit, air-absorbing material, air-absorbing material composition and method for manufacturing glass panel unit". Technical Field

[0002] The present disclosure generally relates to glass panel units, getter materials, getter material compositions, and methods for making glass panel units. More specifically, the present disclosure relates to thermally insulating glass panel units, getter materials, getter material compositions, and methods for making such glass panel units. Background Art

[0003] Patent Document 1 discloses a glass panel unit including a gas adsorbent therein. Patent Document 1 also teaches the use of a zeolite-based material as the gas adsorbent.

[0004] Reference List

[0005] Patent Literature

[0006] Patent Document 1: WO 2019 / 004135 A1 Summary of the invention

[0007] However, Patent Document 1 does not disclose the contents regarding the size of zeolite used as a constituent material of the gas adsorbent, and thus there is still room for improvement.

[0008] The problem to be overcome by the present disclosure is to provide a glass panel unit with an absorbent material, which can achieve sufficient adsorption performance within a low pressure range even if the manufacturing process of the glass panel unit is performed at a lower temperature; and also to provide such an absorbent material, an absorbent material composition, and a method for manufacturing such a glass panel unit.

[0009] A glass panel unit according to one aspect of the present disclosure includes: a first glass plate; a second glass plate facing the first glass plate; a frame member; an evacuated space; and a gas adsorbent. The frame member seals the first glass plate to the second glass plate. The evacuated space is surrounded by the first glass plate, the second glass plate and the frame member. The gas adsorbent is placed in the evacuated space. The gas adsorbent contains a getter material. The getter material contains a plurality of particles of zeolite crystals. Particles having a particle size of 200 nm or more account for more than half of the total weight of the plurality of particles. The activatable temperature of the plurality of particles is equal to or lower than 400°C.

[0010] A glass panel unit according to another aspect of the present disclosure includes: a first glass plate; a second glass plate facing the first glass plate; a frame member; an evacuated space; and a gas adsorbent. The frame member seals the first glass plate to the second glass plate. The evacuated space is surrounded by the first glass plate, the second glass plate and the frame member. The gas adsorbent is placed in the evacuated space. The gas adsorbent contains a getter material. The getter material contains a plurality of particles of zeolite crystals. Particles having a particle size of 200 nm or more account for more than half of the total number of the plurality of particles. The activatable temperature of the plurality of particles is equal to or lower than 400°C.

[0011] A glass panel unit according to another aspect of the present disclosure includes: a first glass plate; a second glass plate facing the first glass plate; a frame member; an evacuated space; and a gas adsorbent. The frame member seals the first glass plate to the second glass plate. The evacuated space is surrounded by the first glass plate, the second glass plate and the frame member. The gas adsorbent is placed in the evacuated space. The gas adsorbent contains a getter material. The getter material contains a plurality of particles of zeolite crystals. Particles having a particle size of 200 nm or more account for more than half of the total volume of the plurality of particles. The activatable temperature of the plurality of particles is equal to or lower than 400°C.

[0012] A glass panel unit according to another aspect of the present disclosure includes: a first glass plate; a second glass plate facing the first glass plate; a frame member; an evacuated space; and a gas adsorbent. The frame member seals the first glass plate and the second glass plate together. The evacuated space is surrounded by the first glass plate, the second glass plate, and the frame member. The gas adsorbent is placed in the evacuated space. The gas adsorbent contains a getter material. The getter material contains a plurality of particles of zeolite crystals and a hydrogenation catalyst.

[0013] A getter material according to another aspect of the present disclosure contains a plurality of particles of zeolite crystals. Particles having a particle size of 200 nm or more account for more than half of the total weight of the plurality of particles. The activatable temperature of the plurality of particles is equal to or lower than 400°C.

[0014] A getter material composition according to another aspect of the present disclosure contains a getter material and a solvent. The getter material contains a plurality of particles of zeolite crystals. The activatable temperature of the plurality of particles is equal to or lower than 400°C.

[0015] A getter material composition according to another aspect of the present disclosure contains a getter material and a solvent. The getter material contains a plurality of particles of zeolite crystals. The plurality of particles include particles having a particle size equal to or greater than 200 nm.

[0016] According to another aspect of the present disclosure, a method for manufacturing a glass panel unit includes a processing step, an assembly step, a bonding step, and an exhaust step. The processing step includes preparing the above-mentioned getter material composition. The assembly step includes preparing an assembly, the assembly including a first glass plate, a second glass plate, a peripheral wall having a frame shape, an internal space, a gas adsorbent made of the above-mentioned getter material composition, and an exhaust port. The bonding step includes sealingly bonding the first glass plate to the second glass plate by melting the peripheral wall. The exhaust step includes exhausting gas from the internal space through the exhaust port to convert the internal space into an evacuated space.

[0017] A glass panel unit according to another aspect of the present disclosure includes: a first glass plate; a second glass plate facing the first glass plate; a frame member; an evacuated space; and a gas adsorbent. The frame member seals the first glass plate to the second glass plate. The evacuated space is surrounded by the first glass plate, the second glass plate and the frame member. The gas adsorbent is placed in the evacuated space. The gas adsorbent contains a getter material. The getter material contains a plurality of particles of zeolite crystals. Particles having a particle size of 200 nm or more account for more than half of the total weight of the plurality of particles. At least one of the softening point, melting point or bondable temperature of the sealant is equal to or lower than 350°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 A is a plan view illustrating a component as an intermediate product of a glass panel unit according to a first embodiment;

[0019] Figure 1 B is along Figure 1 A cross-sectional view thereof taken by plane AA in A;

[0020] Figure 2 is a plan view illustrating a glass panel unit;

[0021] Figure 3 illustrates a step of a method for manufacturing a glass panel unit according to a first embodiment;

[0022] Figure 4 illustrates another step of the method for manufacturing a glass panel unit according to the first embodiment;

[0023] Figure 5 illustrates a further step of the method for manufacturing a glass panel unit according to the first embodiment;

[0024] Figure 6 shows how to carry out the various steps of the method for manufacturing a glass panel unit according to a first embodiment;

[0025] Figure 7illustrates a further step of the method for manufacturing the glass panel unit according to the first embodiment;

[0026] Figure 8 illustrates a further step of the method for manufacturing the glass panel unit according to the first embodiment;

[0027] Fig. 9 is a graph showing the relationship between equilibrium pressure and the amount of adsorbed gas;

[0028] Fig.10 is a graph showing the relationship between equilibrium pressure and the amount of gas adsorbed on a logarithmic axis;

[0029] Fig.11 is a graph showing the relationship between the ratio of the amount of adsorbed gas and the activation temperature;

[0030] Fig.12 is a graph showing the relationship between the amount of residual gas and the size of crystals (particles);

[0031] Fig.13 A is a graph showing the relationship between the amount of residual gas in each of water and an organic solvent and the size of crystals (particles); and

[0032] Fig.13 B is a graph showing the relationship between the ratio of the respective residual gas amounts and the size of the crystals (particles). DETAILED DESCRIPTION

[0033] First, how the inventors conceived the concept of the present disclosure will be described.

[0034] The glass panel unit is provided with thermal insulation properties by creating an evacuated space (or vacuum space) between two glass plates. However, if any residual gas remains in the evacuated space, such thermal insulation properties of the glass panel unit are reduced despite the presence of the evacuated space between the two glass plates. Therefore, in order to reduce the amount of such residual gas remaining in the evacuated space, a gas adsorbent is provided in the evacuated space. A gas adsorbent including a zeolite getter material has been used in the art (see Patent Document 1).

[0035] When placed in air or solution, zeolite adsorbs a large amount of gas therein. Therefore, in order to use zeolite as a gas adsorbent to achieve sufficient adsorption performance in an evacuated space, its adsorption sites need to be exposed by heating the zeolite in a vacuum and thereby desorbing the gas adsorbed into the zeolite (i.e., activating the zeolite). In particular, in copper ion exchange zeolites, strong nitrogen adsorption sites are exposed by reducing copper oxide (i.e., desorbing oxygen from copper oxide). At this point, unless the zeolite is activated at a sufficiently high temperature, oxygen and other gases (such as moisture) cannot be desorbed, and sufficient adsorption performance cannot be achieved.

[0036] During the manufacturing process of the glass panel unit, the zeolite can be activated (for example, in the exhaust step), which starts in the middle or at the end of the first melting step (combining step). At this time, if the zeolite can be sufficiently heated during the exhaust step, sufficient adsorption performance can be achieved. At the same time, in order to shorten the production cycle time, simplify the manufacturing equipment, and cope with reinforced glass, there has been a growing demand for conducting the glass panel unit manufacturing process at a lower temperature. This is why the zeolite preferably exhibits a sufficiently strong adsorption capacity even in the low-temperature exhaust step (i.e., it is preferably activated at a lower temperature).

[0037] When exposed to ultraviolet rays during the manufacturing process of the glass panel unit, or when the glass panel unit is being used after its manufacturing process, even nitrogen (which is generally difficult to adsorb in the low pressure range) is released. Therefore, copper ion exchange type zeolite having the ability to adsorb nitrogen is also particularly preferred. However, unless the copper ion exchange type zeolite is fully activated in a low temperature process (for example, in a degassing step performed at low temperature, or in an activation step performed at low temperature), it is difficult to reveal a strong adsorption site for nitrogen, and sufficient adsorption performance cannot be achieved.

[0038] In the particles of zeolite crystals, their surfaces have many micropores, through which the target gas is absorbed and retained in a complex internal space. Generally, it is believed that the gas adsorption capacity of such zeolite particles is proportional to the size of the surface area. For the total surface area of ​​zeolite particles, if the total weight of a large number of zeolite particles is constant (in other words, the smaller the particle size of the zeolite particles, the larger the number of zeolite particles per unit weight), the total surface area of ​​the zeolite particles increases. This is why the gas adsorption capacity per unit weight increases as the particle size of the zeolite particles decreases. It should be noted that the size of the zeolite particles is considered to be synonymous with the size (crystal size) of the zeolite crystals in this article. In addition, the zeolite particles described herein are considered to be primary particles. That is to say, zeolite particles are not aggregates (secondary particles), but zeolite crystals.

[0039] However, the inventors have found through extensive research that even if the total volume of the zeolite particles is constant in a low pressure range (particularly in a range close to vacuum) in which the pressure is reduced from atmospheric pressure to a predetermined degree, a higher gas adsorption capacity can be achieved when the zeolite particles have a relatively large particle size than when the zeolite particles have a relatively small particle size. The inventors have also found that this trend increases significantly, particularly when the zeolite is activated at low temperatures. The inventors conceived the concept of the present disclosure by finding that a strong gas adsorption capacity will be achieved in a low pressure range by utilizing this property of the zeolite particles. That is, this embodiment enables the provision of a getter material and a getter material composition that will achieve thermal insulation in a vacuum space or an evacuated space to obtain a gas adsorbent having a strong gas adsorption capacity in a low pressure range.

[0040] <First embodiment>

[0041] Next, an overview of the glass panel unit 10 and a method for manufacturing the glass panel unit 10 according to the first embodiment will be described.

[0042] like Figure 2 As shown in FIG. 1 , the glass panel unit 10 includes a first glass plate 20, a second glass plate 30 facing the first glass plate 20, a frame member 40, an evacuated space 50, and a gas adsorbent 60. The frame member 40 seals the first glass plate 20 and the second glass plate 30. The evacuated space 50 is surrounded by the first glass plate 20, the second glass plate 30, and the frame member 40. The gas adsorbent 60 is placed in the evacuated space 50. The gas adsorbent 60 contains a getter material.

[0043] The method for manufacturing such a glass panel unit 10 includes a processing step, an assembly step (see Figure 3-Figure 5 ), the combining step (the first melting step, see Figure 6 ) and exhaust steps (see Figure 6 ). The processing step includes a getter material preparation step. The getter material preparation step includes obtaining a getter material including a plurality of particles of zeolite crystals. The assembling step includes preparing an assembly 100. The assembly 100 includes a first glass plate 200, a second glass plate 300, an outer peripheral wall 410 having a frame shape, an inner space 500, a gas adsorbent 60, and an exhaust port 700 (see Figure 1 A and Figure 1B). The second glass plate 300 faces the first glass plate 200. The peripheral wall 410 is disposed between the first glass plate 200 and the second glass plate 300. The internal space 500 is surrounded by the first glass plate 200, the second glass plate 300 and the peripheral wall 410. The gas adsorbent 60 is placed in the internal space 500 and contains a getter material. The exhaust port 700 allows the internal space 500 to communicate with the external environment. The bonding step includes melting the peripheral wall 410 to seal the first glass plate 200 and the second glass plate 300. The exhaust step includes exhausting gas from the internal space 500 through the exhaust port 700 to convert the internal space 500 into an evacuated space 50. Figure 1-Figure 8 A method for manufacturing the glass panel unit 10 (hereinafter referred to as "manufacturing method") is described in detail. Figure 2 In the following description of this embodiment, direction D1 is a direction parallel to the thickness of the first glass plate 200, direction D2 is a direction perpendicular to direction D1, and direction D3 is a direction perpendicular to both direction D1 and direction D2. Alternatively, these directions D1, D2, and D3 may also be simply regarded as the first direction, the second direction, and the third direction, respectively.

[0044] The manufacturing method includes a preparation step and a removal step.

[0045] The preparation step is to provide Figure 7 The semi-finished product 110 is made of Figure 1 A and Figure 1 The assembly 100 shown in B is formed. That is, the semi-finished product 110 is being manufactured into the glass panel unit 10 (see Figure 2 ) is an intermediate product obtained when the semi-finished product 110 is being formed.

[0046] The preparation steps include processing steps, assembly steps (see Figure 3-Figure 5 ), the combining step (the first melting step; see Figure 6 ), exhaust steps (see Figure 6 ) and the sealing step (second melting step; see Figure 6 and Figure 7 ).

[0047] The processing step is a step of preparing a getter material composition. The getter material composition contains at least zeolite and a solvent (for example, at least one of water or an organic solvent). The gas adsorbent 60 is a dried product of the getter material composition. The processing step includes a heating step, a getter material preparation step, and a mixing step. It should be noted that the getter material composition is preferably a fluid substance (such as a liquid, a paste, an ink, or a slurry), and is preferably capable of being provided, for example, by application or printing.

[0048] The heating step is a step of heating the zeolite contained in the gas adsorbent 60. The temperature of the heating step is preferably higher than the temperature of the exhaust step (i.e., the exhaust temperature Te to be described later), more preferably higher than the temperature of the first melting step (i.e., the first melting temperature Tm1 to be described later), and particularly preferably higher than the temperature of the second melting step (i.e., the second melting temperature Tm2 to be described later). This makes it possible to desorb the gas components that have been adsorbed by the zeolite before manufacturing the component 100. In particular, heating the zeolite in the heating step makes it possible to desorb the oxygen that has been adsorbed in the zeolite by the heating step. This can reduce the amount of oxygen desorbed from the bonding step, and thus the exhaust step can be performed at a lower temperature. Therefore, the first melting step and the second melting step can also be performed at a lower temperature. This can ultimately reduce the manufacturing cost of the glass panel unit 10. It should be noted that the heating step is an optional step and can be omitted.

[0049] Zeolite is a very small particle (fine particle) made of porous crystals, and its surface has many micropores. The gas to be adsorbed is introduced through the micropores of the zeolite and is retained (adsorbed) in a complex internal space. Examples of such gases to be adsorbed into zeolite include water vapor, carbon dioxide, oxygen, nitrogen and hydrocarbons (such as methane). In addition, zeolite can adsorb gases that are difficult to adsorb by any other general adsorbents, such as nitrogen and hydrocarbons (especially nitrogen) in the evacuated space. The zeolite structure has a composition represented by the following general formula (1):

[0050] Me 2 / x O·Al2O3·mSiO2·nH2O,…(1)

[0051] Wherein Me is a cation having a valence of x and existing in the micropores, m is a silica / alumina ratio and is an integer equal to or greater than 2, and n is an integer equal to or greater than 0. In the composition represented by this formula (1), a monovalent negative charge is generated at each Al atom. Therefore, if Me is a cation having a valence of 2 or more, a positive charge is generated in the micropores of the zeolite. On the other hand, if Me is a monovalent cation, the inside of the micropore becomes electrically neutral.

[0052] In the zeolite structure, Me can be a monovalent cation, or a cation having a valence of 2 or more, or a combination of a monovalent cation and a cation having a valence of 2 or more. Examples of monovalent cations include: alkali metal ions, such as Li + 、Na + and K + ; proton; ammonium ion (NH4 + ) and Ag + Examples of cations having a valence of 2 or more include alkaline earth metal ions such as Ca 2+ Mg 2+ and Ba 2+ ; and transition metal ions such as Cu 2+ 、Au 2+ , Fe 2+ 、Zn 2+ and Ni 2+ .

[0053] Examples of the zeolite structure include an A-type zeolite structure, an X-type zeolite structure, a Y-type zeolite structure, an L-type zeolite structure, a β-type zeolite structure, a mordenite structure, a ferrierite structure, a USY zeolite structure, a CHA-type zeolite structure, a SAPO-type zeolite structure, and a ZSM-5 zeolite structure (MFI). The zeolite may have any zeolite structure other than these structures.

[0054] In the general formula (1), water (HO) is contained in the zeolite in the form of crystal water. For example, such water can be contained in the micropores of the zeolite particles. Heating the zeolite allows not only the crystal water but also the gas components (such as oxygen) that have been adsorbed before heating to desorb from the zeolite. This can improve the gas adsorption of the zeolite. It should be noted that if the crystal water is completely desorbed, n in the general formula (1) becomes equal to zero.

[0055] The zeolite obtained by the heating step is suitably a zeolite from which oxygen has been desorbed and to which at least one component selected from nitrogen, carbon monoxide and water (hereinafter sometimes referred to as "adsorbed component") has been adsorbed. That is, the adsorption capacity of the zeolite obtained by the heating step is preferably saturated with the adsorbed component. In this case, desorbing the adsorbed component from the zeolite during heating in the exhaust step allows the zeolite to recover its gas adsorption properties, for example. It should be noted that if the zeolite that has been subjected to the heating step is mixed with water, the nitrogen or methane (if any) adsorbed to the zeolite will be partially replaced by water.

[0056] The zeolite preferably contains a copper ion exchange type zeolite. The copper ion exchange type zeolite is a component represented by the general formula (1) (wherein Me is a copper ion). In this case, the copper ion exchange type zeolite is a component in which the copper ion is loaded by the zeolite structure. Therefore, "copper ion exchange type zeolite" does not specify the component before the copper ion is loaded by the zeolite structure. In addition, the crystal structure of the zeolite is more preferably a ZSM-5 type. Copper ion exchange ZSM-5 type zeolite (Cu-ZSM-5) can thoroughly adsorb nitrogen, methane and other gases under low pressure even at room temperature. It should be noted that the silica / alumina ratio of the ZSM-5 type is preferably represented by a molar ratio equal to or less than 100, and more preferably represented by a molar ratio equal to or greater than 20 and equal to or less than 45. However, this is only an example and should not be interpreted as restrictive. In addition, the copper content preferably falls within the range of 1% by weight to 10% by weight. However, this is only an example and should not be interpreted as restrictive. The zeolite crystals contained in the gas adsorbent 60 according to the present disclosure have predetermined conditions as will be described in detail later.

[0057] The getter material preparation step is a step of obtaining a getter material based on a zeolite that has been subjected to a heating step or has not yet been heated. The getter material preparation step may include, for example, obtaining a composite getter material by mixing zeolite particles (crystals) and particles of a compound other than zeolite. In addition, the getter material preparation step also includes a step of preparing a plurality of particles having a predetermined particle size distribution (including zeolite particles and different types of zeolite particles or particles of a compound other than zeolite). For example, the getter material may include a plurality of types of zeolites having different compositions, crystal structures or particle size distributions from each other, and may also include non-zeolite particles. After the getter material preparation step has been performed, the mixing step is performed.

[0058] The mixing step is a step of obtaining a getter material composition by mixing a getter material and a solvent. The getter material comprises a plurality of particles of zeolite crystals as described above. Optionally, the getter material may comprise particles of a compound other than zeolite. Water, an organic solvent, or a mixture of water and an organic solvent may be used as the solvent.

[0059] If water is used as a solvent, water is present in the getter material composition to cover the getter material. This reduces the possibility of the getter material in the getter material composition state being exposed to the air. In other words, this makes it less likely that the getter material will adsorb air (especially oxygen in the air). This makes the getter material composition easier to store and reduces problems in manufacturing the glass panel unit 10. The content of water in the getter material composition can be selected arbitrarily. Water can be used as a solvent. Alternatively, a solution containing water as a main component can also be used as a solvent. For example, the solvent can be water containing organic matter, calcium, sodium and other components as impurities.

[0060] Alternatively, the solvent may also be a mixture of water and an organic solvent. In this case, the solvent may be a mixed solvent in which water and up to 50% by mass of an organic solvent (such as ethanol) are mixed. Alternatively, the organic solvent may also be an organic solvent such as ethanol, butyl carbitol acetate, or terpineol, or a mixture thereof. If water is used as the solvent, pure water, ultrapure water, ion exchange water, or distilled water may be preferably used as much as possible.

[0061] On the other hand, if an organic solvent is used as the solvent, the molecular size of the organic solvent is preferably approximately the same as or larger than the micropore size of the zeolite (particularly ZSM-5 zeolite). The molecular size of the organic solvent (i.e., the maximum width of the molecule) is preferably equal to or greater than

[0062] If the molecular size of the organic solvent is approximately the same as the size of the micropores of the zeolite, the number of solvent molecules that enter the micropores of the zeolite is reduced. That is, the rate at which the organic solvent molecules diffuse into the zeolite is reduced, and the number of organic solvent molecules that diffuse into the interior of the zeolite crystals is also reduced. Therefore, the organic solvent molecules remain near the surface of the zeolite particles, and therefore not as much energy is required to desorb those organic solvent molecules.

[0063] In addition, if the molecular size of the organic solvent is larger than the micropore size of the zeolite, most of the organic solvent molecules cannot enter the micropores of the zeolite. Therefore, the organic solvent molecules remain on the surface of the zeolite particles, and thus even less energy is required to desorb those organic solvent molecules.

[0064] Therefore, if the molecular size of the organic solvent is approximately the same size as or larger than the micropore size of the zeolite, little organic solvent has diffused into the interior of the zeolite, and therefore, when the gas adsorbent 60 is formed by removing the solvent from the getter material composition, not much energy is required to remove the solvent. In addition, this also reduces the possibility of the organic solvent remaining inside the zeolite, making it easier to achieve the advantages by increasing the particle size of the zeolite.

[0065] On the other hand, if the molecular size of the organic solvent is smaller than the pore size of the zeolite, the organic solvent molecules will diffuse into the interior of the zeolite crystals. In this case, a large amount of energy will be required to desorb the organic solvent molecules.

[0066] The molecular size is larger than the pore size of zeolite (ZSM-5) And examples of the organic solvent which is an aromatic compound include trimethylbenzene, tetramethylbenzene, pentamethylbenzene, hexamethylbenzene and m-xylene.

[0067] The molecular size is larger than the pore size of zeolite (ZSM-5) And examples of the organic solvent which is a non-aromatic compound include cyclic compounds each having a cyclic structure such as cyclooctane, cycloheptane, dimethylquinoline, α-pinene, β-pinene, pinane, α-pinene oxide, pinethoxyl, caryophyllene, verbenone, and isobornylcyclohexanol.

[0068] Molecular size and pore size of zeolite (ZSM-5) Examples of organic solvents of approximately the same size include cyclic compounds each having a ring structure, such as p-xylene, p-menthane, d-limonene, l-limonene, α-terpineol, β-terpineol, γ-terpineol, terpinene, menthol, myrtenal, myrtenol, p-menthane, benzyl benzoate, dihydroterpineol, and dihydroterpineol acetate.

[0069] It can be seen that according to the present disclosure, cyclic compounds (including aromatic compounds or non-aromatic compounds) having a cyclic structure are preferably used as organic solvents. Meanwhile, molecules of organic solvents having a linear structure will easily enter the micropores of zeolite even if their molecular size is large, and are therefore not preferred. In addition, among various cyclic compounds, aromatic compounds are often harmful to the human body, and it is preferred to avoid using aromatic compounds as much as possible. On the contrary, it is preferred to use non-aromatic compounds as organic solvents.

[0070] In addition, it is generally believed that molecules with strong polarity (e.g., organic solvent molecules having OH groups) will be more easily attracted to the polarity of zeolite and will not be easily desorbed. However, the present inventors found that when copper ion exchange type zeolite (Cu-ZSM-5) and various organic solvents were mixed to observe whether the solvent component was desorbed when heated using GCMS, the molecular size and the micropore size of zeolite (ZSM-5) were different. Among various organic solvents of approximately the same size, the molecules of organic solvents (such as p-xylene, p-menthane and d-limonene) with weak polarity and only composed of carbon and hydrogen tend to be less prone to desorption even when heated, and are retained in Cu-ZSM-5 inside. This may be because when zeolite is mixed with solvent, the molecules without polarity will spend a long time to diffuse and enter the inside of zeolite, and the molecules are stored as a part of mixed solution at the same time. On the other hand, solvent molecules containing OH groups or elements such as O, F or N and with relatively strong polarity will be adsorbed around the opening of zeolite micropores to close micropores, and themselves will prevent other molecules from entering micropores, thereby eventually reducing the possibility of solvent molecules diffusing into the inside of zeolite particles. The larger the crystal size of zeolite, the more significantly this advantage is achieved. This is why the crystal size of zeolite is set at, for example, 200nm or larger is advantageous. The crystal size of zeolite is more preferably equal to or greater than 400nm, even more preferably equal to or greater than 500nm, particularly preferably equal to or greater than 600nm. It is even better if the crystal size of the zeolite is equal to or greater than 750 nm, equal to or greater than 1000 nm, equal to or greater than 1500 nm, or equal to or greater than 2000 nm.

[0071] On the other hand, for molecules with a size larger than the pore size of zeolite (ZSM-5) Molecules of organic solvents consisting only of carbon and hydrogen and having weak polarity (such as α-pinene and β-pinene) make it easy to desorb the solvent from Cu-ZSM-5. This is why it is preferred to use a pore size larger than that of the zeolite (ZSM-5). organic solvents, or molecular size and pore size of zeolite (ZSM-5) The reason is that the organic solvent is approximately the same size and has an OH group or an element such as O, N or F in the molecular structure. That is, the organic solvent to be mixed with the Cu-ZSM-5 type zeolite (whose crystal size is equal to or greater than 200nm) preferably includes at least one selected from the following: cyclooctane, cycloheptane, dimethylquinoline, α-pinene, β-pinene, pinane, α-pinene oxide, pinethoxyl, caryophyllene, verbenone, isobornylcyclohexanol, α-terpineol, β-terpineol, γ-terpineol, menthol, myrtenal, myrtenol, benzyl benzoate, dihydroterpineol and dihydroterpineol acetate. In addition, if the processing temperature of the glass panel unit (multi-plate glass unit) is equal to or lower than 350°C (at which the solvent is less likely to be desorbed from the zeolite), this advantage will be particularly significantly achieved. That is, it is more advantageous if at least one of the softening point, melting point, or bondable temperature (the minimum temperature required to seal the glass panel unit with the sealant) of the sealant (which is at least one of the first sealant or the second sealant) is equal to or lower than 350° C. It is even more advantageous if at least one of the softening point, melting point, or bondable temperature of the sealant (which is at least one of the first sealant or the second sealant) is equal to or lower than 300° C.

[0072] In addition, the organic solvent to be mixed with the Cu-ZSM-5 type zeolite having a crystal size equal to or greater than 400 nm more preferably includes at least one selected from the group consisting of cyclooctane, cycloheptane, dimethylquinoline, α-pinene, β-pinene, pinane, α-pinene oxide, pinethoxyl, caryophyllene, verbenone, isobornylcyclohexanol, α-terpineol, β-terpineol, γ-terpineol, menthol, myrtenal, myrtenol, benzyl benzoate, dihydroterpineol, and dihydroterpineol acetate. In addition, if the processing temperature of the glass panel unit (multi-plate glass unit) is equal to or lower than 350° C. (at which the solvent is less likely to desorb from the zeolite), this advantage will be particularly significantly achieved. That is, if at least one of the softening point, melting point, or bondable temperature of the sealant (which is at least one of the first sealant or the second sealant) is equal to or lower than 350° C., this is more advantageous. It is even more advantageous if the sealant (which is at least one of the first sealant or the second sealant) has at least one of a softening point, a melting point or a bondable temperature equal to or below 300°C.

[0073] In addition, the organic solvent to be mixed with the Cu-ZSM-5 type zeolite having a crystal size equal to or greater than 600 nm more preferably includes at least one selected from the following: cyclooctane, cycloheptane, dimethylquinoline, α-pinene, β-pinene, pinane, α-pinene oxide, pinethoxyl, caryophyllene, verbenone, isobornyl cyclohexanol, α-terpineol, β-terpineol, γ-terpineol, menthol, myrtenal, myrtenol, benzyl benzoate, dihydroterpineol and dihydroterpineol acetate. In addition, if the processing temperature of the glass panel unit is equal to or lower than 350° C. (at which temperature the solvent is less likely to desorb from the zeolite), this advantage will be particularly significantly achieved. That is, if at least one of the softening point, melting point or bondable temperature of the sealant (which is at least one of the first sealant or the second sealant) is equal to or lower than 350° C., this is more advantageous. It is even more advantageous if the sealant (which is at least one of the first sealant or the second sealant) has at least one of a softening point, a melting point or a bondable temperature equal to or below 300°C.

[0074] In addition, the organic solvent to be mixed with the Cu-ZSM-5 type zeolite having a crystal size equal to or greater than 750 nm preferably includes at least one selected from the group consisting of cyclooctane, cycloheptane, dimethylquinoline, α-pinene, β-pinene, pinane, α-pinene oxide, pinethoxylated carvol, caryophyllene, verbenone, isobornyl cyclohexanol, α-terpineol, β-terpineol, γ-terpineol, menthol, myrtenal, myrtenol, benzyl benzoate, dihydroterpineol, and dihydroterpineol acetate. In addition, if the processing temperature of the glass panel unit is equal to or lower than 350° C. (at which the solvent is less likely to desorb from the zeolite), this advantage will be particularly significantly achieved. That is, if at least one of the softening point, melting point, or bondable temperature of the sealant (which is at least one of the first sealant or the second sealant) is equal to or lower than 350° C., this is more advantageous. It is even more advantageous if the sealant (which is at least one of the first sealant or the second sealant) has at least one of a softening point, a melting point or a bondable temperature equal to or below 300°C.

[0075] In addition, preferably, the solvent of the getter material composition includes an organic solvent having a boiling point equal to or lower than 300° C. This makes it easier to remove the organic solvent from the getter material composition and form the gas adsorbent 60 even at a low temperature.

[0076] It can be seen that advantageously, at least one of the softening point, melting point or bonding temperature of the sealant is equal to or lower than 300°C, and the crystal size of the zeolite is equal to or greater than 200nm. The crystal size of the zeolite is more preferably equal to or greater than 300nm, even more preferably equal to or greater than 400nm, particularly preferably equal to or greater than 400nm, more particularly preferably equal to or greater than 500nm, and still more preferably equal to or greater than 600nm. Even better, the crystal size of the zeolite is equal to or greater than 750nm, equal to or greater than 1000nm, equal to or greater than 1500nm, or equal to or greater than 2000nm.

[0077] The getter material can include not only a plurality of particles of zeolite crystals, but also a plurality of particles of carbon dioxide adsorbents. In this case, a composite getter material with excellent carbon dioxide adsorption performance can be obtained. Examples of such carbon dioxide adsorbent particles include aluminum oxide (such as γ-Al2O3), zinc oxide, silicon dioxide, titanium dioxide, platinum group elements (such as platinum), lithium silicate, activated carbon, calcium oxide, calcium hydroxide, magnesium oxide, magnesium hydroxide, sodium hydroxide, yttrium oxide, metal coordination compounds (such as cobalt coordination compounds) and cerium compounds (such as cerium dioxide and cerium hydroxide). The particles made of any one of these carbon dioxide adsorbents act as CO2 adsorbents. This allows the CO2 released from the organic solvent to be adsorbed into the carbon dioxide adsorbent, thereby reducing the possibility of carbon dioxide being adsorbed into the zeolite particles. This can reduce the possibility that the function of the particles of the zeolite crystals is disturbed by carbon dioxide. In addition, similar advantages will be achieved by such an absorbent material: in which zeolite particles that have been ion-exchanged with a metal (such as Ba, Sr, Pt, Pd or Ru) and have a higher carbon dioxide adsorption performance than Cu-ZSM-5 and are different from Cu-ZSM-5, or particles with a crystal structure different from Cu-ZSM-5 (such as zeolite 13X particles or A-type zeolite particles) are mixed with Cu-ZSM-5.

[0078] In addition, it is also preferred that the getter material contains a hydrogenation catalyst. A hydrogenation catalyst is a catalyst that initiates a hydrogenation reaction. As used herein, "hydrogenation reaction" refers to a reaction in which hydrogen atoms are added to multiple bond sites (such as carbon-carbon bonds) of a compound (such as a hydrocarbon) such as an organic solvent using hydrogen as a reducing agent. Such a reaction is easily produced when a compound and a metal catalyst are in contact with each other.

[0079] In this embodiment, the hydrogenation catalyst may be a commonly known hydrogenation catalyst, examples of which include platinum group elements (such as ruthenium, rhodium, platinum and palladium); metals such as nickel, cobalt, molybdenum, tungsten, iron, copper, titanium, zirconium and aluminum; or compounds thereof (such as oxides). Adding any of these to the getter material makes it possible to promote the vaporization of the organic solvent so that the organic solvent can be easily removed in the sealing step, and decompose the hydrocarbons into H2, CO2, H2O or any other hydrocarbons with a higher reactivity. This allows the decomposed molecules to be removed by vaporization or adsorption into the getter material. In particular, when the getter material and the organic solvent are mixed, this makes it easier to remove unnecessary hydrocarbons, thereby achieving significant advantages. Optionally, the hydrogenation catalyst may also be supported by another substance or added to another substance. Alternatively, a metal powder (such as a platinum group element, such as platinum black or palladium black) may be mixed into a metal porous body or powder having a size equal to or less than one micron.

[0080] It should be noted that the catalyst support on which the hydrogenation catalyst is supported is preferably a porous body. The specific surface area of ​​the porous body is preferably equal to or greater than 20 m 2 / g, and the specific surface area is more preferably equal to or greater than 50m 2 / g. Alternatively, the porous body can also be supported by the above-mentioned carbon dioxide adsorbent. However, if copper ion exchange zeolite is used as zeolite, the copper ion exchange zeolite has the property of being activated by reducing copper in a vacuum and showing strong adsorption capacity. In this case, it is preferred to use a carbon dioxide adsorbent other than cerium dioxide. Even when cerium dioxide is used, significant advantages will be achieved. Meanwhile, if a substance with oxygen storage properties (such as cerium dioxide or cerium-zirconium solid solution) is mixed with copper ion exchange zeolite, the oxygen released from cerium dioxide or cerium-zirconium solid solution will inhibit the activation of copper ion exchange zeolite, and sometimes cause the decline of its performance. In addition, cerium will react with the silicon dioxide part of zeolite to cause the deterioration of copper ion exchange zeolite. In addition, from the perspective of production cost and stability, it is preferred to minimize the use of cerium as one of the precious rare earth metals. For these reasons, the catalyst carrier of the hydrogenation catalyst is particularly preferably selected from at least one of aluminum oxide, silicon dioxide, activated carbon and barium sulfate. In addition, the catalyst carrier of the hydrogenation catalyst is particularly preferably an Al compound (such as aluminum oxide) or a Si compound (such as silicon dioxide), because these compounds have the same metal component as the zeolite. In addition, the average particle size of the catalyst carrier of the hydrogenation catalyst is preferably equal to or greater than 1nm and equal to or less than 50μm. It should be noted that the average particle size of the catalyst carrier of the hydrogenation catalyst can be verified by observing via SEM. In addition, from the perspective of the use efficiency of the hydrogenation catalyst, the mass ratio of the hydrogenation catalyst to the catalyst carrier is preferably equal to or greater than 0.01% by weight and equal to or less than 30% by weight.

[0081] The catalyst carrier on which the hydrogenation catalyst is supported can be at least one porous material selected from, for example, aluminum oxide, silicon dioxide, activated carbon, barium sulfate, calcium carbonate, silicon carbide, titanium dioxide and zirconium oxide. In addition, porous aluminum oxide is particularly preferred because porous aluminum oxide itself has carbon dioxide adsorption capacity. If the hydrogenation catalyst is supported on ceria, or if ceria is mixed with a getter material as a carbon dioxide adsorbent, the content of ceria is preferably at most 30% by weight of the entire getter material. The content of ceria is more preferably equal to or less than 15% by weight, even more preferably equal to or less than 5% by weight, and particularly preferably equal to or less than 1% by weight.

[0082] Examples of preferred combinations of hydrogenation catalysts and catalyst supports include Ru / Al2O3, Rh / Al2O3, Pt / Al2O3, Pd / Al2O3, Ir / Al2O3, Os / Al2O3, Au / Al2O3, Ni / Al2O3, Co / Al2O3, Mo / Al2O3, W / Al2O3, Fe / Al2O3, Cu / Al2O3, Ti / Al2O3, Zr / Al2O3, Al / Al2O3, Ru / SiO2, Rh / SiO2, Pt / SiO2 ... C represents activated carbon. It should be noted that each of the combinations listed above is represented by A / B: hydrogenation catalyst / catalyst support.

[0083] In addition, if a substance (including a platinum group element, gold or a compound thereof) is supported on porous cerium (such as alumina or silica) (such as Ru / Al2O3, Rh / Al2O3, Pt / Al2O3, Pd / Al2O3, Au / Al2O3, Ru / SiO2, Rh / SiO2, Pt / SiO2, Pd / SiO2 or Au / SiO2) as a combination of a hydrogenation catalyst and a catalyst carrier, then when the combination of the hydrogenation catalyst and the catalyst carrier is used together with a copper ion-exchanged zeolite, oxidation and reduction will be caused with a high degree of stability and will exhibit particularly good properties.

[0084] On the other hand, the activation of copper ion exchange type zeolite is inhibited by a catalyst (such as silver or silver oxide) which is oxidized in air at a temperature equal to or lower than 350° C. and reduced in a vacuum at a temperature equal to or lower than 350° C. to release a large amount of oxygen. Therefore, it is preferred to avoid mixing a substance having such a property with copper ion exchange type zeolite as much as possible. For example, the content of a substance having such a property is preferably less than 5% by weight at most, more preferably equal to or lower than 1% by weight, and even more preferably equal to or lower than 0.1% by weight, relative to the entire getter material.

[0085] The hydrogenation catalyst supported on the catalyst carrier is preferably a powder having a particle size smaller than that of the zeolite particles or the carbon dioxide adsorbent particles. Examples of hydrogenation catalyst powders include ruthenium 5 wt%-alumina powder (product code JAN4987481323469), platinum 5 wt%-alumina powder (product code JAN4987481317161) and palladium 5 wt%-alumina powder (product code JAN4987481317109), all of which are manufactured by FUJIFILM Wako PureChemical Corporation; and 5 wt% Pd alumina powder (ID code: AA-2501), 5 wt% Pd barium sulfate (ID code: OP-2505), palladium black (BL-2901), 5 wt% Pt alumina powder (ID code: AA-1501), platinum black (ID code: BL-1901) and 5 wt% Ru alumina powder (ID code: AA-4501), all of which are manufactured by NEChemcat Corporation.

[0086] Next, a specific example will be described. A getter material composition was prepared by mixing 10 wt% of a hydrogenation catalyst powder with 90 wt% of a Cu-ZSM-5 powder having a crystal size of 400 nm and using α-terpineol as a solvent. Using this getter material composition, a glass panel unit was prepared as a prototype. Therefore, the thermal conductivity of the getter material composition consisting only of Cu-ZSM-5 was 12 W / m 2 On the other hand, when a getter material composition was prepared by mixing 5 wt% of ruthenium, 10 wt% of alumina powder, and 90 wt% of Cu-ZSM-5 powder having a crystal size of 400 nm and using α-terpineol as a solvent, the thermal conductivity was 0.87 W / m 2 K.

[0087] Meanwhile, when a getter material composition was prepared by mixing 5 wt % of platinum, 10 wt % of alumina powder, and 90 wt % of Cu-ZSM-5 powder having a crystal size of 400 nm and using α-terpineol as a solvent, the thermal conductivity was 0.78 W / m2 K. In addition, when a getter material composition was prepared by mixing 5 wt% of palladium, 10 wt% of alumina powder, and 90 wt% of Cu-ZSM-5 powder having a crystal size of 400 nm and using α-terpineol as a solvent, the thermal conductivity was 0.76 W / m 2 K. In addition, the thermal conductivity of the following glass panel is 2W / m 2 K: In the glass panel, a getter material was prepared by mixing 10 wt% of alumina powder containing no hydrogenation catalyst and 90 wt% of Cu-ZSM-5 powder having a crystal size of 400 nm. When the gas retained in the glass panel using the getter material mixed with alumina containing no hydrogenation catalyst was analyzed, a lot of hydrocarbon-based gases were detected.

[0088] In addition, the thermal conductivity of the following glass panel is 2.6W / m 2 K: In the glass panel, the getter material was prepared by mixing 10 wt% of cerium oxide without a hydrogenation catalyst and 90 wt% of Cu-ZSM-5 powder having a crystal size of 400 nm. The experiment was conducted in the same manner by using a mixture of 50 wt% of α-terpineol having a boiling point of 219°C and 50 wt% of a high boiling point solvent (β-caryophyllene) having a boiling point of 260°C as a solvent. In this case, when 5 wt% of ruthenium-alumina powder was used, the thermal conductivity was 2.3 W / m 2 When 5 wt% of platinum-alumina powder is used, the thermal conductivity is 0.78 W / m 2 When 5 wt% of palladium-alumina powder is used, the thermal conductivity is 0.76 W / m 2 K. When alumina powder without hydrogenation catalyst was used, the thermal conductivity was 8.3 W / m 2 K. It can be seen that when the solvent contains a high-boiling-point solvent having a boiling point of 250° C. or higher, a more significant difference can be recognized depending on whether a hydrogenation catalyst is contained or not.

[0089] In addition, in the case where the hydrogenation catalyst contains a platinum group element (such as ruthenium, palladium or platinum), even when a high boiling point solvent having a boiling point of 250° C. or higher is used, relatively good thermal conductivity can be maintained. In addition, for palladium and platinum, the thermal conductivity hardly changes depending on whether such a high boiling point solvent having a boiling point of 250° C. or higher is used. This is why a hydrogenation catalyst such as a platinum group element will produce a particularly beneficial effect when the solvent contains a component that is hardly vaporizable (such as a high boiling point solvent or resin component having a boiling point of 250° C. or higher). In addition, if such a high boiling point solvent or resin component having a boiling point of 250° C. or higher is mixed with the solvent, palladium or platinum will produce a more beneficial effect. On the other hand, in a getter material not containing a platinum group element, the solvent to be mixed with the getter material more preferably includes a solvent having a boiling point lower than 250° C. as a main component (preferably including more than 50% by weight of such a solvent).

[0090] It should be noted that these thermal conductivity values ​​are comparative values ​​assuming that the total amount of each getter material powder is constant. This is why carbon dioxide adsorbents (such as alumina) adsorb carbon dioxide released due to the decomposition of organic solvents (especially when the getter material is mixed with an organic solvent), thereby achieving the advantage of keeping the internal pressure of the glass panel low. In addition, the hydrogenation catalyst can also promote the vaporization of the organic solvent so that it can be more easily removed by the sealing step, and can decompose the hydrocarbon-based gas generated when the organic solvent becomes a gas so that the hydrocarbon-based gas is adsorbed to the zeolite, carbon dioxide adsorbent or the hydrogenation catalyst itself. Therefore, the hydrogenation catalyst achieves the advantage of reducing the increase in the internal pressure of the glass panel.

[0091] In addition, when using a high boiling point solvent or a resin component, rather than using a low boiling point solvent, these advantages of the hydrogenation catalyst tend to be more significantly realized. The organic solvent with a ring structure has a relatively large molecular weight, and therefore tends to have a high boiling point. Therefore, by mixing the organic solvent with a ring structure, zeolite and the hydrogenation catalyst to prepare the getter material composition, the organic solvent can be properly removed after application, while minimizing the damage to the zeolite caused by the organic solvent. When the crystal size of the zeolite is equal to or greater than 200nm, this trend is more clearly observed. The crystal size of the zeolite is preferably equal to or greater than 300nm, more preferably equal to or greater than 400nm, even more preferably equal to or greater than 500nm, particularly preferably equal to or greater than 600nm.

[0092] In addition, the crystal size (particle size) of the zeolite is more preferably equal to or greater than 750nm, even more preferably equal to or greater than 1000nm, particularly preferably equal to or greater than 1500nm or equal to or greater than 2000nm. It should be noted that such a high boiling point solvent or resin component having a boiling point equal to or greater than 250°C generally has a high viscosity. Therefore, mixing such a high boiling point solvent or resin component enables the sedimentation of the getter material composition to be more effectively reduced and the stability of application to be increased. Examples of such high boiling point solvents include β-caryophyllene, benzyl benzoate and isobornyl cyclohexanol. Examples of such resin components include polycarbonate, acrylic resin, polyester, polyurethane and phenolic resin. That is, any one of the solvents and resin binders commonly used for purposes such as screen printing can be used. At least one of these solvents and resin components can be used.

[0093] As can be seen from the foregoing description, the combined use of zeolite, carbon dioxide adsorbent and hydrogenation catalyst enables the provision of high-performance getter material compositions and getter materials even when these materials are mixed with organic solvents, while suppressing the decline in performance. At the same time, since carbon dioxide adsorbents and hydrogenation catalysts are not suitable for adsorbing nitrogen, in particular, zeolite is preferably a copper ion exchange type zeolite, more preferably a ZSM-5 type zeolite. It should be noted that, for example, even when only zeolite and carbon dioxide adsorbent are used in combination or when only zeolite and hydrogenation catalyst are used in combination, the same advantages will be achieved to a certain extent. In addition, it is effective to use zeolite, carbon dioxide adsorbent and hydrogenation catalyst in combination to adsorb hydrocarbon-based gases and carbon dioxide released from sealants, glass substrates, columns and other components.

[0094] In this embodiment, the getter material may consist exclusively of zeolite particles. In this case, 100% by weight of the particles forming the getter material are zeolite particles.

[0095] Alternatively, in this embodiment, the getter material may also be a mixture of zeolite particles and carbon dioxide adsorbent particles. In this case, the getter material preferably contains zeolite particles and carbon dioxide adsorbent particles in a weight ratio of 1 (zeolite particles) to 0.01-0.99 (carbon dioxide adsorbent particles).

[0096] Alternatively, in this embodiment, the getter material may also be a mixture of zeolite particles and hydrogenation catalyst powder. In this case, the getter material preferably contains zeolite particles and hydrogenation catalyst powder in a weight ratio of 1 (zeolite particles) to 0.0001-0.3 (hydrogenation catalyst powder).

[0097] Alternatively, in this embodiment, the getter material may also be a mixture of zeolite particles, carbon dioxide adsorbent particles and hydrogenation catalyst powder. In this case, the getter material preferably contains zeolite particles, carbon dioxide adsorbent particles and hydrogenation catalyst powder in a weight ratio of 1 (zeolite particles) to 0.01-0.99 (carbon dioxide adsorbent particles) to 0.0001-0.3 (hydrogenation catalyst powder).

[0098] Furthermore, in this embodiment, the getter material composition preferably contains a getter material and a solvent in a predetermined ratio. For example, the getter material composition preferably contains a getter material and a solvent in a weight ratio of 1 (getter material) to 0.1-100 (solvent).

[0099] In addition, in this embodiment, the getter material composition preferably contains a getter material, a solvent and a resin component in a predetermined ratio. For example, the getter material composition preferably contains a getter material, a solvent and a resin component in a weight ratio of 1 (getter material) to 0.1-100 (solvent) to 0.01-2 (resin component).

[0100] Furthermore, in this embodiment, the getter material composition preferably contains a getter material, a solvent having a boiling point lower than 250° C., and a high boiling point solvent having a boiling point equal to or higher than 250° C. in predetermined ratios. For example, the getter material composition preferably contains a getter material, a solvent having a boiling point lower than 250° C., and a high boiling point solvent having a boiling point equal to or higher than 250° C. in a weight ratio of 1 (getter material) to 0.1-100 (solvent having a boiling point lower than 250° C.) to 0.01-2 (high boiling point solvent having a boiling point equal to or higher than 250° C.).

[0101] The following is an overview of the advantages to be achieved by the hydrogenation catalysts added to getter materials and getter material compositions.

[0102] For example, in order to form a getter material in a narrow gap of an evacuated glass panel unit (multi-plate glass unit), it is preferred to mix the getter material with a solvent and apply the mixture to a glass substrate. At this time, any application method such as dispensing, screen printing, slit coating, spray coating or spin coating can be used as appropriate.

[0103] Advantages to be achieved by applying a mixture of a getter material powder and a solvent include: (1) enabling the formation of a thin film (e.g., to a thickness less than that of a sealant); (2) allowing the getter material powder to aggregate when drying and enabling a reduction in apparent volume compared to applying the getter material powder directly to a glass substrate; (3) increasing the degree of freedom in the shape of a glass substrate to be mass-produced; and (4) eliminating the need to use a member to fix the getter material because the getter material electrostatically adheres to the substrate when drying.

[0104] On the other hand, the disadvantages brought about include: (1) failure in applying the getter material composition because the use of a solvent with a low boiling point causes the solvent to dry out during the storage or application step of the getter material composition; (2) inability to maintain sufficient stability during application because the getter material powder will settle unless a solvent with a relatively high viscosity is used; (3) once the solvent molecules are adsorbed into the getter material, especially when a high-viscosity solvent, which generally has a high boiling point, is mixed with a getter material having the property of adsorbing gas, a great deal of energy is required to desorb the solvent molecules; (4) unless the solvent is sufficiently desorbed after application, a significant reduction in the adsorption performance of the getter material is caused (and further causes the solvent molecules to be released from the getter material in the form of gas, and conversely may cause an increase in the amount of gas retained in the glass panel unit).

[0105] That is, the use of a solvent with a high boiling point to achieve a solution to be applied with stability makes it difficult to fully desorb the solvent, resulting in a decrease in the adsorption performance of the getter material, which is a problem. In particular, the lower the processing temperature of the glass panel unit, the more difficult it is to fully desorb the solvent after the getter material composition has been applied, and the more likely it is to cause performance degradation. In addition, for example, even if a certain organic solvent is heated to its boiling point, the solvent will not actually be completely vaporized. In particular, when an organic solvent is mixed with Cu-ZSM-5, the solvent molecules will not be completely desorbed unless the solvent is heated to a temperature 100-150°C higher than the boiling point. A few organic solvents can be completely vaporized at a temperature equal to or lower than 350°C. This is why this is a serious problem, especially when the processing temperature is equal to or lower than 350°C, or when the softening point or melting point of the sealant (which is at least one of the first sealant or the second sealant) is equal to or lower than 350°C.

[0106] The applied getter material composition undergoes: (A) desorption of its organic solvent when the getter material composition is heated in a drying step or a subsequent sealing step (e.g., a first melting step); (B) activation of its getter material when the getter material composition is heated in a vacuum; and (C) release of (most of) carbon dioxide, nitrogen, methane, and other gases from the interior of the component 100 that has been separated from the vacuum pump, and adsorption of those gases into the getter material (e.g., after the second melting step). Copper ion-exchanged zeolite is allowed to achieve its advantages in stage (A) and stage (C) by mixing a hydrogenation catalyst with the copper ion-exchanged zeolite.

[0107] First, in stage (A), hydrogenation catalyst vaporizes organic solvent by promoting the decomposition and reaction of organic solvent, thereby reducing the possibility that organic solvent is retained in copper ion exchange type zeolite and causes its performance degradation. In addition, in stage (C), hydrogenation catalyst (for example, particularly platinum group element catalyst) also acts as a strong carbon dioxide adsorbent with chemical adsorption properties or a gas adsorbent based on hydrocarbon. Therefore, it is possible to prevent the adsorption site (which can also adsorb nitrogen and methane gas) of copper ion exchange type zeolite from being occupied by carbon dioxide, and therefore compared with the situation that only copper ion exchange type zeolite or only hydrogenation catalyst is used as a getter material, the getter material in the form of a mixture of copper ion exchange type zeolite and hydrogenation catalyst can not only adsorb more carbon dioxide but also adsorb more nitrogen and methane gas, thereby ultimately enabling the residual gas pressure of the glass panel unit to be kept sufficiently low.

[0108] This advantage will be even more significantly achieved when the processing temperature is equal to or lower than 350°C (i.e., under conditions that make it difficult to desorb the organic solvent and fully activate the copper ion exchange zeolite). That is, when the softening point or melting point of the sealant (which is at least one of the first sealant or the second sealant) is equal to or lower than 350°C, this advantage becomes even more significant. At the same time, when combined with Cu-ZSM-5, the organic solvent preferably includes a cyclic compound. However, in general, cyclic compounds generally have a high boiling point. The combined use of Cu-ZSM-5, a solvent (including an organic solvent) and a hydrogenation catalyst enables the provision of an inhaler material composition that not only exhibits sufficient adsorption performance but also exhibits good stability when applied.

[0109] By using Cu-ZSM-5, solvent (including organic solvent) and hydrogenation catalyst in combination, it is possible to provide a getter material composition that not only shows enough adsorption properties but also shows good stability when applied. When combined with Cu-ZSM-5, the organic solvent preferably includes a cyclic compound. However, in general, cyclic compounds usually have a high boiling point. Using cyclic compounds as organic solvents reduces the possibility that organic solvents enter the inside of Cu-ZSM-5, thereby allowing hydrogenation catalysts to react more smoothly with organic solvents, and making it easier to achieve the advantages of hydrogenation catalysts. In addition, making the crystal size of Cu-ZSM-5 equal to or greater than 400nm, more preferably equal to or greater than 600nm, even more preferably 750nm enables to provide a getter material composition that shows even better adsorption properties in a low pressure range by further reducing the deterioration that would otherwise be caused by organic solvents. Furthermore, mixing Cu-ZSM-5 with a hydrogenation catalyst and an organic solvent (including a cyclic compound) makes it possible to reduce the proportion of the organic solvent inside the Cu-ZSM-5 crystals and promote the reaction between the organic solvent and the hydrogenation catalyst, thereby making it easier and even more efficient to desorb the solvent.

[0110] An exemplary getter material may include 51 wt% to 99 wt% of a copper ion exchange type zeolite having a crystal size of 400 nm or more and 5000 nm or less and 1 wt% to 49 wt% of a porous powder having a hydrogenation catalyst supported thereon (and wherein the weight ratio of the hydrogenation catalyst to the entire porous powder is 0.1 wt% or more and 20 wt% or less). The getter material more preferably includes 51 wt% to 99 wt% of Cu-ZSM-5 having a crystal size of 400 nm or more and 5000 nm or less and 1 wt% to 49 wt% of a porous powder having a hydrogenation catalyst supported thereon (and wherein the weight ratio of the hydrogenation catalyst to the entire porous powder is 0.1 wt% or more and 20 wt% or less). Alternatively, the getter material may contain 51 to 99 wt % of a copper ion exchange type zeolite having a crystal size of 400 nm or more and 5000 nm or less and 1 to 49 wt % of a hydrogenation catalyst powder.

[0111] In addition, the exemplary getter material composition may include 20 wt % to 60 wt % of a copper ion exchange type zeolite having a crystal size of 400 nm or more and 5000 nm or less, 0.5 wt % to 40 wt % of a porous powder on which a hydrogenation catalyst is supported (and wherein the weight ratio of the hydrogenation catalyst to the entire porous powder is equal to or greater than 0.1 wt % and equal to or less than 20 wt %), and 30 wt % to 95 wt % of an organic solvent. The getter material composition more preferably includes 20 wt % to 60 wt % of Cu-ZSM-5 having a crystal size of 400 nm or more and 5000 nm or less, 0.5 wt % to 40 wt % of a porous powder on which a hydrogenation catalyst is supported (and wherein the weight ratio of the hydrogenation catalyst to the entire porous powder is equal to or greater than 0.1 wt % and equal to or less than 20 wt %), and 30 wt % to 95 wt % of an organic solvent whose main component is a cyclic compound (in this case, 50 wt % or more of the organic solvent is a cyclic compound). Alternatively, the getter material composition may contain 20 to 60 wt % of a copper ion exchange type zeolite having a crystal size of 400 nm or more and 5000 nm or less, 0.1 to 40 wt % of a hydrogenation catalyst powder, and 30 to 95 wt % of an organic solvent.

[0112] After the mixing step, an assembly step is performed.

[0113] The assembling step is a step of preparing the assembly 100 .

[0114] like Figure 1 A and Figure 1 As shown in FIG. 1B , the assembly 100 includes a first glass plate 200, a second glass plate 300, a peripheral wall 410, and a partition 420. The assembly 100 also has an inner space 500 surrounded by the first glass plate 200, the second glass plate 300, and the peripheral wall 410. The assembly 100 also includes a gas adsorbent 60 and a plurality of columns (spacers) 70 in the inner space 500. The assembly 100 also has an exhaust port 700.

[0115] The first glass plate (first glass substrate) 200 is a member forming the basis of the first glass plate 20 to be described later, and is made of the same material as the first glass plate 20. The second glass plate (second glass substrate) 300 is a member forming the basis of the second glass plate 30 to be described later, and is made of the same material as the second glass plate 30. The first glass plate 200 and the second glass plate 300 have the same planar shape. In this embodiment, the size of the first glass plate 200 is large enough to form at least one first glass plate 20 to be described later, and the size of the second glass plate 300 is large enough to form at least one second glass plate 30 to be described later.

[0116] The first glass plate 200 and the second glass plate 300 each have a polygonal flat plate shape (eg, a rectangular shape in this embodiment).

[0117] The first glass plate 200 includes a body 210 and a low-emissivity film 220 .

[0118] The low emissivity film 220 is disposed in the internal space 500 and covers the main body 210. The low emissivity film 220 is in contact with the main body 210. The low emissivity film 220 is also called an "infrared reflective film" and has a light-transmitting property but reflects infrared rays. Therefore, the low emissivity film 220 can improve the thermal insulation properties of the glass panel unit 10. For example, the low emissivity film 220 can be a thin metal film. For example, the low emissivity film 220 can contain silver. For example, the low emissivity film 220 can be a Low-E film.

[0119] The first glass plate 200 includes a main body 210 as described above. The main body 210 has a first surface 211 and a second surface 212. The first surface 211 is a flat surface and is covered with a low emissivity film 220. The second surface 212 is a flat surface parallel to the first surface 211 and is positioned opposite to the internal space 500 along the direction D1. The main body 210 defines the main shape of the first glass plate 200 and thus has a rectangular flat plate shape. Examples of the material of the main body 210 include soda-lime glass, high strain point glass, chemically strengthened glass, alkali-free glass, quartz glass, microcrystalline glass (neoselam) and heat-strengthened glass. The thickness of the first glass plate 200 may be 0.1 mm to 20 mm.

[0120] The second glass plate 300 includes a body 310. The body 310 has a first surface 311 and a second surface 312. The first surface 311 is a flat surface facing the low emissivity film 220. The second surface 312 is a flat surface parallel to the first surface 311 and is located opposite to the internal space 500 along the direction D1. The body 310 defines the main shape of the second glass plate 300 and thus has a rectangular flat plate shape. The body 310 has the same shape as the body 210. In this embodiment, the second glass plate 300 consists only of the body 310. Optionally, the second glass plate 300 may include not only the body 310 but also a low emissivity film corresponding to the low emissivity film 220. If the second glass plate 300 includes a low emissivity film, the low emissivity film covers the body 310 in the internal space 500 and is in contact with the body 310. Examples of the material of the body 310 include soda-lime glass, high strain point glass, chemically strengthened glass, alkali-free glass, quartz glass, microcrystalline glass, and heat-strengthened glass. The second glass plate 300 may have a thickness of 0.1 mm to 20 mm.

[0121] The peripheral wall 410 contains a first sealant (ie, a first hot melt adhesive). The peripheral wall 410 is disposed between the first glass plate 200 and the second glass plate 300. The peripheral wall 410 has a Figure 1 A. In particular, the peripheral wall 410 has a rectangular frame shape. The peripheral wall 410 is formed along the outer periphery of each of the first glass plate 200 and the second glass plate 300. Therefore, in the assembly 100, the internal space 500 is created to be surrounded by the peripheral wall 410, the first glass plate 200 and the second glass plate 300.

[0122] For example, the first hot melt adhesive may include glass frit. For example, the glass frit may be a low melting point glass frit. Examples of low melting point glass frit include bismuth-based glass frit, lead-based glass frit and vanadium-based glass frit. In this embodiment, the first hot melt adhesive is configured as vanadium-based glass frit. The first hot melt adhesive is not necessarily glass frit, but may also be, for example, a low melting point metal or a hot melt adhesive. Optionally, the first hot melt adhesive may also contain an organic binder or an organic solvent or both an organic binder and an organic solvent. In this case, even if the gas derived from the organic binder and / or the organic solvent is released into the evacuated space 50 after the sealing step (the second melting step), the gas may also be adsorbed into the gas adsorbent 60, thereby reducing the possibility that the gas is retained in the evacuated space 50.

[0123] For example, the organic binder may include a resin. Examples of resins include poly(isobutyl methacrylate), ethyl cellulose, aliphatic polycarbonate, acrylic resins, and butyral resins. The organic binder need not be one of these resins, but may also include any component. In any case, the resin constituting the organic binder is preferably a resin with a low molecular weight and that can be easily decomposed.

[0124] Examples of organic solvents include esters such as butyl carbitol acetate and ethyl carbitol acetate. However, the organic solvent is not necessarily one of these components, but may also include at least one selected from solvents used for general screen printing such as terpene-based solvents and solvents for dispensing applications.

[0125] If the peripheral wall 410 also contains resin, even the gas derived from the resin and released into the internal space 500 after the assembling step will be exhausted in the exhaust step. In addition, even if the gas derived from the resin remains as residual gas in the evacuated space 50 after the exhaust step, the residual gas can be adsorbed into the gas adsorbent 60.

[0126] The partition 420 is placed in the internal space 500. The partition 420 partitions the internal space 500 into a first space 510 and a second space (ventilation space) 520. Therefore, the first space 510 is a space from which gas is exhausted in the exhaust step. The second space 520 is a space for exhausting gas from the first space 510. The partition 420 is disposed closer to the center of the second glass plate 300 than to the center of the second glass plate 300 along the length (i.e., Figure 1 A in the right / left direction) (i.e., Figure 1 A), so that the first space 510 has a larger area than the second space 520. The partition 420 is formed along the width of the second glass plate 300 (ie, Figure 1 A) is provided in the inner space 500. However, neither longitudinal end of the partition 420 contacts the outer peripheral wall 410. In this embodiment, the width of the second glass plate 300 is parallel to the direction D2, and the length of the second glass plate 300 is parallel to the direction D3.

[0127] The partition 420 includes a main body portion (partitioner main body portion) 421 forming its main body and a blocking portion 422. The blocking portion 422 includes a first blocking portion 4221 and a second blocking portion 4222. The main body portion 421 extends linearly along a direction D2. The direction D2 may be aligned with, for example, the width of the second glass plate 300. In addition, along the D2 direction, both ends of the main body portion 421 are not in contact with the peripheral wall 410. The first blocking portion 4221 is formed to extend from one of the two ends of the main body portion 421 toward the second space 520, and the second blocking portion 4222 is formed to extend from the other end of the main body portion 421 toward the second space 520. One end of the main body portion 421 may be a first end, and the other end thereof may be a second end.

[0128] The partition 420 contains a second sealant (second hot melt adhesive). For example, the second hot melt adhesive can be glass frit. For example, the glass frit can be a low melting point glass frit. Examples of low melting point glass frits include bismuth-based glass frits, lead-based glass frits, and vanadium-based glass frits. In this embodiment, the second hot melt adhesive is configured as vanadium-based glass frit. The second hot melt adhesive does not have to be glass frit, but can also be, for example, a low melting point metal or a hot melt adhesive. In this embodiment, the same type of adhesive is used as the first hot melt adhesive and the second hot melt adhesive. That is, the first sealant and the second sealant are the same material.

[0129] like Figure 1As shown in FIG. 1A , the air passage 600 allows the first space 510 and the second space 520 to communicate with each other in the internal space 500. The air passage 600 includes the first air passage 610 and the second air passage 620. The first air passage 610 is a first end portion of the partition 420 (ie, Figure 1 The second air passage 620 is a gap between the second end of the partition 420 (i.e., the upper end of the partition 420) and the outer peripheral wall 410. Figure 1 A gap between the lower end portion in FIG. 4 and the outer peripheral wall 410.

[0130] The exhaust port 700 is a hole that allows the second space 520 to communicate with the external environment. The exhaust port 700 is used to discharge the gas from the first space 510 through the second space 520 and the air channel 600 (i.e., the first air channel 610 and the second air channel 620). Therefore, the air channel 600, the second space 520 and the exhaust port 700 together form an exhaust path for discharging the gas from the first space 510. The exhaust port 700 is provided to pass through the second glass plate 300 to allow the second space 520 to communicate with the external environment. Specifically, the exhaust port 700 is provided at a corner portion of the second glass plate 300.

[0131] The gas adsorbent 60 and the plurality of spacers 70 are arranged in the first space 510. In particular, the gas adsorbent 60 is formed along the width of the second glass plate 300 so as to be adjacent to the second end portion (ie, Figure 1 A). That is, the gas adsorbent 60 is placed at the end of the first space 510 (the evacuated space 50). This makes the gas adsorbent 60 less noticeable. In addition, the gas adsorbent 60 is positioned away from the partition 420 and the air passage 600. This reduces the possibility that the gas adsorbent 60 interferes with the exhaust of gas from the first space 510.

[0132] The assembling step is a step of forming the first glass plate 200, the second glass plate 300, the peripheral wall 410, the partition 420, the internal space 500, the air passage 600, the exhaust port 700, the gas adsorbent 60 and the plurality of spacers 70 to obtain the assembly 100. The assembling step includes the following first to sixth steps. Optionally, the order of performing the second to fifth steps may be changed as appropriate.

[0133] The first step is a step of forming the first glass plate 200 and the second glass plate 300 (ie, a substrate forming step). For example, the first step includes preparing the first glass plate 200 and the second glass plate 300. If necessary, the first step may also include cleaning the first glass plate 200 and the second glass plate 300.

[0134] The second step is a step of forming the exhaust port 700. The second step includes providing the exhaust port 700 through the second glass plate 300. The second step includes cleaning the second glass plate 300, if necessary.

[0135] The third step is a step of forming the spacer 70 (spacer forming step) (see Figure 3 ). The third step includes pre-forming a plurality of spacers 70 and placing the plurality of spacers 70 at predetermined positions on the second glass plate 300 using a patch mounter or any other tool. When the assembly 100 becomes a semi-finished product 110, the plurality of spacers 70 will be used to maintain a predetermined gap distance between the first glass plate 200 and the second glass plate 300. Examples of constituent materials for such spacers 70 include metal, glass, and resin. The spacers 70 may contain one or more materials selected from these materials.

[0136] In the third step according to this embodiment, as described above, the spacers 70 are pre-formed and placed on the second glass plate 300. Alternatively, a plurality of spacers 70 may also be formed on the second glass plate 300 by a known thin film forming technique. Still alternatively, if the spacers 70 include a resin, the plurality of spacers 70 may also be formed by a combination of a photolithography technique and an etching technique (rather than the above-described forming method). In this case, for example, the plurality of spacers 70 may be made of a photocurable material.

[0137] It should be noted that the size, number, spacing and arrangement pattern of the spacers 70 can be appropriately selected. Each of the spacers 70 has the shape of a cylinder, and its height is approximately equal to the predetermined gap distance. For example, the spacer 70 can have a diameter of 0.5 mm, a height of 100 μm and a spacing of 20 mm therebetween. Optionally, the spacer 70 can also have any other desired shape, such as a rectangular columnar shape or a spherical shape. Alternatively, for example, the spacer 70 can also have a diameter of 0.1 mm to 5 mm, a height of 10 μm to 3000 μm and a spacing of 2 mm to 100 mm therebetween.

[0138] The fourth step is a step of forming the gas adsorbent 60 (gas adsorbent forming step) (see Figure 3 ). The fourth step includes forming the gas adsorbent 60 by applying the getter material composition prepared in the processing step onto the second glass plate 300 using, for example, a dispenser, and then drying the getter material composition thus applied. That is, the fourth step includes a drying step of drying the getter material composition. Drying the getter material composition allows the getter material to restore its gas adsorption property. In addition, applying the getter material composition enables the size of the gas adsorbent 60 to be reduced. This allows the gas adsorbent 60 to be formed even in the narrow first space 510.

[0139] Next, an exemplary getter material composition application step will be described. It should be noted that the application step to be described below is merely an example and should not be construed as limiting.

[0140] First, a hydrogenation catalyst or a porous powder on which a hydrogenation catalyst is supported is prepared. The hydrogenation catalyst powder or the porous powder is preferably pulverized as needed to adjust its particle size to 20 μm or less according to D50. Thereafter, 0.01 to 49 parts by mass of the hydrogenation catalyst or the porous powder on which the hydrogenation catalyst is supported and 50 to 99.99 parts by mass of Cu-ZSM-5 powder having a crystal size of 400 nm or more and 5000 nm or less are mixed with each other, and the mixture thus obtained is used as a getter material.

[0141] Next, 5 to 70 parts by mass of the getter material 5 and 30 to 95 parts by mass of the organic solvent are mixed with each other, and the mixture thus obtained is used as a getter material composition. At this time, the organic solvent preferably includes a cyclic compound. In addition, adding a high boiling point solvent having a boiling point equal to or higher than 250° C. as an organic solvent can reduce the possibility of nozzle clogging (for example, due to drying of the solvent in the application head of the applicator).

[0142] The getter material composition is injected into a syringe (such as a dispenser) and then applied to the outer periphery of the first glass plate or the second glass plate provided with a sealant or a spacer. At this time, the application range is preferably within 15 mm from the edge of the glass substrate. In this case, when the glass panel unit is assembled into the sash, the getter material will be hidden behind the sash. It should be noted that the sealant, the spacer and the getter material composition can be provided to the substrate in any order without limitation. For example, after the spacer has been placed, the getter material composition can be applied, and then the sealant can be formed. Alternatively, the getter material composition, the spacer and the sealant can be provided in this order.

[0143] Next, the glass substrate is subjected to a drying step, whereby the solvent of the getter material composition is partially dried and the powder is adhered to the glass substrate. Thereafter, the first glass substrate and the second glass substrate are placed one on top of the other, and the assembly is subjected to a sealing step to be described later. Alternatively, a sealant may be applied to the first glass plate or the second glass plate, and then the assembly may be subjected to a drying step. Thereafter, a getter material composition may be applied to the first glass plate or the second glass plate, and then the assembly may be subjected to a drying step again. This can prevent the getter material from adsorbing volatile components of the solvent of the sealant and reduce degradation of the getter material. However, higher productivity will be achieved by drying the sealant and the getter material at the same time.

[0144] The first melting step (to be described later) is performed in air. In this processing step, the residual solvent of the getter material composition is desorbed. The hydrogenation catalyst produces the effect of promoting solvent desorption during the first melting step. In addition, the crystal size of Cu-ZSM-5 is set to 400nm or larger, preferably equal to or greater than 600nm, more preferably equal to or greater than 750nm so that the influence of the solvent can be further reduced. In addition, adding a cyclic compound to the solvent makes it possible to further reduce the influence of the solvent. It should be noted that at this time point, the solvent is preferably desorbed from the getter material composition as much as possible. Fully desorbing the solvent component from the getter material composition allows the getter material composition to restore the state of the getter material again. Then, after the first glass substrate and the second glass substrate are combined together in the first melting step, the exhaust step is then performed. During the exhaust step, the getter material is activated and becomes adsorbable.

[0145] Next, in the second melting step (to be described later), the glass panel unit 10 is sealed and separated from the vacuum pump. Thereafter, the gas released into the evacuated space 50 of the glass panel unit 10 is adsorbed into the getter material. At this time, the hydrogenation catalyst preferentially adsorbs silicon dioxide and hydrocarbon-based gases, thereby making the adsorption sites of Cu-ZSM-5 available for adsorption of nitrogen and methane gases. In addition, the crystal size of Cu-ZSM-5 is set to be equal to or greater than 400nm, preferably equal to or greater than 600nm so that a good vacuum can be maintained in a low pressure range.

[0146] The fifth step is a step of arranging the outer peripheral wall 410 and the partition 420 (sealant arranging step) (see Figure 3 ). The fifth step includes forming the peripheral wall 410 by applying a first sealant onto the second glass plate 300 using, for example, a dispenser, and then drying the first sealant. The fifth step also includes forming the partition 420 by applying a second sealant onto the second glass plate 300 using, for example, a dispenser, and then drying the second sealant.

[0147] By performing the first to fifth steps, a second glass plate 300 (eg Figure 3 ). On the second glass plate 300, a peripheral wall 410, a partition 420, an air passage 600, an exhaust port 700, a gas adsorbent 60, and a plurality of spacers 70 have been formed.

[0148] The sixth step is a step of arranging the first glass plate 200 and the second glass plate 300 (arranging step). Figure 4 As shown in FIG. 1 , in the sixth step, the first glass plate 200 and the second glass plate 300 are arranged to be parallel to each other and face each other.

[0149] Figure 5 The assembly 100 shown in is obtained by performing the assembly steps. After the assembly steps have been performed, as shown in FIG. Figure 6 As shown in , a first melting step (bonding step), an exhaust step, and a second melting step (sealing step) are performed.

[0150] The first melting step is a step of once melting the peripheral wall 410 to seal and combine the first glass plate 200 and the second glass plate 300 together with the peripheral wall 410. Specifically, the first glass plate 200 and the second glass plate 300 are loaded into a melting furnace and heated at a first melting temperature Tm1 for a predetermined time (first melting time) tm1 (see Figure 6 ). In this embodiment, the first sealant and the second sealant are the same material as described above, and therefore the softening point of the first sealant (first softening point) is the same as the softening point of the second sealant (second softening point). Therefore, the first melting temperature Tm1 is set to a temperature equal to or higher than the first softening point and the second softening point. Even if the first melting temperature Tm1 is equal to or higher than the first softening point and the second softening point, the partition 420 does not close the air passage 600 in the first melting step because the exhaust step is started after the first melting step (see Figure 6 ). That is, in the first melting step, the air channel 600 is still available. In the first melting step, if the first softening point and the second softening point are 265° C., the first melting temperature Tm1 may be set to, for example, 290° C. For example, the first melting time tm1 may be 15 minutes.

[0151] In this embodiment, the implementation in which the first softening point is the same as the second softening point not only encompasses the implementation in which the first softening point is exactly the same as the second softening point, but also encompasses the implementation in which the first softening point is approximately equal to the second softening point.

[0152] Heating the peripheral wall 410 at the first melting temperature Tm1 allows the peripheral wall 410 to be softened while reducing deformation of the partition 420. This makes it easier to sealably combine the first and second glass sheets 200 and 300 with the peripheral wall 410.

[0153] The exhaust step is a step of exhausting gas from the first space 510 through the air passage 600, the second space 520 and the exhaust port 700 to transform the first space 510 into the evacuated space 50. For example, the gas may be exhausted using a vacuum pump. Figure 5As shown in , the vacuum pump may be connected to the assembly 100 via an exhaust pipe 810 and a sealing head 820. For example, the exhaust pipe 810 may be coupled to the second glass plate 300 so that the inside of the exhaust pipe 810 and the exhaust port 700 are communicated with each other. Then, the sealing head 820 is attached to the exhaust pipe 810, thereby connecting the suction port of the vacuum pump to the exhaust port 700. The first melting step, the exhaust step, and the second melting step are performed while the assembly 100 remains loaded in the melting furnace. Therefore, the exhaust pipe 810 is coupled to the second glass plate 300 at least before the first melting step.

[0154] The exhaust step includes exhausting gas from the first space 510 through the air passage 600, the second space 520, and the exhaust port 700 at a temperature equal to or higher than the exhaust temperature Te for a predetermined time (exhaust time) te or longer (see Figure 6 ). The exhaust temperature Te is set to a temperature lower than the second softening point (e.g., 265°C) of the second sealant. For example, the exhaust temperature Te may be 250°C. This prevents the partition 420 from deforming even in this exhaust step. During this exhaust step, at least water in the gas adsorbent 60 is vaporized and released into the first space 510. Then, water is discharged from the first space 510 through the air channel 600, the second space 520, and the exhaust port 700. Therefore, discharging the water released from the gas adsorbent 60 allows the getter material to further restore its gas adsorption properties. The exhaust time te is set to create an evacuated space 50 with a predetermined vacuum degree (e.g., a vacuum degree of 0.1 Pa or less). For example, the exhaust time te may be set to 30 minutes. In addition, at this time, the activation temperature of the gas adsorbent 60 is the exhaust temperature Te. That is, the getter material powder is contained in the gas adsorbent 60, and the activatable temperature of the getter material is equal to or lower than the exhaust temperature Te.

[0155] The second melting step is a step of closing at least the air passage 600 by deforming the partition 420 to form the boundary wall 42 and thereby obtaining the semi-finished product 110. That is, the second melting step includes closing the air passage 600 by deforming the partition 420. In other words, the first space 510 is closed by the deformed partition 420, so that the first space 510 and the second space 520 are separated from each other. In this way, the frame member 40 (see FIG. 4 ) surrounding the evacuated space 50 is formed. Figure 7 ). In this embodiment, the partition 420 is deformed so that both longitudinal ends of the partition 420 (i.e., the first blocking portion 4221 and the second blocking portion 4222) are in contact with the peripheral wall 410 and become one with the peripheral wall 410. Figure 7As shown in FIG. 5 , a boundary wall 42 is formed, which hermetically divides the internal space 500 into a first space 510 (evacuated space 50) and a second space 520. More specifically, once the partition 420 is melted at a predetermined temperature (second melting temperature) Tm2 equal to or higher than the second softening point of the second sealant, the partition 420 is deformed. Specifically, the first glass plate 200 and the second glass plate 300 are heated at the second melting temperature Tm2 in the melting furnace for a predetermined time (second melting time) tm2 (see FIG. 5 ). Figure 6 ). The second melting temperature Tm2 and the second melting time tm2 are set so that the partition 420 is softened to close the air channel 600. The lower limit of the second melting temperature Tm2 is the second softening point (e.g., 265°C). For example, the second melting temperature Tm2 can be set to 300°C. In addition, for example, the second melting time tm2 can be 30 minutes. In this embodiment, the sealing step is the second melting step. In short, the sealing step is a step of spatially separating the evacuated space 50 from other spaces. In this embodiment, the space other than the evacuated space 50 corresponds to the second space 520.

[0156] In this embodiment, if Figure 6 As shown in , the exhaust step starts after the first melting step and ends at the end of the second melting step. Therefore, during the second melting step, the gas is exhausted from the first space 510 through the air channel 600, the second space 520 and the exhaust port 700. This creates a pressure difference between the inside and the outside of the assembly 100. The pressure difference brings the first glass plate 200 and the second glass plate 300 closer to each other. Therefore, the second melting step includes forming the boundary wall 42 of the closed air channel 600 by deforming the partition 420 at the second melting temperature Tm2, ​​while exhausting the gas from the first space 510 through the air channel 600, the second space 520 and the exhaust port 700.

[0157] In addition, Figure 6 In the second melting step shown in , after the second melting time tm2 has passed, the temperature in the melting furnace is lowered to room temperature at a constant rate. Then, the sealing head 820 is removed to end the second melting step and the exhaust step.

[0158] By performing these preparation steps, Figure 7 The semi-finished product 110 shown in FIG. Figure 7 As shown in FIG. 1 , the semi-finished product 110 includes a first glass plate 200, a second glass plate 300, a peripheral wall 41, and a boundary wall 42. In addition, the semi-finished product 110 also has an evacuated space 50 and a second space 520. The semi-finished product 110 also includes a gas adsorbent 60 and a plurality of columns (spacers) 70 in the evacuated space 50. The semi-finished product 110 also has an exhaust port 700.

[0159] The first glass plate 200 and the second glass plate 300 each have a rectangular flat plate shape. The first glass plate 200 and the second glass plate 300 have the same planar shape.

[0160] The boundary wall 42 separates the evacuated space 50 from the second space 520 (in space). In other words, the second space 520 of the semi-finished product 110 is connected to the external environment (in space) through the exhaust port 700, and thus the boundary wall 42 separates the evacuated space 50 from the external environment. The boundary wall 42 and the peripheral wall 410 together form a frame member 40 surrounding the evacuated space 50. The frame member 40 not only completely surrounds the evacuated space 50, but also seals and combines the first glass plate 200 and the second glass plate 300 together.

[0161] The gas adsorbent 60 is placed in the evacuated space 50. Specifically, the gas adsorbent 60 has an elongated flat plate shape and is disposed on the second glass plate 300. The gas adsorbent 60 is used to adsorb unnecessary gas (such as residual gas). For example, the unnecessary gas may be gas emitted from the hot melt adhesive (i.e., the first hot melt adhesive and the second hot melt adhesive) when the hot melt adhesive forming the frame member 40 is heated.

[0162] A plurality of spacers 70 are placed in the evacuated space 50. The plurality of spacers 70 are used to maintain a desired gap distance between the first glass plate 200 and the second glass plate 300.

[0163] As described above, the evacuated space 50 is created by exhausting gas from the first space 510 through the second space 520 and the exhaust port 700. In other words, the evacuated space 50 is the first space 510 whose vacuum degree is a predetermined value or less. For example, the predetermined value may be 0.1 Pa. The evacuated space 50 is completely sealed by the first glass plate 200, the second glass plate 300, and the frame member 40, and is therefore separated from the second space 520 and the exhaust port 700.

[0164] The removing step is performed after the preparing step has been performed. The removing step is a step of removing the portion 11 having the second space 520 from the semi-finished product 110 to obtain a Figure 8 The glass panel unit 10 is shown in a partial form with an evacuated space 50 .

[0165] The glass panel unit 10 includes a first glass plate 20 and a second glass plate 30. The first glass plate 20 is a portion of the first glass plate 200 corresponding to the first space 510 (ie, the evacuated space 50). The second glass plate 30 is a portion of the second glass plate 300 corresponding to the first space 510 (ie, the evacuated space 50).

[0166] On the other hand, the unnecessary portion 11 includes the portion 230 of the first glass plate 200 corresponding to the second space 520 and the portion 320 of the second glass plate 300 corresponding to the second space 520. It should be noted that in consideration of the manufacturing cost of the glass panel unit 10, the unnecessary portion 11 is preferably as small as possible.

[0167] Specifically, in the removing step, the semi-finished product 110 unloaded from the melting furnace is cut along the boundary wall 42 to be divided into a portion (glass panel unit) 10 having the evacuated space 50 and a portion (unnecessary portion) 11 having the second space 520. It should be noted that the shape of the portion (i.e., the cutting line) where the semi-finished product 110 is cut off is determined by the shape of the glass panel unit 10. Since the glass panel unit 10 has a rectangular shape, the cutting line has a linear shape aligned with the length of the boundary wall 42.

[0168] Figure 2 The glass panel unit 10 shown in FIG. 1 is obtained through the above-mentioned preparation steps and removal steps.

[0169] Figure 2 The glass panel unit (i.e., a glass panel unit as a final product) 10 according to this embodiment is illustrated. The glass panel unit 10 includes a first glass plate 20, a second glass plate 30, and a frame member 40. In addition, the glass panel unit 10 also has an evacuated space 50 surrounded by the first glass plate 20, the second glass plate 30, and the frame member 40. The glass panel unit 10 also includes a gas adsorbent 60 and a plurality of columns (spacers) 70 in the evacuated space 50. In the glass panel unit 10, neither the first glass plate 20 nor the second glass plate 30 has an exhaust port 700.

[0170] The first glass plate 20 and the second glass plate 30 may each have a rectangular flat plate shape. The first glass plate 20 and the second glass plate 30 have the same planar shape.

[0171] The first glass plate 20 according to this embodiment is obtained by removing the unnecessary portion 230 from the first glass plate 200 through a removal step. Therefore, the first glass plate 20 has the same configuration as the first glass plate 200. That is, the first glass plate 20 includes a body forming a main shape of the first glass plate 20 and a low-emissivity film 220. In the evacuated space 50, the body is covered with the low-emissivity film 220. The first glass plate 20 has a rectangular flat plate shape.

[0172] The second glass plate 30 according to this embodiment is obtained by removing the unnecessary portion 320 from the second glass plate 300 through a removal step. Therefore, the second glass plate 30 has the same configuration as the second glass plate 300. That is, the second glass plate 30 includes a body forming a main shape of the second glass plate 30. In this embodiment, the second glass plate 30 consists only of the body. Optionally, the second glass plate 30 may include not only the body but also a low emissivity film corresponding to the low emissivity film 220. If the second glass plate 30 includes the low emissivity film, the low emissivity film covers the body of the second glass plate 30 in the evacuated space 50 and is in contact with it.

[0173] The frame member 40 is disposed between the first glass plate 20 and the second glass plate 30 to sealably combine the first glass plate 20 with the second glass plate 30. Therefore, the evacuated space 50 is surrounded by the first glass plate 20, the second glass plate 30, and the frame member 40. The frame member 40 has a polygonal (e.g., quadrilateral in this embodiment) frame shape corresponding to the shapes of the first glass plate 20 and the second glass plate 30. The frame member 40 is formed along the outer periphery of each of the first glass plate 20 and the second glass plate 30.

[0174] A plurality of spacers 70 are placed in the evacuated space 50. The plurality of spacers 70 are used to maintain a desired gap distance between the first glass sheet 20 and the second glass sheet 30.

[0175] <How do gas adsorbents adsorb gases>

[0176] The gas adsorbent 60 is placed in the evacuated space 50 of the glass panel unit 10. The getter material contained in the gas adsorbent 60 contains a plurality of particles having an activatable temperature equal to or lower than 400°C. As used herein, "activatable temperature" refers to a temperature required for the plurality of particles contained in the gas adsorbent 60 to be activated. That is, the plurality of particles contained in the gas adsorbent 60 are activated at a temperature equal to or higher than the activatable temperature. The activated particles in the gas adsorbent 60 have their gas adsorption capacity increased. In other words, when the activatable temperature is reached, the particles in the gas adsorbent 60 are activated by releasing the adsorbed gas therefrom and become to have an increased gas adsorption capacity. If the gas adsorbent 60 has been heated at a predetermined heating temperature for a sufficiently long time in a vacuum equal to or lower than 0.001 Pa and then the amount of adsorbed nitrogen is measured at a nitrogen equilibrium pressure of 0.1 Pa under an environment of 20°C, the activatable temperature is the temperature at which the amount of adsorbed nitrogen becomes equal to or greater than 4×10 –11mol / g of the minimum required heating temperature. The amount of adsorbed nitrogen is used as follows to see if the activation temperature is equal to or higher than the activatable temperature. Specifically, as a pretreatment, 0.5 g of the adsorbent is heated at a predetermined temperature (i.e., the activation temperature) for 12 hours or longer while exhausting the gas from the furnace using, for example, a turbo pump (such as BELSORP-MAX manufactured by Microtrac BEL Corporation). Thereafter, the temperature is lowered to 20°C, and the amount of adsorbed nitrogen is measured at an equilibrium pressure of 0.1 Pa using nitrogen having a purity equal to or greater than 6N as the adsorbate. If the amount of the adsorbed gas is equal to or greater than 4×10 –11 mol / g, it can be confirmed that the predetermined temperature (activation temperature) is equal to or higher than the activatable temperature.

[0177] Next, particles contained in the gas adsorbent 60 and made of zeolite crystals will be described.

[0178] In the getter material contained in the gas adsorbent 60, the zeolite particles accounting for half or more of the total weight of a large number (or a plurality) of zeolite particles each have a particle size equal to or greater than 200 nm. In other words, the sum of the respective weights of those zeolite particles each having a particle size equal to or greater than 200 nm accounts for half or more of the total weight of the plurality of zeolite particles forming the getter material. Optionally, the sum of the respective weights of those zeolite particles each having a particle size equal to or greater than 200 nm may be the total weight of the plurality of zeolite particles contained in the getter material and the gas adsorbent 60. In this case, the particle size of each of the plurality of zeolite particles contained in the getter material and the gas adsorbent 60 is equal to or greater than 200 nm.

[0179] As described above, generally (for example, under a pressure equal to or higher than 100Pa), the smaller the particle size of the zeolite particles and the larger the number of zeolite particles, the larger the total surface area of ​​the zeolite particles, and the higher the gas adsorption capacity of the zeolite becomes. If the zeolite particles have a relatively small particle size, the depth of the internal space extending inward from the micropores on the surface (that is, the length of the path extending from the surface) is relatively short. Therefore, the gas (molecule) cannot reach the depth of the internal space of the particle, but is retained (adsorbed) near the surface. The gas retained near the surface will be desorbed from the particle within a predetermined time (which varies from particle to particle). However, there is another gas to be newly adsorbed. Therefore, a balance is established between the gas desorbed from the particle and the gas adsorbed on the particle. From the perspective of this balance, the lower the pressure, the smaller the amount of newly adsorbed gas, and the smaller the balance point between desorption and adsorption. Therefore, the gas adsorption capacity per unit weight decreases. In addition, under constant pressure, the smaller the particle size and the larger the total surface area, the higher the gas adsorption capacity per unit weight becomes.

[0180] However, in a low pressure range (e.g., equal to or lower than 100Pa, and in particular equal to or lower than 30Pa), from a different point of view from equilibrium, the desorption of gas from large particles will be reduced. Specifically, in relatively large particles, the surface area per unit weight is relatively small, but the depth of the internal space extending inward from the micropores on the surface is relatively long. Therefore, compared with the case of relatively small particles, a larger number of gas molecules can reach the depth of the internal space of the particles. Once the gas molecules have reached the depth of the internal space, it is difficult to desorb from the particles. This is why in a low pressure range, the larger the particle size of the particles, the higher the gas adsorption capacity per unit weight.

[0181] Next, the particle size of the zeolite particles will be described. If the zeolite particles have a spherical shape, the particle size is the diameter of the sphere. On the other hand, if the zeolite particles have a non-spherical shape, the zeolite particles generally have an ellipsoidal shape or a rectangular parallelepiped shape. In this case, the shortest width of the zeolite particles will be the most significant influence on the gas adsorption capacity. As used herein, "shortest width" refers to the length of the shortest line segment among multiple line segments passing through the center of mass on the plane including the center of mass of the particle. For example, if the zeolite particles have an ellipsoidal shape, the shortest width is the length in the short axis direction of the zeolite particles. On the other hand, if the zeolite particles have, for example, a rectangular parallelepiped shape, the shortest width is the length of the shortest side among multiple sides of the rectangular parallelepiped. If the shape of the zeolite particles is neither a rectangular parallelepiped shape nor an ellipsoidal shape, the shortest width refers to the minimum particle width in a set of lines with the longest width and the maximum vertical particle width on any plane including a line with the longest width of the particle. It should be noted that if the zeolite particles have a spherical shape, the shortest width is the diameter of the sphere.

[0182] In this case, the shortest width of the particle is adopted as an indicator for the following reasons. Specifically, the portion corresponding to the shortest width tends to have a wide surface area. In addition, the shorter the depth of the internal space of the portion corresponding to the shortest width, the more likely the gas that has reached the internal space is to be desorbed. This is why the shortest width of the zeolite particle will most significantly affect the gas adsorption capacity of the zeolite particle per unit weight.

[0183] The particle size can be determined by measuring the short axis width of the particle through observation via a so-called “scanning electron microscope (SEM).” If the particle has a flat plate shape, the thickness of the plate particle can be measured as its short axis width.

[0184] In addition, the weight ratio of each particle can be determined by calculating the volume ratio thereof based on each shape of the particles observed via SEM. It should be noted that if non-zeolite particles are included, the volume ratio is calculated excluding those non-zeolite particles.

[0185] Fig. 9 and Fig.10 The results of an experiment conducted to compare the gas adsorption capacity of copper ion-exchanged ZSM-5 particles having a particle size of 50 nm and copper ion-exchanged ZSM-5 particles having a particle size of 400 nm are shown. Fig. 9 and Fig.10 (showing the relationship between equilibrium pressure and the amount of gas adsorbed), the abscissa represents the equilibrium pressure (Pa), and the ordinate represents the amount of nitrogen adsorbed at 20° C. (in arbitrary units). It should be noted that Fig. 9 The ordinate and abscissa axes in are common axes, but Fig.10 The vertical axis and horizontal axis in are logarithmic axes. Fig.10 It can be seen that around the point where the equilibrium pressure is about 30 Pa, the graph shifts in the gas adsorption capacity levels of the copper ion-exchanged ZSM-5 particles having a particle size of 50 nm and the copper ion-exchanged ZSM-5 particles having a particle size of 400 nm.

[0186] In this embodiment, preferably, the particle diameter of each of the particles accounting for half or more of the total weight of the plurality of (i.e., multiple) particles contained in the gas adsorbent 60 is equal to or greater than 200 nm. More preferably, the particle diameter of each of the particles accounting for half or more of the total weight of the plurality of particles contained in the gas adsorbent 60 is equal to or greater than 300 nm. Even more preferably, the particle diameter of each of the particles accounting for half or more of the total weight of the plurality of particles contained in the gas adsorbent 60 is equal to or greater than 400 nm. In other words, preferably, the sum of the respective weights of the particles each having a particle diameter equal to or greater than 400 nm is half or more of the total weight of the plurality of particles contained in the gas adsorbent 60.

[0187] Fig.11 The results of an experiment conducted to compare the gas adsorption capacity of particles having a particle size of 50 nm and particles having a particle size of 400 nm are shown. Fig.11 In (showing the relationship between the ratio of the amount of adsorbed gas and the activation temperature), the abscissa represents the activation temperature (°C), and the ordinate represents the ratio of the amount of nitrogen adsorbed into particles with a particle size of 400 nm to the amount of nitrogen adsorbed into particles with a particle size of 50 nm at an equilibrium pressure of 0.1 Pa in an environment of 20°C. Fig.11It can be seen from the graph that the ratio of the amount of gas adsorbed is larger in the case where the activation temperature is 350° C. than in the case where the activation temperature is 400° C., and the ratio of the amount of gas adsorbed is much larger in the case where the activation temperature is 250° C. than in the case where the activation temperature is 350° C. This is probably because in the case of the copper ion exchange type zeolite, setting the activation temperature (i.e., the temperature in the exhaust step) to a temperature equal to or lower than 350° C. significantly reduces the possibility of revealing strong nitrogen adsorption sites through copper oxide reduction, and instead increases the ratio of the crystal size effect.

[0188] Therefore, the advantages of this embodiment are more significantly achieved when the exhaust temperature (equivalent to the activation temperature) during the manufacturing process of the glass panel unit 10 is equal to or lower than 400° C., even more significantly achieved when the exhaust temperature is equal to or lower than 350° C., and particularly significantly achieved when the exhaust temperature is equal to or lower than 300° C. In addition, since the exhaust step is performed at a temperature near or lower than the melting temperature of the sealant (i.e., the first sealant and the second sealant), the glass panel unit 10 according to the present invention achieves significant advantages when the melting temperature of the sealant (which is at least one of the first sealant or the second sealant) is equal to or lower than 400° C., more significantly achieved when the melting temperature of the sealant is equal to or lower than 350° C., and particularly significantly achieved when the melting temperature of the sealant is equal to or lower than 300° C.

[0189] Fig.12 The relationship between the amount of residual gas and the size of the crystal (crystal size) is shown in FIG. Figure 6 The catalyst was activated under the same conditions as the exhaust step (at exhaust temperature Te = 250°C) between the first melting step and the second melting step shown in FIG. Fig.12 In the graph shown, the abscissa represents the crystal size (which is the size of the crystal (nm)), and the ordinate represents the amount of residual gas (in arbitrary units). Fig.12 It can be seen that the amount of residual gas is smaller when the crystal size is 400 nm and when the crystal size is 200 nm than when the crystal size is 50 nm.

[0190] Therefore, in the glass panel unit 10, the getter material preferably includes copper ion exchange type zeolite having a crystal size equal to or greater than 400nm, and the softening point or melting point of the sealant (which is at least one of the first sealant or the second sealant) is preferably equal to or lower than 350°C.

[0191] The glass panel unit 10 makes it easier to reduce the nitrogen partial pressure in the evacuated space 50 to 0.1 Pa or less. This means that even if nitrogen, which is difficult to adsorb into ordinary adsorbents, remains in the evacuated space of the glass panel unit 10 or is released into the evacuated space of the glass panel unit 10, a sufficiently high vacuum degree can still be generated, and good thermal insulation properties can be easily achieved.

[0192] Furthermore, this embodiment makes it easier to make the total amount of nitrogen adsorbed equal to or greater than 0.1 V (Pa·m 3 ), where V(m 3 ) is the volume of the evacuated space 50. This means that even if the pressure in the evacuated space 50 may be raised to 0.1 Pa or more by the nitrogen gas remaining in or released into the evacuated space 50, the partial pressure of the nitrogen gas may be lowered to 0.1 Pa or less by adsorbing the nitrogen gas into the gas adsorbent 60 according to this embodiment.

[0193] In addition, the particle diameter of particles accounting for half or more of the total weight of the plurality of particles is preferably equal to or less than 30 μm, more preferably equal to or less than 10 μm.

[0194] Fig.13 A shows the relationship between the amount of residual gas in the glass panel unit 10 and the size of the crystal (crystal size). Fig.13 As can be seen from Figure A, the amount of residual gas in the glass panel unit 10 is different depending on whether the solvent of the getter material composition is water or an organic solvent. That is, depending on whether the solvent of the getter material composition is water or an organic solvent, not only the volume of the solvent retained in each particle of the zeolite crystal is different, but also the gas adsorption capacity of the gas adsorbent 60 is different.

[0195] As from Fig.13 A It is clear that if the crystal size of zeolite is very small, the gas adsorbent using an organic solvent as a solvent for the getter material composition has a large amount of residual gas (i.e., the gas adsorbent has a relatively low performance). However, when the crystal size of zeolite is 400 nm, the gas adsorbent using an organic solvent as a solvent for the getter material composition and the gas adsorbent using water as a solvent for the getter material composition have almost the same amount of residual gas (i.e., the residual gas amount ratio becomes approximately equal to 1). When the crystal size of zeolite is greater than 400 nm, the properties of the gas adsorbent (i.e., gas adsorption capacity) are better when the organic solvent is used as a solvent for the getter material composition than when water is used as a solvent for the getter material composition. For example, when the crystal size of zeolite is equal to or greater than 600 nm, the residual gas amount ratio is equal to or less than 1.

[0196] like Fig.13As shown in FIG. 2B , when the particle size of the zeolite crystal particles is equal to or greater than 500 nm, the residual gas amount ratio is equal to or less than 1, and therefore it is more advantageous to use an organic solvent (rather than water) as the solvent of the getter material composition. That is, the gas adsorbent becomes higher in gas adsorption capacity by using an organic solvent as the solvent of the getter material composition (rather than using water as its solvent). It should be noted that the residual gas amount ratio is obtained by the following equation (2):

[0197] Residual gas volume ratio = [Residual gas volume when using organic solvent] ÷ [Residual gas volume when using water] (2)

[0198] Therefore, when an organic solvent is used as a solvent for the getter material composition, the particle size of each particle of the zeolite crystal (i.e., crystal size) is preferably at least 200 nm, more preferably equal to or greater than 300 nm, even more preferably equal to or greater than 400 nm, still more preferably equal to or greater than 500 nm, and particularly preferably equal to or greater than 600 nm. Even better, the particle size of the particles of the zeolite crystal is equal to or greater than 750 nm, equal to or greater than 1000 nm, equal to or greater than 1500 nm, or equal to or greater than 2000 nm. That is, the getter material composition preferably contains a copper ion exchange type zeolite having a crystal size equal to or greater than 400 nm (or equal to or greater than 600 nm), and preferably contains an organic solvent having a ring structure.

[0199] For example, in the getter material composition, the particle diameter of those particles accounting for half or more of the total weight of the plurality of particles of zeolite crystals is preferably equal to or greater than 200 nm, and the average particle diameter of those particles is preferably equal to or greater than 200 nm. This makes it possible to provide a gas adsorbent 60 that is likely to exhibit sufficient adsorption performance in a low pressure range. The average particle diameter (average size) of the plurality of particles of zeolite crystals can be determined by measuring the short axis width of each of the plurality of particles through SEM observation and calculating the average value thereof as described above.

[0200] The inventors experimented in the same manner using 0.5 parts by mass of zeolite particles each having a crystal size less than 200nm (e.g., a crystal size of 50nm) and 0.5 parts by mass of zeolite particles each having a crystal size equal to or greater than 200nm (e.g., a crystal size of 400nm) mixed with an organic solvent. As a result, the amount of residual gas was close to (i.e., from the same to 1.5 times larger) the amount of residual gas in the case where the zeolite particles (wherein the crystal size of each is 400nm) were mixed with an organic solvent. However, when 0.75 parts by mass of zeolite particles each having a crystal size less than 200nm (e.g., a crystal size of 50nm) and 0.25 parts by mass of zeolite particles each having a crystal size equal to or greater than 200nm (e.g., a crystal size of 400nm) were mixed with an organic solvent, the amount of residual gas was almost the same as the amount of residual gas in the case where the zeolite particles (wherein the crystal size of each is 50nm) were mixed with an organic solvent (i.e., from 0.8 times larger to the same). This may be because zeolite particles with relatively small crystal sizes are releasing gas under the low pressure state that should be established when using zeolite particles each with a large crystal size. As the proportion of such zeolite particles with relatively small crystal sizes increases, the release of gas as a whole exceeds the adsorption of gas in the getter material in the low pressure range, thereby reducing the advantages to be achieved by particles with relatively large crystal sizes. This is why those zeolite particles each with a crystal size of less than 200 nm preferably account for less than half of the total weight of the plurality of particles of zeolite crystals.

[0201] In addition, the sum of the respective weights of the zeolite particles each having a crystal size less than 300nm more preferably accounts for less than half of the total weight of the plurality of particles of zeolite crystals. The sum of the respective weights of the zeolite particles each having a crystal size less than 400nm more preferably accounts for less than half of the total weight of the plurality of particles of zeolite crystals. The sum of the respective weights of the zeolite particles each having a crystal size less than 500nm more preferably accounts for less than half of the total weight of the plurality of particles of zeolite crystals. The sum of the respective weights of the zeolite particles each having a crystal size less than 600nm more preferably accounts for less than half of the total weight of the plurality of particles of zeolite crystals. The sum of the respective weights of the zeolite particles each having a crystal size less than 750nm more preferably accounts for less than half of the total weight of the plurality of particles of zeolite crystals. The sum of the respective weights of the zeolite particles each having a crystal size less than 1000nm more preferably accounts for less than half of the total weight of the plurality of particles of zeolite crystals. The sum of the respective weights of the zeolite particles each having a crystal size less than 1500nm more preferably accounts for less than half of the total weight of the plurality of particles of zeolite crystals. The sum of the respective weights of the zeolite particles each having a crystal size less than 2000 nm more preferably accounts for less than half of the total weight of the plurality of particles of zeolite crystals. In addition, the sum of the respective weights of the zeolite particles each having a crystal size less than 200 nm may account for less than half of the total weight of the plurality of particles of zeolite crystals, and the sum of the respective weights of the zeolite particles each having a crystal size equal to or greater than 400 nm may account for more than 25% of the total weight of the plurality of particles of zeolite crystals. This may reduce the impact of particles having small crystal sizes.

[0202] It should be noted that the size ratio of the zeolite particles (crystals) is expressed on a weight basis in the previous paragraph. Even if the comparison is based on the number or volume of particles, almost the same trend is observed. That is, the number of particles with a respective crystal size less than 200nm preferably accounts for less than half of the total number of multiple particles of zeolite crystals. Alternatively, the sum of the respective volumes of particles with a respective crystal size less than 200nm preferably accounts for less than half of the total volume of multiple particles of zeolite crystals.

[0203] In addition, the sum of the respective volumes of the zeolite particles each having a crystal size less than 300nm more preferably accounts for less than half of the total volume of multiple particles of zeolite crystals. The sum of the respective volumes of the zeolite particles each having a crystal size less than 400nm more preferably accounts for less than half of the total volume of multiple particles of zeolite crystals. The sum of the respective volumes of the zeolite particles each having a crystal size less than 500nm more preferably accounts for less than half of the total volume of multiple particles of zeolite crystals. The sum of the respective volumes of the zeolite particles each having a crystal size less than 600nm more preferably accounts for less than half of the total volume of multiple particles of zeolite crystals. The sum of the respective volumes of the zeolite particles each having a crystal size less than 750nm more preferably accounts for less than half of the total volume of multiple particles of zeolite crystals. The sum of the respective volumes of the zeolite particles each having a crystal size less than 1000nm more preferably accounts for less than half of the total volume of multiple particles of zeolite crystals. The sum of the respective volumes of the zeolite particles each having a crystal size less than 1500nm more preferably accounts for less than half of the total volume of multiple particles of zeolite crystals. More preferably the sum of the individual volumes of the zeolite particles, each having a crystal size of less than 2000 nm, accounts for less than half of the total volume of the plurality of particles of zeolite crystals.

[0204] In addition, the number of zeolite particles each having a crystal size less than 300nm more preferably accounts for less than half of the total number of multiple particles of zeolite crystals. The number of zeolite particles each having a crystal size less than 400nm more preferably accounts for less than half of the total number of multiple particles of zeolite crystals. The number of zeolite particles each having a crystal size less than 500nm more preferably accounts for less than half of the total number of multiple particles of zeolite crystals. The number of zeolite particles each having a crystal size less than 600nm more preferably accounts for less than half of the total number of multiple particles of zeolite crystals. The number of zeolite particles each having a crystal size less than 750nm more preferably accounts for less than half of the total number of multiple particles of zeolite crystals. The number of zeolite particles each having a crystal size less than 1000nm more preferably accounts for less than half of the total number of multiple particles of zeolite crystals. The number of zeolite particles each having a crystal size less than 1500nm more preferably accounts for less than half of the total number of multiple particles of zeolite crystals. The number of zeolite particles each having a crystal size less than 2000nm more preferably accounts for less than half of the total number of multiple particles of zeolite crystals.

[0205] In addition, the sum of the individual volumes of the zeolite particles each having a crystal size less than 200 nm may account for less than half of the total volume of the plurality of particles of the zeolite crystal, and the sum of the individual volumes of the zeolite particles each having a crystal size equal to or greater than 400 nm may account for more than 25% of the total volume of the plurality of particles of the zeolite crystal. This may reduce the impact of particles having a small crystal size. In addition, the number of zeolite particles each having a crystal size less than 200 nm may account for less than half of the total number of the plurality of particles of the zeolite crystal, and the number of zeolite particles each having a crystal size equal to or greater than 400 nm may account for more than 25% of the total number of the plurality of particles of the zeolite crystal.

[0206] Fig.13 A and Fig.13 The glass panel unit 10 used in B has the following details:

[0207] Getter material as a constituent material of the gas adsorbent: Cu-ZSM-5 (copper ion exchange type zeolite);

[0208] ·Weight of gas adsorbent: 100 mg;

[0209] Solvent for the getter material composition: α-pinene or water (it should be noted that the getter material composition was applied after the getter material and the solvent were mixed with each other and the mixture thus obtained was left to stand for one week);

[0210] Volume of evacuated space: 9000mm 3 ;

[0211] First melting temperature: 290°C;

[0212] Exhaust temperature and time: 250℃ and 30min;

[0213] Second melting temperature: 300°C; and

[0214] • Sealant: Vanadium-based glass frit (softening point 270° C.; the same material was used as the first sealant and the second sealant).

[0215] (Variant)

[0216] It should be noted that the above-mentioned embodiments are merely exemplary embodiments of the various embodiments of the present disclosure and should not be construed as restrictive. On the contrary, the above-mentioned exemplary embodiments can be easily modified in various ways according to design selection or any other factors without departing from the scope of the present disclosure. Next, the variations of the exemplary embodiments will be listed one after another. In the following description, the above-mentioned exemplary embodiments will be referred to as "basic embodiments" hereinafter.

[0217] In the above basic embodiment, among the first glass plate 200 and the second glass plate 300, only the first glass plate 200 includes the low emissivity film 220. In a variation, the second glass plate 300 may also include the low emissivity film. That is, each of the first glass plate 200 and the second glass plate 300 may include the low emissivity film. Therefore, each of the first glass plate 20 and the second glass plate 30 may also include the low emissivity film. Alternatively, both the first glass plate 20 and the second glass plate 30 may not include any low emissivity film.

[0218] In the above basic embodiment, in the first glass plate 200 and the second glass plate 300, the first glass plate 200 includes the low emissivity film 220, but the second glass plate 300 does not include the low emissivity film. However, in another modification, the second glass plate 300 may include the low emissivity film, while the first glass plate 200 may not include the low emissivity film 220. Therefore, in the glass panel unit 10 according to this modification, the second glass plate 30 may include the low emissivity film, while the first glass plate 20 may not include the low emissivity film 220.

[0219] In the above basic embodiment, the exhaust step starts after the first melting step has ended. In a variation, if the temperature in the melting furnace is below the first softening point after the first melting time tm1 has elapsed, the exhaust step may start midway through the first melting step.

[0220] In the above basic embodiment, the exhaust step ends when the second melting step ends. In a variation, the exhaust step may begin after the first melting step has ended, and may end before the second melting step ends.

[0221] In the above basic embodiment, the glass panel unit 10 has a rectangular shape. Alternatively, in a variation, the glass panel unit 10 may also have a circular shape, a polygonal shape, or any other desired shape. That is, the first glass plate 20 and the second glass plate 30 do not have to be rectangular, but may also have a circular shape, a polygonal shape, or any other desired shape.

[0222] The first glass plate 20 and the second glass plate 30 do not necessarily have the same planar shape and the same planar size. In addition, the first glass plate 20 does not necessarily have to be as thick as the second glass plate 30. The same statement also applies to the first glass plate 200 and the second glass plate 300.

[0223] The outer peripheral wall 410 also does not necessarily have the same planar shape as the first glass plate 200 and the second glass plate 300 .

[0224] Optionally, the peripheral wall 410 may include other elements (eg, a core material).

[0225] In addition, in the assembly 100, the peripheral wall 410 is only disposed between the first glass plate 200 and the second glass plate 300, and does not combine the first glass plate 200 with the second glass plate 300. However, alternatively, at the stage of the assembly 100, the peripheral wall 410 may combine the first glass plate 200 with the second glass plate 300. In short, in the assembly 100, the peripheral wall 410 only needs to be disposed between the first glass plate 200 and the second glass plate 300, and does not necessarily combine the first glass plate 200 with the second glass plate 300.

[0226] In addition, in the above-mentioned basic embodiment, the partition 420 is not in contact with the peripheral wall 410. This allows the air passages 610, 620 to be formed in the respective gaps between the two ends of the partition 420 and the peripheral wall 410. However, this is only an example and should not be interpreted as limiting. Alternatively, only one of the two ends of the partition 420 may be coupled to the peripheral wall 410. In this case, only one air passage 600 may be formed between the partition 420 and the peripheral wall 410. Alternatively, the partition 420 may even have its two ends coupled to the peripheral wall 410. In this case, the air passage 600 may be a through hole provided by the partition 420. Alternatively, the air passage 600 may also be a gap between the partition 420 and the first glass plate 200. Alternatively, the partition 420 may be composed of two or more partitions arranged at a certain distance. In this case, the air passage 600 may be a gap left between the two or more partitions.

[0227] In the above basic embodiment, the air channel 600 includes two air channels 610, 620. Alternatively, only one air channel 600 may be provided, or the air channel 600 may include three or more air channels. In addition, the air channel 600 may have any shape without limitation.

[0228] In addition, in the above basic embodiment, the internal space 500 is divided into one first space 510 and one second space 520. However, this is only an example and should not be construed as limiting. Alternatively, the internal space 500 may also be divided into one or more first spaces 510 and one or more second spaces 520 by the partition 420. If the internal space 500 has two or more first spaces 510, two or more glass panel units 10 can be obtained from a single semi-finished product 110.

[0229] In the above basic embodiment, the first space 510 is the evacuated space 50. However, the evacuated space 50 may be replaced by the evacuated space. The evacuated space is the first space 510 under reduced pressure. As used herein, "reduced pressure condition" refers to a condition in which the pressure is lower than the atmospheric pressure.

[0230] In the above basic embodiment, the evacuated space 50 is spatially separated from the external environment by the boundary wall 42. However, in a variation, only the inner or outer peripheral portion of the exhaust port 700 may be sealed with a sealant. In addition, the sealing may also be accomplished by locally heating only the outer peripheral portion of the exhaust port 700 and thereby melting the sealant, rather than closing the air passage 600 in the second melting step. Alternatively, the sealing may also be accomplished by evacuating the entire furnace and thereby reducing the pressure inside the glass panel unit 10, and then heating the glass panel unit 10 in a vacuum and thereby melting the outer peripheral sealant without forming any exhaust port 700.

[0231] In the above-described basic embodiment, the evacuated space 50 is spatially separated from the external environment by the boundary wall 42. However, in a modification, the evacuated space 50 may also be spatially separated from the external environment by a sealing portion formed by melting and cutting off the middle portion of the exhaust pipe connected to the exhaust port 700. That is, the boundary wall 42 does not necessarily have to be used as a member for spatially separating the evacuated space 50 from the external environment.

[0232] (Summary)

[0233] As can be seen from the above description of the exemplary embodiment and its variations, the glass panel unit (10) according to the first aspect includes: a first glass plate (20); a second glass plate (30) facing the first glass plate (20); a frame member (40); an evacuated space (50); and a gas adsorbent (60). The frame member (40) seals the first glass plate (20) and the second glass plate (30). The evacuated space (50) is surrounded by the first glass plate (20), the second glass plate (30) and the frame member (40). The gas adsorbent (60) is placed in the evacuated space (50). The gas adsorbent (60) contains a getter material. The getter material contains a plurality of particles of zeolite crystals. Particles having a particle size of 200 nm or more account for more than half of the total weight of the plurality of particles. The activatable temperature of the plurality of particles is equal to or lower than 400°C.

[0234] The glass panel unit (10) according to the first aspect can achieve sufficient adsorption performance in a low pressure range.

[0235] The glass panel unit (10) according to the second aspect can be implemented in combination with the first aspect. In the glass panel unit (10) according to the second aspect, the weight of the remaining part of the plurality of particles having a particle size less than 200 nm accounts for less than half of the total weight of the plurality of particles.

[0236] The glass panel unit (10) according to the second aspect can achieve sufficient adsorption performance in a low pressure range.

[0237] The glass panel unit (10) according to the third aspect can be implemented in combination with the first aspect or the second aspect. In the glass panel unit (10) according to the third aspect, particles having a particle size of 400 nm or more account for more than half of the total weight of the plurality of particles.

[0238] The third aspect makes it easier to achieve sufficient adsorption performance in a low pressure range.

[0239] The glass panel unit (10) according to the fourth aspect can be implemented in combination with any one of the first to third aspects. In the glass panel unit (10) according to the fourth aspect, the partial pressure of nitrogen in the evacuated space (50) is equal to or less than 0.1Pa.

[0240] The fourth aspect makes it easier to provide a glass panel unit (10) having excellent thermal insulation properties.

[0241] The glass panel unit (10) according to the fifth aspect can be implemented in combination with any one of the first to fourth aspects. In the glass panel unit (10) according to the fifth aspect, the total amount of nitrogen adsorbed by the plurality of particles at 20° C. is equal to or greater than 0.1 V (Pa·m 3 ), where V(m 3 ) is the volume of the evacuated space (50).

[0242] The fifth aspect makes it easier to provide a glass panel unit (10) having excellent thermal insulation properties.

[0243] The glass panel unit (10) according to the sixth aspect can be implemented in combination with any one of the first to fifth aspects. In the glass panel unit (10) according to the sixth aspect, the zeolite is a copper ion exchange type zeolite.

[0244] The sixth aspect makes it easier for the gas adsorbent (60) to achieve sufficient adsorption performance.

[0245] The glass panel unit (10) according to the seventh aspect can be implemented in combination with any one of the first to sixth aspects. In the glass panel unit (10) according to the seventh aspect, the plurality of particles are primary particles, and the particle diameter is the shortest width of the plurality of particles.

[0246] The glass panel unit (10) according to the seventh aspect can achieve sufficient adsorption performance in a low pressure range.

[0247] The glass panel unit (10) according to the eighth aspect includes: a first glass plate (20); a second glass plate (30) facing the first glass plate (20); a frame member (40); an evacuated space (50); and a gas adsorbent (60). The frame member (40) seals the first glass plate (20) and the second glass plate (30). The evacuated space (50) is surrounded by the first glass plate (20), the second glass plate (30) and the frame member (40). The gas adsorbent (60) is placed in the evacuated space (50). The gas adsorbent (60) contains a getter material. The getter material contains a plurality of particles of zeolite crystals. Particles having a particle size of 200 nm or more account for more than half of the total number of the plurality of particles. The activatable temperature of the plurality of particles is equal to or lower than 400°C.

[0248] The glass panel unit (10) according to the eighth aspect can achieve sufficient adsorption performance in a low pressure range.

[0249] The glass panel unit (10) according to the ninth aspect includes: a first glass plate (20); a second glass plate (30) facing the first glass plate (20); a frame member (40); an evacuated space (50); and a gas adsorbent (60). The frame member (40) seals the first glass plate (20) and the second glass plate (30). The evacuated space (50) is surrounded by the first glass plate (20), the second glass plate (30) and the frame member (40). The gas adsorbent (60) is placed in the evacuated space (50). The gas adsorbent (60) contains a getter material. The getter material contains a plurality of particles of zeolite crystals. Particles having a particle diameter of 200 nm or more account for more than half of the total volume of the plurality of particles. The activatable temperature of the plurality of particles is equal to or lower than 400°C.

[0250] The glass panel unit (10) according to the ninth aspect can achieve sufficient adsorption performance in a low pressure range.

[0251] A glass panel unit (10) according to a tenth aspect includes: a first glass plate (20); a second glass plate (30) facing the first glass plate (20); a frame member (40); an evacuated space (50); and a gas adsorbent (60). The frame member (40) seals the first glass plate (20) and the second glass plate (30). The evacuated space (50) is surrounded by the first glass plate (20), the second glass plate (30) and the frame member (40). The gas adsorbent (60) is placed in the evacuated space (50). The gas adsorbent (60) contains a getter material. The getter material contains a plurality of particles of zeolite crystals and a hydrogenation catalyst.

[0252] The glass panel unit (10) according to the tenth aspect can achieve sufficient adsorption performance in a low pressure range.

[0253] The getter material according to the eleventh aspect contains a plurality of particles of zeolite crystals. Particles having a particle size of 200 nm or more account for more than half of the total weight of the plurality of particles. The plurality of particles has an activatable temperature equal to or lower than 400°C.

[0254] The getter material according to the eleventh aspect can achieve sufficient adsorption performance in a low pressure range.

[0255] The getter material according to the twelfth aspect may be implemented in combination with the eleventh aspect. In the getter material according to the twelfth aspect, particles having a particle diameter of 400 nm or more account for more than half of the total weight of the plurality of particles.

[0256] The getter material according to the twelfth aspect can achieve sufficient adsorption performance in a low pressure range.

[0257] The getter material according to the thirteenth aspect can be implemented in combination with the eleventh aspect or the twelfth aspect. In the getter material according to the thirteenth aspect, particles having a particle diameter of 600 nm or more account for more than half of the total weight of the plurality of particles.

[0258] The getter material according to the thirteenth aspect can achieve sufficient adsorption performance in a low pressure range.

[0259] The getter material according to the fourteenth aspect can be implemented in combination with any one of the eleventh aspect to the thirteenth aspect. In the getter material according to the fourteenth aspect, a particle diameter of each of the plurality of particles is equal to or larger than 1000 nm.

[0260] The getter material according to the fourteenth aspect can achieve sufficient adsorption performance in a low pressure range.

[0261] The getter material according to the fifteenth aspect can be implemented in combination with any one of the eleventh aspect to the fourteenth aspect. In the getter material according to the fifteenth aspect, the plurality of particles are primary particles, and the particle diameter is the shortest width of the plurality of particles.

[0262] The getter material according to the fifteenth aspect can achieve sufficient adsorption performance in a low pressure range.

[0263] The getter material according to the sixteenth aspect may be implemented in combination with any one of the eleventh aspect to the fifteenth aspect. The getter material according to the sixteenth aspect further includes a carbon dioxide adsorbent (other than ceria).

[0264] The getter material according to the sixteenth aspect more easily adsorbs carbon dioxide, and it is possible to achieve sufficient adsorption performance in a low pressure range.

[0265] The getter material according to the seventeenth aspect can be implemented in combination with the sixteenth aspect. In the getter material according to the seventeenth aspect, the carbon dioxide adsorbent includes at least one selected from the group consisting of silicon dioxide, aluminum oxide, and activated carbon.

[0266] The getter material according to the seventeenth aspect more easily adsorbs carbon dioxide, and it is possible to achieve sufficient adsorption performance in a low pressure range.

[0267] The getter material according to the eighteenth aspect may be implemented in combination with any one of the eleventh aspect to the seventeenth aspect. The getter material according to the eighteenth aspect further includes a hydrogenation catalyst.

[0268] The getter material according to the eighteenth aspect can more easily hydrogenate a given compound, and can achieve sufficient adsorption performance in a low pressure range.

[0269] The getter material according to the nineteenth aspect can be implemented in combination with the eighteenth aspect. In the getter material according to the nineteenth aspect, the hydrogenation catalyst is powder.

[0270] The getter material according to the nineteenth aspect can more easily hydrogenate a given compound, and can achieve sufficient adsorption performance in a low pressure range.

[0271] The getter material according to the twentieth aspect can be implemented in combination with the eighteenth aspect or the nineteenth aspect. In the getter material according to the twentieth aspect, the hydrogenation catalyst is supported by a catalyst carrier, and the catalyst carrier includes at least one selected from silica, alumina and activated carbon.

[0272] The getter material according to the twentieth aspect reduces the possibility of desorption of the hydrogenation catalyst by allowing the hydrogenation catalyst to be supported by the catalyst carrier.

[0273] The getter material according to the twenty-first aspect can be implemented in combination with any one of the eleventh aspect to the twentieth aspect. In the getter material according to the twenty-first aspect, the zeolite is a copper ion exchange type zeolite.

[0274] The getter material according to the twenty-first aspect can achieve sufficient adsorption performance.

[0275] A getter material composition according to a twenty-second aspect comprises a getter material and a solvent. The getter material comprises a plurality of particles of zeolite crystals. The plurality of particles have an activatable temperature of 400° C. or less.

[0276] The getter material composition according to the twenty-second aspect enables provision of a gas adsorbent (60) that can achieve sufficient adsorption performance in a low pressure range.

[0277] The getter material composition according to the twenty-third aspect contains a getter material and a solvent. The getter material contains a plurality of particles of zeolite crystals. The plurality of particles include particles having a particle diameter equal to or greater than 200 nm.

[0278] The getter material composition according to the twenty-third aspect enables provision of a gas adsorbent (60) that can achieve sufficient adsorption performance in a low pressure range.

[0279] The getter material composition according to the twenty-fourth aspect can be implemented in combination with the twenty-second aspect or the twenty-third aspect. In the getter material composition according to the twenty-fourth aspect, particles having a particle size of 200 nm or more account for more than half of the total weight of the plurality of particles, and the average particle size of the plurality of particles is equal to or greater than 200 nm.

[0280] The getter material composition according to the twenty-fourth aspect enables provision of a gas adsorbent (60) that can achieve sufficient adsorption performance in a low pressure range.

[0281] The getter material composition according to the twenty-fifth aspect can be implemented in combination with any one of aspects 22 to 24. In the getter material composition according to the twenty-fifth aspect, the solvent includes an organic solvent having a boiling point of 300°C or lower.

[0282] The getter material composition according to the twenty-fifth aspect can reduce the energy required to desorb the organic solvent, thereby making it easier to provide the gas adsorbent (60).

[0283] The getter material composition according to the twenty-sixth aspect can be implemented in combination with any one of the twenty-second aspect to the twenty-fifth aspect. In the getter material composition according to the twenty-sixth aspect, the solvent includes an organic solvent having a cyclic structure.

[0284] The getter material composition according to the twenty-sixth aspect can reduce the energy required to desorb the organic solvent, thereby making it easier to provide the gas adsorbent (60).

[0285] The getter material composition according to the twenty-seventh aspect may be implemented in combination with any one of aspects 22 to 26. In the getter material composition according to the twenty-seventh aspect, the solvent includes an organic solvent having a non-aromatic group.

[0286] The getter material composition according to the twenty-seventh aspect can reduce the energy required to desorb the organic solvent, thereby making it easier to provide the gas adsorbent (60).

[0287] The getter material composition according to the twenty-eighth aspect can be implemented in combination with any one of the twenty-second aspect to the twenty-seventh aspect. The getter material further contains a carbon dioxide adsorbent.

[0288] The getter material composition according to the twenty-eighth aspect makes it easier to provide a gas adsorbent (60) having excellent gas adsorption performance.

[0289] The getter material composition according to the twenty-ninth aspect can be implemented in combination with any one of aspects 22 to 28. The getter material further contains a hydrogenation catalyst.

[0290] The getter material composition according to the twenty-ninth aspect makes it easier to provide a gas adsorbent (60) having excellent gas adsorption performance.

[0291] The method for manufacturing a glass panel unit (10) according to the thirtieth aspect comprises a processing step, an assembling step, a bonding step and an exhaust step. The processing step comprises preparing a getter material composition according to any one of the twenty-second aspect to the twenty-ninth aspect. The assembling step comprises preparing an assembly (100), the assembly (100) comprising a first glass plate (20), a second glass plate (30), a peripheral wall (410) having a frame shape, an internal space (500), a gas adsorbent (60) made of the above-mentioned getter material composition and an exhaust port (700). The bonding step comprises sealingly bonding the first glass plate (20) to the second glass plate (30) by melting the peripheral wall (410). The exhaust step comprises exhausting gas from the internal space (500) through the exhaust port (700) so that the internal space (500) is transformed into an evacuated space (50).

[0292] The thirtieth aspect makes it possible to provide a glass panel unit (10) that can achieve sufficient adsorption performance in a low pressure range.

[0293] According to the thirty-first aspect, the glass panel unit (10) includes: a first glass plate (20); a second glass plate (30) facing the first glass plate (20); a frame member (40); an evacuated space (50); and a gas adsorbent (60). The frame member (40) seals the first glass plate (20) and the second glass plate (30). The evacuated space (50) is surrounded by the first glass plate (20), the second glass plate (30) and the frame member (40). The gas adsorbent (60) is placed in the evacuated space (50). The gas adsorbent (60) contains a getter material. The getter material contains a plurality of particles of zeolite crystals. Particles having a particle size of 200 nm or more account for more than half of the total weight of the plurality of particles. At least one of the softening point, melting point or bondable temperature of the sealant is equal to or lower than 350°C.

[0294] The glass panel unit (10) according to the thirty-first aspect can achieve sufficient adsorption performance in a low pressure range.

[0295] Reference numerals list

[0296] 10 Glass panel units

[0297] 20 First Glass Plate

[0298] 30 Second Glass Plate

[0299] 40 Frame members

[0300] 50 Empty Space

[0301] 60 Gas Adsorbent

Claims

1. A getter material composition comprising a getter material and a solvent, The getter material contains a plurality of particles of zeolite crystals, The zeolite is a copper ion exchange zeolite, Particles having a particle size of 200 nm or more account for more than half of the total weight of the plurality of particles, The solvent includes an organic solvent as a main component.

2. The getter material composition according to claim 1, wherein The average particle size of the plurality of particles is equal to or greater than 200 nm.

3. The getter material composition according to claim 1, wherein The solvent includes an organic solvent having a boiling point of 300° C. or lower as a main component.

4. The getter material composition according to claim 1, wherein The solvent includes an organic solvent having a cyclic structure as a main component.

5. The getter material composition according to claim 1, wherein The solvent includes an organic solvent having a non-aromatic group as a main component.

6. The getter material composition according to claim 1, wherein The solvent includes, as a main component, an organic solvent having a molecular size as large as or larger than the micropore size of the getter material.

7. The getter material composition according to claim 1, wherein The getter material also contains a carbon dioxide adsorbent.

8. The getter material composition according to claim 1, wherein The getter material also contains a hydrogenation catalyst.

9. A method for manufacturing a glass panel unit, the method comprising: A processing step, the processing step comprising preparing a getter material composition as claimed in any one of claims 1 to 8; an assembling step, the assembling step comprising preparing an assembly including a first glass plate, a second glass plate, an outer peripheral wall having a frame shape, an inner space, a gas adsorbent made of the getter material composition, and an exhaust port; a bonding step including sealingly bonding the first glass plate to the second glass plate by melting the peripheral wall; and An exhaust step includes exhausting gas from the internal space through the exhaust port to convert the internal space into an evacuated space.

Citation Information

Patent Citations

  • Insulator including gas adsorbing material

    CN105051442A

  • Gas adsorbent and vacuum heat insulation member provided with the same

    CN106714960A

  • Gas adsorbent, gas adsorbent manufacturing method, and the glass panel unit

    CN107073441A

  • Vacuum heat insulating material, heat insulating structure using vacuum heat insulating material, and home electric appliance, house wall, and transport device using vacuum heat insulating material and heat insulating structure

    WO2019167666A1

  • Getter material, method for manufacturing getter material, method for manufacturing getter-material-containing composition, and method for manufacturing glass panel unit

    WO2019188424A1