Preparation method of macroporous adsorption resin for waste gas treatment

Through the combination of high crosslinking resin and composite molecular sieve, the problem of low adsorption efficiency of large-pore adsorption resin in industrial waste gas treatment is solved, and efficient adsorption and stability improvement of harmful gases and particulate matter is achieved.

CN118874435AInactive Publication Date: 2024-11-01BENGBU TIANXING ION-RESIN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411145087.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing large-pore adsorption resins have problems such as low adsorption efficiency, complex preparation process and difficult to recover when dealing with industrial waste gas, especially the adsorption efficiency of harmful particulate matter and gas pollutants in industrial waste gas is insufficient.

Method used

Carboxymethylcellulose is polymerized with monomers such as diethylenebenzene, 2-chloro-3-(4-hydroxyphenyl)-1-propylene, and a high degree of crosslinking is formed by primary crosslinking and secondary crosslinking reaction. Resin, and a composite molecular sieve was added to increase the specific surface area and pore size, and a waste gas treatment macroporous adsorption resin with high selective adsorption capacity was prepared.

Benefits of technology

The adsorption efficiency of industrial waste gases such as phenol, hydrogen sulfide and dichloromethane is significantly improved, the stability and recovery of resins are enhanced, and the adsorption performance of solid pollutants is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005001989340000031
    Figure BDA0005001989340000031
  • Figure BDA0005001989340000032
    Figure BDA0005001989340000032
  • Figure BDA0005001989340000051
    Figure BDA0005001989340000051
Patent Text Reader

Abstract

The invention discloses a preparation method of macroporous adsorption resin for waste gas treatment, belongs to the technical field of waste gas treatment, and aims to solve the technical problem of low adsorption efficiency of the macroporous adsorption resin on harmful particles and gas pollutants in industrial waste gas in the prior art. The invention relates to a preparation method of macroporous adsorption resin for waste gas treatment. The preparation method comprises the following steps: forming a water phase by carboxymethyl cellulose and water; the preparation method comprises the following steps: carrying out a reaction on 4, 4-dichloromethyl biphenyl, divinylbenzene, 2-chloro-3-(4-hydroxyphenyl)-1-propylene and 4, 4-dichloromethyl biphenyl to obtain secondary cross-linked resin; and dispersing the composite molecular sieve into the secondary cross-linked resin to obtain the macroporous adsorption resin for waste gas treatment. The secondary cross-linked resin has more polar functional groups and higher cross-linking degree, so that the adsorption efficiency and stability of the secondary cross-linked resin are improved; the composite molecular sieve is prepared by using fly ash and silica fume as raw materials and modifying the raw materials with polysilyl modified organosilane, and the composite molecular sieve has high adsorption efficiency on harmful gases such as dichloromethane.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of waste gas treatment, and in particular relates to a method for preparing a macroporous adsorption resin for waste gas treatment. Background Art

[0002] Industrial waste gas refers to the general term for pollutant gases generated and discharged into the air during industrial production, including harmful particulate matter and gaseous pollutants such as phenol, ammonia, hydrogen sulfide, and dichloromethane. These industrial waste gases discharged into the atmosphere will pollute the environment, endanger ecological health, and pose a threat to human safety. For example, dichloromethane has an extremely low boiling point and is very easy to evaporate into the surrounding environment. Excessive inhalation can cause harm to the human body, and dichloromethane will decompose under the action of light to produce highly toxic phosgene. Common process technologies for treating industrial waste gas include adsorption, absorption, condensation, plasma, photocatalysis, and biological methods. Among them, the adsorption method uses porous solid adsorption materials as adsorbents. The adsorption method has the advantages of simple process, high removal rate, low energy consumption, and no secondary pollution.

[0003] Common adsorption materials include inorganic adsorption materials and organic adsorption materials; adsorption resins, as common organic adsorption materials, specifically include gel-type adsorption resins, macroporous adsorption resins, ultra-high cross-linked adsorption resins, etc.; macroporous adsorption resins are a type of adsorption resins with good macroporous network structure and no exchange groups, mainly prepared with styrene, divinylbenzene, etc. as raw materials; among them, macroporous adsorption resins have the advantages of high adsorption capacity, good adsorption selectivity and large wall surface area.

[0004] Patent application CN109180848A discloses a high-stability hydrogen-bonded hydrophilic macroporous adsorption resin and a method for treating hydrogen peroxide tail gas. Styrene, divinylbenzene, methyl acrylate, and benzene are used as polymerization monomers, and macroporous resin balls are prepared by suspension polymerization; the macroporous resin balls are then subjected to chloromethylation reaction with chloromethyl ether to obtain chlorine balls; the chlorine balls are then subjected to Friedel-Crafts crosslinking reaction with phenolic compounds to prepare hydrogen-bonded hydrophilic macroporous adsorption resin. The above-mentioned prior art modifies the macroporous resin balls to have ester bonds and hydroxyl groups, thereby improving the adsorption efficiency of the prepared macroporous adsorption resin for hydrogen peroxide and xylene waste gas. However, compared with inorganic adsorption materials, macroporous adsorption resins have the defects of complex preparation process, difficult recovery, and low adsorption efficiency for harmful waste gas when adsorbing industrial waste gas; in addition, how to further improve the adsorption efficiency of macroporous adsorption resins for solid pollutants in industrial waste gas is also a technical problem that needs to be solved urgently.

[0005] In view of the technical defects in this aspect, a solution is now proposed. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing a macroporous adsorption resin for waste gas treatment, so as to solve the technical problem in the prior art that the macroporous adsorption resin has low adsorption efficiency for harmful particles in industrial waste gas and low adsorption efficiency for gaseous pollutants.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A method for preparing a macroporous adsorption resin for waste gas treatment comprises the following steps:

[0009] S1, carboxymethyl cellulose and deionized water are mixed and stirred at 50° C. until the carboxymethyl cellulose is completely dissolved in the deionized water to obtain an aqueous phase;

[0010] S2, 55%wt of divinylbenzene, 2-chloro-3-(4-hydroxyphenyl)-1-propylene, a mixed porogen and an initiator are mixed and stirred to obtain a mixed monomer liquid; the mixed monomer liquid is transferred to an aqueous phase, stirred and dispersed at 25°C until the particle size is uniform, and then reacted at 70-80°C for 10-12h to perform a primary polymerization to obtain a product; the product is subjected to a post-process treatment to obtain a primary cross-linked resin;

[0011] Under the action of an initiator, divinylbenzene and 2-chloro-3-(4-hydroxyphenyl)-1-propylene undergo addition polymerization to form polymer segments; a mixed porogen is used to adjust the specific surface area and pore size of the prepared primary cross-linked resin, and the invention uses a mixture of a good solvent having a solubility coefficient similar to that of the polymerized monomer and a non-good solvent having a solubility coefficient greatly different from that of the polymer as the mixed porogen; in addition, an aqueous solution of carboxymethyl cellulose is used as an aqueous phase, and the above-mentioned monomers undergo addition polymerization in the aqueous phase, which is conducive to forming a stable colloidal liquid, and the aqueous phase plays a role in promoting cross-linking in the cross-linking reaction of the resin; the product after the monomer polymerization is subjected to a post-process treatment to remove the porogen remaining in the pores of the product, so as to prepare a product primary cross-linked resin.

[0012] The reaction principle of preparing a primary cross-linked resin by addition polymerization of divinylbenzene and 2-chloro-3-(4-hydroxyphenyl)-1-propylene monomer is as follows:

[0013]

[0014] S3, adding 4,4-dichloromethylbiphenyl to dichloroethane to obtain a 4,4-dichloromethylbiphenyl solution; then adding the 4,4-dichloromethylbiphenyl solution to the primary cross-linked resin, mixing and stirring at 100-200 r / min for 30-60 min at room temperature to obtain a mixture; adding anhydrous aluminum chloride to the mixture at 0-5°C, stirring evenly, heating to 60-80°C and reacting for 3-4h, performing secondary polymerization, and obtaining a secondary cross-linked resin;

[0015] 4,4-Dichloromethylbiphenyl is used as a halogenated hydrocarbon, and the prepared primary cross-linked resin is used as an aromatic compound. Under the action of anhydrous aluminum chloride as an acid catalyst, a nucleophilic substitution reaction occurs to prepare a secondary cross-linked resin.

[0016] The reaction formula of 4,4-dichloromethylbiphenyl reacting with a primary cross-linking resin to obtain a secondary cross-linking resin is as follows:

[0017]

[0018] S4. The composite molecular sieve is evenly dispersed in the secondary cross-linked resin to obtain a mixture; the mixture is post-processed and sieved to obtain particles with a particle size of 0.315-1.25 mm, which is the macroporous adsorption resin for waste gas treatment.

[0019] Furthermore, in step S1, the dosage ratio of carboxymethyl cellulose and deionized water is 1-2g:200g; in step S2, the mixed pore-forming agent includes ethanol and methyl isobutyl carbinol, and the initiator is dibenzoyl peroxide; the dosage ratio of divinylbenzene, 2-chloro-3-(4-hydroxyphenyl)-1-propylene, ethanol, methyl isobutyl carbinol and initiator is 60-70g:50-60g:50mL:50mL:1-2g; the post-processing step includes: distilling the product under reduced pressure at 100-110°C until the oil phase liquid surface of the product maintains a constant volume, then stopping the distillation to obtain a primary cross-linked resin.

[0020] Furthermore, in step S3, the dosage ratio of 4,4-dichloromethylbiphenyl and dichloroethane is 10-20mL:50mL; the catalyst is anhydrous aluminum chloride, and the dosage ratio of 4,4-dichloromethylbiphenyl solution, primary cross-linked resin and catalyst is 60-70mL:150-200g:3-5g; the rotation speed of the mixture and the catalyst is 100-200r / min, and the mixing and stirring time is 30-60min; in step S4, the post-processing step includes: washing the secondary cross-linked resin with acetone, 0.5mol / L HCl solution and deionized water in sequence, and then vacuum drying at 80°C to constant weight to obtain a composite resin.

[0021] Furthermore, in step S4, the method for preparing the composite molecular sieve comprises the following steps:

[0022] A1. Fly ash and silica fume are mixed and ball-milled to obtain inorganic powder; the inorganic powder is sieved through a 100-mesh sieve and then added to a micro-granulator for granulation to obtain spherical inorganic powder;

[0023] A2, spherical inorganic powder and 1 mol / L H2SO4 solution are mixed, reacted, and filtered to obtain acidified spherical inorganic powder; the acidified spherical inorganic powder is added to a steam curing kettle for steam curing to obtain a polyhydroxy molecular sieve;

[0024] A3. Mix the liquid modified organosilane and the polyhydroxy molecular sieve, shake well, react at 60-70° C. for 4-5 hours, and then filter to obtain a solid; dry the solid to obtain a composite molecular sieve.

[0025] The present invention uses fly ash and silica fume as raw materials for preparing a composite molecular sieve; the present invention pre-granulates inorganic powder and then performs high-temperature steam curing to prepare zeolite; in order to increase the hydroxyl content in the prepared composite molecular sieve, the present invention pre-acidifies the spherical inorganic powder; and adopts a liquid phase silanization method to load organic silane onto the surface of a multi-hydroxy molecular sieve to prepare the composite molecular sieve.

[0026] Furthermore, in step A1, the usage ratio of fly ash and silica fume is 80-90g:10-20g; the rotation speed of the granulator is 200-300r / min, and the granulation time is 30-60min.

[0027] Furthermore, in step A2, the dosage ratio of spherical inorganic powder and H2SO4 solution is 100-110g:15-20mL; the reaction temperature is 30-40°C, and the reaction time is 1-2h; the steaming temperature is 190-210°C, and the steaming time is 24-36h; in step A3, the dosage ratio of liquid-modified organic silane and polyhydroxy molecular sieve is 80-100mL:20-30g; the solid vacuum drying temperature is 100-120°C, and the vacuum drying time is 1-2h.

[0028] Furthermore, the preparation method of the liquid phase modified organosilane comprises the following steps:

[0029] B1, trimethylsilyl chloride, ether and 4-chlorophenylmagnesium bromide are mixed and reacted at 25-30° C. for 2-3 hours to obtain a product; the product is filtered to obtain liquid phase (2-chlorophenyl)-trimethylsilane;

[0030] Diethyl ether is used as a solvent, 4-chlorophenylmagnesium bromide is used as a chloroalkyl Grignard reagent, and reacts with trimethylsilyl chloride to prepare chloroalkylsilane (2-chlorophenyl)-trimethylsilane.

[0031] The reaction mechanism of 4-chlorophenylmagnesium bromide and trimethylsilyl chloride is as follows:

[0032]

[0033] B2, mixing liquid (2-chlorophenyl)-trimethylsilane and methyltri(cyclohexylamino)silane, and performing reflux reaction at 70-80° C. for 2-3 hours to obtain modified organosilane;

[0034] The reaction formula of preparing modified organosilane by reacting (2-chlorophenyl)-trimethylsilane with methyltri(cyclohexylamino)silane is as follows:

[0035]

[0036] B3. Shake the modified organosilane and polyhydroxy molecular sieve evenly, react at 60-70°C for 4-5h, and then filter to obtain a solid; vacuum dry the solid to obtain a composite molecular sieve.

[0037] Furthermore, in step B1, the amount ratio of trimethylchlorosilane, ether and 4-chlorophenylmagnesium bromide is 30-40g:100mL:50-60g; in step B2, the amount ratio of (2-chlorophenyl)-trimethylsilane and methyltri(cyclohexylamino)silane is 60-100g:20-30g; in step B3, the amount ratio of modified organic silane and polyhydroxy molecular sieve is 80-100mL:20-30g; the temperature of solid vacuum drying is 100-120°C, and the time of solid vacuum drying is 1-2h.

[0038] The present invention has the following beneficial effects:

[0039] 1. The macroporous adsorption resin prepared by the present invention has a high cross-linking property; divinylbenzene and 2-chloro-3-(4-hydroxyphenyl)-1-propylene monomer undergo a primary cross-linking reaction to prepare a primary cross-linked resin containing chlorine polar functional groups; the primary cross-linked resin and 4,4-dichloromethylbiphenyl undergo a nucleophilic substitution reaction again to prepare a secondary cross-linked resin containing more polar functional groups, a higher cross-linking degree and a larger molecular weight; the secondary cross-linked resin has a higher selective adsorption efficiency for phenol and hydrogen sulfide in industrial waste gas.

[0040] 2. The present invention adds a certain amount of composite molecular sieve when preparing the secondary cross-linked resin; the composite molecular sieve uses fly ash and silica ash as the main raw materials; fly ash is rich in Al2O3 and SiO2, and silica ash is mainly composed of amorphous silicon dioxide, Fe3O4, Al2O3, CaO and other metal compounds, and the above raw materials are cheap and easy to obtain; the raw materials are prepared into spherical particles, which helps to increase their specific surface area; the spherical inorganic powder is acidified with sulfuric acid to increase its hydroxyl content and obtain a polyhydroxy molecular sieve. (2-Chlorophenyl)-trimethylsilane and methyltri(cyclohexylamino)silane react to prepare a polysilane-modified organic silane; the increase in the number of active sites of the polyhydroxy molecular sieve and the modified organic silane is conducive to improving their own modification degree, and the compatibility of the composite molecular sieve and the secondary cross-linked resin is also improved; the composite molecular sieve prepared by the present invention has a high adsorption efficiency for industrial waste gases such as dichloromethane. DETAILED DESCRIPTION

[0041] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Example 1

[0043] This embodiment provides a method for preparing a composite molecular sieve for use as a macroporous adsorption resin for waste gas treatment, comprising the following steps:

[0044] A1. Preparation of polyhydroxy molecular sieves

[0045] 1. Mix 80g of fly ash and 10g of silica fume, add them to a ball mill, grind them, and pass them through a 100-mesh sieve to obtain inorganic powder; then add the inorganic powder to a micro-granulator for granulation. The speed of the micro-granulator drum is 200r / min, and the granulation time is 20min to obtain spherical inorganic powder.

[0046] 2. Add 100 g of spherical inorganic powder and 15 mL of 1 mol / L H2SO4 solution into a 250 mL beaker, mix well, react at 30 ° C for 1 hour, and then filter to obtain acidified spherical inorganic powder; send the acidified spherical inorganic powder into a steam curing kettle, steam cure at 190 ° C for 24 hours to obtain a polyhydroxy molecular sieve.

[0047] A2. Preparation of modified organosilane

[0048] 1. Add 30 g of trimethylchlorosilane and 100 mL of ether into a 250 mL three-necked flask, then add 50 g of 4-chlorophenylmagnesium bromide, transfer the three-necked flask to a water bath, and react in a water bath at 25 ° C for 2 h accompanied by mechanical stirring at 100 r / min to obtain the product; filter the product to obtain liquid (2-chlorophenyl)-trimethylsilane.

[0049] 2. Add 6 g of liquid (2-chlorophenyl)-trimethylsilane and 20 g of methyltri(cyclohexylamino)silane into a 250 mL three-necked flask, set a reflux stirring device on the three-necked flask, and reflux at 70° C. for 2 h to obtain modified organosilane.

[0050] 3. Add 80 mL of liquid-modified organosilane and 20 g of polyhydroxy molecular sieve into a 250 mL round-mouth flask and shake well; then transfer the round-mouth flask to a water bath, react at 60 ° C for 4 hours, and then filter to obtain a solid; the solid is placed in an oven at 100 ° C for 1 hour to obtain a composite molecular sieve.

[0051] Example 2

[0052] This embodiment provides a method for preparing a composite molecular sieve for use as a macroporous adsorption resin for waste gas treatment, comprising the following steps:

[0053] A1. Preparation of polyhydroxy molecular sieves

[0054] 1. Mix 85g of fly ash and 15g of silica fume, add them to a ball mill, grind them, and pass them through a 100-mesh sieve to obtain inorganic powder; then add the inorganic powder to a micro-granulator for granulation. The speed of the micro-granulator drum is 250r / min, and the granulation time is 40min to obtain spherical inorganic powder.

[0055] 2. Add 105 g of spherical inorganic powder and 16 mL of 1 mol / L H2SO4 solution into a 250 mL beaker, mix well, react at 35 ° C for 1.5 h, and then filter to obtain acidified spherical inorganic powder; send the acidified spherical inorganic powder into a steam-curing kettle and steam-cure at 200 ° C for 30 h to obtain a polyhydroxy molecular sieve.

[0056] A2. Preparation of modified organosilane

[0057] 1. Add 36 g of trimethylchlorosilane and 100 mL of ether into a 250 mL three-necked flask, then add 55 g of 4-chlorophenylmagnesium bromide, transfer the three-necked flask to a water bath, and react in a water bath at 26 ° C for 2.5 h accompanied by mechanical stirring at 100 r / min to obtain the product; the product is distilled under reduced pressure to obtain liquid (2-chlorophenyl)-trimethylsilane.

[0058] 2. Add 80 g of liquid (2-chlorophenyl)-trimethylsilane and 25 g of methyltri(cyclohexylamino)silane into a 250 mL three-necked flask, set a reflux stirring device on the three-necked flask, and reflux for reaction at 75° C. for 2.6 h to obtain modified organosilane.

[0059] 3. Add 90 mL of liquid-modified organosilane and 25 g of polyhydroxy molecular sieve into a 250 mL round-mouth flask and shake well; then transfer the round-mouth flask to a water bath, react at 66 ° C for 4.3 hours, and then filter to obtain a solid; place the solid in an oven at 110 ° C for 1.3 hours to obtain a composite molecular sieve.

[0060] Example 3

[0061] This embodiment provides a method for preparing a composite molecular sieve for use as a macroporous adsorption resin for waste gas treatment, comprising the following steps:

[0062] A1. Preparation of polyhydroxy molecular sieves

[0063] 1. Mix 90g of fly ash and 20g of silica fume, add them to a ball mill, grind them, and pass them through a 100-mesh sieve to obtain inorganic powder; then add the inorganic powder to a micro-granulator for granulation. The speed of the micro-granulator drum is 300r / min, and the granulation time is 60min to obtain spherical inorganic powder.

[0064] 2. Add 110 g of spherical inorganic powder and 20 mL of 1 mol / L H2SO4 solution into a 250 mL beaker, mix well, react at 40 ° C for 2 h, and then filter to obtain acidified spherical inorganic powder; send the acidified spherical inorganic powder into a steam-curing kettle, steam-cured at 210 ° C for 36 h to obtain a polyhydroxy molecular sieve.

[0065] A2. Preparation of modified organosilane

[0066] 1. Add 40 g of trimethylchlorosilane and 100 mL of ether into a 250 mL three-necked flask, then add 60 g of 4-chlorophenylmagnesium bromide, transfer the three-necked flask to a water bath, and react in a water bath at 30 ° C for 3 h accompanied by mechanical stirring at 100 r / min to obtain the product; the product is distilled under reduced pressure to obtain liquid (2-chlorophenyl)-trimethylsilane.

[0067] 2. Add 100 g of liquid (2-chlorophenyl)-trimethylsilane and 30 g of methyltri(cyclohexylamino)silane into a 250 mL three-necked flask, set a reflux stirring device on the three-necked flask, and reflux at 80° C. for 3 h to obtain modified organosilane.

[0068] 3. Add 100 mL of liquid-modified organosilane and 30 g of polyhydroxy molecular sieve into a 250 mL round-mouth flask and shake well; then transfer the round-mouth flask to a water bath, react at 70 ° C for 5 hours, and then filter to obtain a solid; place the solid in an oven at 120 ° C for 2 hours to obtain a composite molecular sieve.

[0069] Example 4

[0070] This embodiment provides a method for preparing a macroporous adsorption resin for waste gas treatment, comprising the following steps:

[0071] S1. Weigh 1 g of hydroxymethyl cellulose and 200 g of deionized water into a 500 mL beaker, transfer the beaker to a water bath, and mix and stir at 50° C. until the hydroxymethyl cellulose is completely dissolved in the deionized water to obtain an aqueous phase.

[0072] S2. Add 60 g of 55% wt divinylbenzene, 50 g of 2-chloro-3-(4-hydroxyphenyl)-1-propylene, 50 mL of good solvent ethanol, 50 mL of non-good solvent methyl isobutyl carbinol and 1 g of initiator dibenzoyl peroxide into a beaker, mix and stir for 30 minutes at a rate of 5 minutes to obtain a mixed monomer liquid; transfer the mixed monomer liquid to the aqueous phase, stir and disperse at 25°C until the particle size is uniform, then transfer the beaker to a water bath, react at 70°C for 10 hours to obtain a product; perform reduced pressure distillation on the product at 100°C until the oil phase liquid level of the product remains unchanged, then stop distillation to obtain a primary cross-linked resin.

[0073] S3. Add 10 mL of 4,4-dichloromethylbiphenyl to 50 mL of dichloroethane to obtain a 4,4-dichloromethylbiphenyl solution; then add 60 mL of the 4,4-dichloromethylbiphenyl solution to 150 g of the primary cross-linked resin, stir at 100 r / min for 30 min at room temperature, and stir evenly to obtain a mixture. Add 3 g of anhydrous aluminum chloride to the mixture at 0°C in an ice water bath and stir evenly; then transfer the beaker to a water bath, heat to 60°C and react for 3 hours to obtain a secondary cross-linked resin.

[0074] S4. Add the composite molecular sieve prepared in Example 1 to the secondary cross-linked resin, mix and stir at 100 r / min for 30 min to uniformly disperse the composite molecular sieve in the secondary cross-linked resin to obtain a mixture; wash the mixture with acetone, 0.5 mol / L HCl solution and deionized water in sequence, and then vacuum dry it at 80°C to constant weight, and then sieve to obtain particles with a particle size of 0.315-1.25 mm, which is the macroporous adsorption resin for waste gas treatment.

[0075] Example 5

[0076] This embodiment provides a method for preparing a macroporous adsorption resin for waste gas treatment, comprising the following steps:

[0077] S1. Weigh 1.7 g of hydroxymethyl cellulose and 200 g of deionized water into a 500 mL beaker, transfer the beaker to a water bath, and mix and stir at 50° C. until the hydroxymethyl cellulose is completely dissolved in the deionized water to obtain an aqueous phase.

[0078] S2, add 66g of 55%wt divinylbenzene, 55g of 2-chloro-3-(4-hydroxyphenyl)-1-propylene, 50mL of good solvent ethanol, 50mL of non-good solvent methyl isobutyl carbinol and 2g of initiator dibenzoyl peroxide into a beaker, mix and stir for 50min at 8min to obtain a mixed monomer liquid; transfer the mixed monomer liquid to the water phase, stir and disperse at 25°C until the particle size is uniform, then transfer the beaker to a water bath, react at 75°C for 11h to obtain a product. The product is subjected to reduced pressure distillation at 105°C until the oil phase liquid level of the product remains unchanged, then stop distillation to obtain a primary cross-linked resin.

[0079] S3. Add 150 mL of 4,4-dichloromethylbiphenyl to 50 mL of dichloroethane to obtain a 4,4-dichloromethylbiphenyl solution; then add 63 mL of the 4,4-dichloromethylbiphenyl solution to 180 g of the primary cross-linked resin, stir at room temperature at 160 r / min for 50 min, and stir evenly to obtain a mixture. Add 4 g of anhydrous aluminum chloride to the mixture at 3°C ​​in an ice-water bath and stir evenly; then transfer the beaker to a water bath, heat to 70°C and react for 3.3 hours to obtain a secondary cross-linked resin.

[0080] S4. Add the composite molecular sieve prepared in Example 2 to the secondary cross-linked resin, mix and stir at 150 r / min for 50 min to uniformly disperse the composite molecular sieve in the secondary cross-linked resin to obtain a mixture; wash the mixture with acetone, 0.5 mol / L HCl solution, and deionized water in sequence, and then vacuum dry it at 80°C to constant weight, and then sieve to obtain particles with a particle size of 0.315-1.25 mm, which is the macroporous adsorption resin for exhaust gas treatment.

[0081] Example 6

[0082] This embodiment provides a method for preparing a macroporous adsorption resin for waste gas treatment, comprising the following steps:

[0083] S1. Weigh 2 g of hydroxymethyl cellulose and 200 g of deionized water into a 500 mL beaker, transfer the beaker to a water bath, and mix and stir at 50° C. until the hydroxymethyl cellulose is completely dissolved in the deionized water to obtain an aqueous phase.

[0084] S2, add 70g of 55%wt divinylbenzene, 60g of 2-chloro-3-(4-hydroxyphenyl)-1-propylene, 50mL of good solvent ethanol, 50mL of non-good solvent methyl isobutyl carbinol and 2g of initiator dibenzoyl peroxide into a beaker, mix and stir for 60min for 10min to obtain a mixed monomer liquid; transfer the mixed monomer liquid to the water phase, stir and disperse at 25°C until the particle size is uniform, then transfer the beaker to a water bath, react at 80°C for 12h to obtain a product. The product is subjected to reduced pressure distillation at 110°C until the oil phase liquid level of the product remains unchanged, then stop distillation to obtain a primary cross-linked resin.

[0085] S3. Add 20 mL of 4,4-dichloromethylbiphenyl to 50 mL of dichloroethane to obtain a 4,4-dichloromethylbiphenyl solution; then add 70 mL of the 4,4-dichloromethylbiphenyl solution to 200 g of the primary cross-linked resin, stir at 200 r / min for 60 min at room temperature, and stir evenly to obtain a mixture. Add 5 g of anhydrous aluminum chloride to the mixture at 5°C in an ice-water bath and stir evenly; then transfer the beaker to a water bath, heat to 80°C and react for 4 hours to obtain a secondary cross-linked resin.

[0086] S4. Add the composite molecular sieve prepared in Example 3 to the secondary cross-linked resin, mix and stir at 200 r / min for 60 min to uniformly disperse the composite molecular sieve in the secondary cross-linked resin to obtain a mixture; wash the mixture with acetone, 0.5 mol / L HCl solution, and deionized water in sequence, and then vacuum dry it at 80°C to constant weight, and then sieve to obtain particles with a particle size of 0.315-1.25 mm, which is the macroporous adsorption resin for waste gas treatment.

[0087] Comparative Example 1

[0088] The difference between this comparative example and Example 6 is that step A3 is eliminated, and the primary cross-linked resin is used instead of the secondary cross-linked resin to prepare a macroporous adsorption resin for waste gas treatment.

[0089] Comparative Example 2

[0090] The difference between this comparative example and Example 6 is that in step A4, when preparing the composite molecular sieve, liquid phase (2-chlorophenyl)-trimethylsilane is used to replace the modified organic silane to prepare the composite molecular sieve.

[0091] Comparative Example 3

[0092] The difference between this comparative example and Example 6 is that in step A4, no composite molecular sieve is added to the secondary cross-linked resin, and the secondary cross-linked resin is used as the macroporous adsorption resin for waste gas treatment.

[0093] Performance testing:

[0094] 1. Prepare 25 mL of 100 mg / L phenol solution and add it to a 100 mL conical flask. Then weigh 0.5 g of the macroporous adsorption resin for waste gas treatment prepared in Examples 4-6 and add it to the conical flask, seal it with a sealing film, and then place the conical flask in a constant temperature water bath oscillator. After oscillating at 15°C for 24 hours, take it out to obtain an adsorption liquid; use a disposable dropper to take out a certain amount of adsorption liquid into a test tube, measure the absorbance, and calculate the adsorption amount. Then prepare 100 mg / L hydrogen sulfide solution and 100 mg / L ammonia water respectively, repeat the above operation, measure the absorbance, calculate the adsorption amount, and after unit conversion, the adsorption amount is expressed in mmol / L.

[0095] The adsorption amount is calculated as follows:

[0096] q=(C0-Ce)V / 1000m(1-X)

[0097] Where, q is the adsorption amount (mmol / L), c0 and c e are the concentrations of the adsorbate solution before and after adsorption (mmol / L), V is the volume of the adsorption solution (mL), m is the mass of the macroporous adsorption resin for waste gas treatment (g), and X is the water content of the macroporous adsorption resin for waste gas treatment.

[0098] 2. Carry out the adsorption experiment of dichloromethane in a three-stage temperature-controlled micro fixed-bed reactor; the adsorption column is a quartz tube with an outer diameter of 10mm, a wall thickness of 1mm, and a height of 50cm. Quartz wool is respectively installed at the upper and lower ends of the adsorbent to fix it. Nitrogen and dichloromethane gas are mixed at a certain rate ratio through a gas flow controller to make the dichloromethane concentration 7.583g / cm3. Dynamic adsorption is carried out at room temperature, and the saturated adsorption amount of dichloromethane is recorded; wherein, the flow rate is 50mL / min, and the mass of the adsorbent is 0.5g; gas chromatography is then used to detect the concentration of dichloromethane in the tail gas. The adsorbent is specifically the macroporous adsorption resin for waste gas treatment prepared in Examples 4-6 and Comparative Examples 1-3. The specific test results are shown in Table 1:

[0099] Table 1. Test data of each test sample

[0100]

[0101] According to the results in Table 1, the adsorption resins for waste gas treatment prepared in Examples 4-6 of the present invention have a high adsorption capacity for harmful components in industrial waste gas such as phenol, hydrogen sulfide, ammonia water, and dichloromethane. However, in Comparative Example 1, the primary cross-linked resin is used instead of the secondary cross-linked resin, which reduces the number of polar functional groups of the prepared adsorption resin and the cross-linking degree of the adsorption resin, thereby reducing the adsorption efficiency of industrial waste gas components such as phenol, hydrogen sulfide, ammonia water, and dichloromethane to varying degrees.

[0102] In Comparative Example 2, the organosilane was not modified when preparing the composite molecular sieve, resulting in poor compatibility between the prepared composite molecular sieve and the secondary cross-linked resin, which is not conducive to improving the adsorption efficiency of the prepared macroporous adsorption resin for waste gas treatment for harmful gases such as hydrogen sulfide and dichloromethane.

[0103] In Comparative Example 3, the prepared secondary cross-linked resin does not contain the composite molecular sieve, which not only reduces the adsorption efficiency of hydrogen sulfide and dichloromethane gases, but also reduces the adsorption efficiency of the prepared macroporous adsorption resin for other organic industrial waste gas components.

[0104] The above contents are merely examples and explanations of the structure of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

[0105] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0106] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a macroporous adsorption resin for waste gas treatment, characterized in that: The following steps are involved: S1, carboxymethyl cellulose and deionized water are mixed and stirred at 50° C. until the carboxymethyl cellulose is completely dissolved in the deionized water to obtain an aqueous phase; S2, 55%wt of divinylbenzene, 2-chloro-3-(4-hydroxyphenyl)-1-propylene, a mixed pore-forming agent and an initiator are uniformly mixed to obtain a mixed monomer liquid; the mixed monomer liquid is transferred to an aqueous phase, stirred and dispersed at 25°C until the particle size is uniform, and then a primary polymerization is carried out at 70-80°C for 10-12h to obtain a product; the product is subjected to a post-process treatment to obtain a primary cross-linked resin; S3, adding 4,4-dichloromethylbiphenyl to dichloroethane to obtain a 4,4-dichloromethylbiphenyl solution; then adding the 4,4-dichloromethylbiphenyl solution to a primary cross-linked resin, mixing evenly to obtain a mixture; adding a catalyst to the mixture at 0-5°C, mixing and stirring, and then heating to 60-80°C for secondary polymerization for 3-4h to obtain a secondary cross-linked resin; S4. The composite molecular sieve is evenly dispersed in the secondary cross-linked resin to obtain a mixture; the mixture is post-processed and sieved to obtain particles with a particle size of 0.315-1.25 mm, which is the macroporous adsorption resin for waste gas treatment.

2. The method for preparing a macroporous adsorption resin for waste gas treatment according to claim 1, characterized in that: In step S1, the dosage ratio of carboxymethyl cellulose and deionized water is 1-2g:200g; in step S2, the mixed pore-forming agent includes ethanol and methyl isobutyl carbinol, and the initiator is dibenzoyl peroxide; the dosage ratio of divinylbenzene, 2-chloro-3-(4-hydroxyphenyl)-1-propylene, ethanol, methyl isobutyl carbinol and initiator is 60-70g:50-60g:50mL:50mL:1-2g; the post-processing step includes: performing reduced pressure distillation on the product at 100-110°C until the oil phase liquid surface of the product maintains a constant volume, and then stopping the distillation to obtain a primary cross-linked resin.

3. The method for preparing a macroporous adsorption resin for waste gas treatment according to claim 1, characterized in that: In step S3, the dosage ratio of 4,4-dichloromethylbiphenyl and dichloroethane is 10-20mL:50mL; the catalyst is anhydrous aluminum chloride, and the dosage ratio of 4,4-dichloromethylbiphenyl solution, primary cross-linking resin and catalyst is 60-70mL:150-200g:3-5g; the rotation speed of the mixture and the catalyst is 100-200r / min, and the mixing time is 30-60min; In step S4, the post-processing step includes: washing the secondary cross-linked resin with acetone, 0.5 mol / L HCl solution and deionized water in sequence, and then vacuum drying at 80° C. to constant weight to obtain a composite resin.

4. The method for preparing a macroporous adsorption resin for waste gas treatment according to claim 1, characterized in that: In step S4, the method for preparing the composite molecular sieve comprises the following steps: A1. Fly ash and silica fume are mixed, ball-milled, and passed through a 100-mesh sieve to obtain an inorganic powder; the inorganic powder is added to a micro-granulator for granulation to obtain a spherical inorganic powder; A2, spherical inorganic powder and 1 mol / L H2SO4 solution are mixed, reacted, and filtered to obtain acidified spherical inorganic powder; the acidified spherical inorganic powder is added to a steam curing kettle for steam curing to obtain a polyhydroxy molecular sieve; A3. Mix the liquid modified organosilane and the polyhydroxy molecular sieve, shake well, react at 60-70° C. for 4-5 hours, and filter to obtain a solid; vacuum dry the solid to obtain a composite molecular sieve.

5. The method for preparing a macroporous adsorption resin for waste gas treatment according to claim 4, characterized in that: In step A1, the usage ratio of fly ash and silica fume is 80-90g:10-20g; the rotation speed of the granulator is 200-300r / min, and the granulation time is 30-60min.

6. The method for preparing a macroporous adsorption resin for waste gas treatment according to claim 4, characterized in that: In step A2, the dosage ratio of spherical inorganic powder and H2SO4 solution is 100-110g:15-20mL; the reaction temperature is 30-40°C and the reaction time is 1-2h; the steaming temperature is 190-210°C and the steaming time is 24-36h; in step A3, the dosage ratio of liquid-modified organosilane and polyhydroxy molecular sieve is 80-100mL:20-30g; the temperature of solid vacuum drying is 100-120°C and the vacuum drying time is 1-2h.

7. The method for preparing a macroporous adsorption resin for waste gas treatment according to claim 4, characterized in that: The preparation method of liquid phase modified organosilane comprises the following steps: B1, trimethylsilyl chloride, ether and 4-chlorophenylmagnesium bromide are mixed and reacted at 25-30° C. for 2-3 hours to obtain a product; the product is filtered to obtain a liquid phase (2-chlorophenyl)-trimethylsilane; B2, mixing liquid (2-chlorophenyl)-trimethylsilane and methyltri(cyclohexylamino)silane, and performing reflux reaction at 70-80° C. for 2-3 hours to obtain modified organosilane; B3. Shake the modified organosilane and polyhydroxy molecular sieve evenly, react at 60-70°C for 4-5h, and then filter to obtain a solid; vacuum dry the solid to obtain a composite molecular sieve.

8. The method for preparing a macroporous adsorption resin for waste gas treatment according to claim 7, characterized in that: In step B1, the amount ratio of trimethylchlorosilane, ether and 4-chlorophenylmagnesium bromide is 30-40g:100mL:50-60g; in step B2, the amount ratio of (2-chlorophenyl)-trimethylsilane and methyltri(cyclohexylamino)silane is 60-100g:20-30g; in step B3, the amount ratio of modified organic silane and polyhydroxy molecular sieve is 80-100mL:20-30g; the temperature of solid vacuum drying is 100-120°C, and the time of solid vacuum drying is 1-2h.