Mineral processing technology for recovering low-grade lepidolite
By using a combined collector for flotation and selection of lithium mica under alkaline conditions, the low recovery rate and high cost problems caused by desilting and acid addition in lithium mica ore dressing are solved, and the efficient recovery of low-grade lithium mica is achieved. Process flow.
Patent Information
- Application Number
- CN202411250900.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-09-06
AI Technical Summary
The desludge and acid addition processes in the existing lithium mica ore dressing process lead to low lithium recovery and concentrate grade, high production costs and easy corrosion of the equipment, making it difficult to recycle low-grade lithium mica economically and effectively.
Lithium mica flotation and selection are performed to reduce amygest ganglite and gypsum The heterophase condensation of lithium mica improves the recovery rate and concentrate grade of lithium mica, and avoids desilting and acid use.
It improves the recovery rate and concentrate grade of lithium mica, simplifies the ore dressing process, reduces the dosage and production costs of drugs, and avoids equipment corrosion and environmental pollution.
Smart Images

Figure CN118874672A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lepidolite beneficiation, and in particular to a beneficiation process for recovering low-grade lepidolite. Background Art
[0002] With the rapid development of new energy vehicles, energy storage, medicine, atomic energy industry and other fields, the global demand for lithium consumption is growing rapidly, and the extraction of lithium from different lithium-containing ores has become a research hotspot. Lithium-containing ores mainly include spodumene, lepidolite, pyroxenite and petalite. Among them, lepidolite is not a mainstream commercial lithium resource because the concentrate produced by mineral processing has low lithium content, which leads to increased downstream smelting costs. However, due to the large reserves of lepidolite, with the current surge in demand for lithium, the extraction of lithium from lepidolite is increasingly valued.
[0003] At present, the conventional lithium mica beneficiation process includes grinding, desludging, desulfurization, lithium flotation and other processes. The beneficiation process flow chart is as follows: Figure 1 As shown. When conducting lithium mica beneficiation based on this method, physical desludging or flotation desludging is required first, and the loss of lithium during the desludging process is large, resulting in a low lithium recovery rate. Before lithium flotation, it is necessary to adjust the pH value of the pulp to about 4-5 by adding acid, and then add a cationic collector for flotation. In the lithium mica selection process after flotation, it is necessary to continue to add acid to adjust the pH value to 2-3. After 2-4 times of selection, the lithium mica concentrate can be finally obtained. This method requires the use of a large amount of acid, which not only has high production costs, but also easily corrodes the flotation equipment. The large amount of acidic water produced also poses a great challenge to safety and environmental protection. In addition, a large amount of foam will be generated during the flotation process, resulting in an unstable flotation process, frequent troughing, and affecting the flotation of lithium mica. The final recovery rate and concentrate grade are both low. Especially for low-grade lithium mica, it is difficult to recycle it economically and efficiently according to the conventional lithium mica beneficiation process.
[0004] In view of this, it is still necessary to provide a mineral processing process that can efficiently recover low-grade lithium mica to solve the above problems. Summary of the invention
[0005] In view of the technical problems existing in the background technology, the present application provides a beneficiation process for recovering low-grade lepidolite, aiming to solve the problem that lepidolite recovery requires desludging and acid addition and the recovery rate and concentrate grade are low.
[0006] The present application embodiment provides a beneficiation process for recovering low-grade lepidolite, comprising the following steps:
[0007] Grinding low-grade lepidolite ore to obtain a first ore pulp;
[0008] Desulfurizing the first slurry to obtain sulfide ore and desulfurized tailings;
[0009] Adding a pH adjuster to the desulfurized tailings to obtain an alkaline second slurry;
[0010] adding an inhibitor and a combined collector to the second slurry in sequence, performing a lepidolite flotation operation, and obtaining a flotation lithium coarse concentrate and tailings;
[0011] The flotation lithium coarse concentrate is subjected to a beneficiation operation to obtain a lepidolite concentrate and beneficiated tailings.
[0012] In some embodiments, the combined collector includes the following components by mass fraction:
[0013] 70% to 80% of sulfonated sodium oleate, 10% to 20% of transformer oil, 0.5% to 1% of 12-hydroxystearic acid, 0.5% to 2% of diethylethanolamine and 5% to 10% of cationic collector.
[0014] In this embodiment, through the synergistic effect of the components in the combined collector, the surface of the lepidolite mineral can be efficiently and selectively adsorbed under alkaline conditions, thereby greatly improving the recovery rate of the lepidolite; and, the combined collector can also effectively reduce the heterogeneous agglomeration of muddy gangue and lepidolite, and can improve the grade of the lepidolite concentrate even without prior desludging, effectively shortening the mineral processing process and achieving efficient recovery of low-grade lepidolite.
[0015] In some embodiments, the cationic collector is one of dodecylamine and octadecylamine, or a mixture of the two.
[0016] In some embodiments, the combined collector is used in an amount of 300 to 550 g / t.
[0017] In this embodiment, the combined collector can efficiently float the lepidolite mineral. If the combined collector is used in too low an amount, the grade and recovery rate of the lepidolite concentrate will be reduced; if the combined collector is used in too high an amount, not only will the reagent cost be increased, but also the grade and recovery rate of the lepidolite concentrate will be affected.
[0018] In some embodiments, the pH value of the second slurry is 8-9.
[0019] In this embodiment, the components of the combined collector can give full play to the corresponding synergistic effects to improve the grade and recovery rate of the lithium mica concentrate. If the pH value of the second slurry is too high, it will corrode the equipment, and the flotation process will be easy to run due to the large amount of foam, and the operation will be unstable, resulting in the lithium mica concentrate grade not meeting the standard; if the pH value of the second slurry is too low, strong acid will be used, which will not only corrode the equipment but also bring hidden dangers to production safety, and the lithium mica concentrate grade and recovery rate will be affected.
[0020] In some embodiments, the pH adjuster is sodium carbonate, and the added amount of the pH adjuster is 1000-3000 g / t.
[0021] In some embodiments, the inhibitor is water glass, and the dosage of the inhibitor is 300-1000 g / t.
[0022] In some embodiments, the reagent used in the desulfurization operation includes butyl xanthate, and the amount of butyl xanthate used is 30-100 g / t.
[0023] In some embodiments, the slurry concentration during the grinding is 60% to 70%, and the grinding fineness is -0.074 mm particle size accounting for 50% to 60%; after the grinding, the slurry concentration is adjusted so that the concentration of the first slurry is 30% to 40%.
[0024] In some embodiments, the number of selections in the selection operation is 2 to 4 times, and each selection is a blank selection.
[0025] In this embodiment, the beneficiation process does not require the addition of acid or other reagents, which effectively avoids acid corrosion to equipment and its impact on the environment, while reducing the amount of reagents used and effectively reducing the mineral processing cost.
[0026] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the technical solution of the present application, the following is a brief introduction to the drawings used in the present application. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0028] Figure 1 This is a schematic diagram of the conventional lithium mica beneficiation process;
[0029] Figure 2 Schematic diagram of the process flow of the mineral processing technology for recovering low-grade lepidolite in the embodiment of the present application. DETAILED DESCRIPTION
[0030] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.
[0031] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.
[0032] In the description of the embodiments of the present application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features.
[0033] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0034] Conventional lithium mica beneficiation process requires desliming first, and then flotation with a cationic collector under acidic conditions. After flotation, acid needs to be added for concentration. Based on this conventional lithium mica beneficiation process, the recovery rate and concentrate grade are both low. It can only be used to recover lithium mica ores with a raw ore grade of more than 0.5%. It is difficult to recover low-grade (the raw ore contains LiO 2 In addition, the large amount of acid added can easily corrode the flotation equipment, affecting the safety of the mineral processing process, and a large amount of acidic wastewater will be generated after the mineral processing, which is not conducive to environmental protection.
[0035] In order to solve the technical problem that desliming and acid addition are required for the recovery of lepidolite, and the recovery rate and concentrate grade are both low, the present application provides a beneficiation process for recovering low-grade lepidolite, by designing a combined collector that can be used under alkaline conditions and enabling it to reduce the heterogeneous agglomeration of argillaceous gangue and lepidolite, thereby achieving efficient recovery of low-grade lepidolite without the need for desliming.
[0036] Please refer to Figure 2 The present application embodiment provides a beneficiation process for recovering low-grade lepidolite, comprising the following steps:
[0037] Grinding low-grade lepidolite ore to obtain a first ore pulp;
[0038] Desulfurizing the first slurry to obtain sulfide ore and desulfurized tailings;
[0039] Adding a pH adjuster to the desulfurized tailings to obtain an alkaline second slurry;
[0040] adding an inhibitor and a combined collector to the second slurry in sequence, performing a lepidolite flotation operation, and obtaining a flotation lithium coarse concentrate and tailings;
[0041] The flotation lithium coarse concentrate is subjected to a beneficiation operation to obtain a lepidolite concentrate and beneficiated tailings.
[0042] Through the above method, lithium mica can be selectively recovered in an alkaline environment. The whole process does not require desludging operations, the process flow is shorter, the equipment is not easily corroded, the reagent system is simplified, and the flotation effect of lithium mica can be improved. A higher-grade lithium mica concentrate can be obtained with a higher recovery rate, thereby achieving efficient recovery of low-grade lithium mica.
[0043] Furthermore, in some embodiments, the combined collector includes the following components by mass fraction:
[0044] 70% to 80% of sulfonated sodium oleate, 10% to 20% of transformer oil, 0.5% to 1% of 12-hydroxystearic acid, 0.5% to 2% of diethylethanolamine and 5% to 10% of cationic collector.
[0045] In the technical scheme of the embodiment of the present application, the sulfonic acid group in the fatty chain of sulfonated sodium oleate can effectively improve its solubility in the ore pulp, and can improve its selective action on the surface of the lithium mica mineral. At the same time, sulfonated sodium oleate can also work synergistically with cationic collectors and transformer oil, greatly reducing the overall amount of the combined collector, and using its hydrophobic group to selectively form chemical adsorption with the surface of the lithium mica mineral in the ore pulp, thereby greatly improving the recovery rate of lithium mica. On this basis, 12-hydroxystearic acid and diethylethanolamine can improve the dispersibility of the agent in the ore pulp, so that the muddy gangue that was originally easy to cover the surface of the lithium mica mineral can be fully dispersed in the ore pulp, reducing the heterogeneous coagulation of muddy gangue and lithium mica, thereby improving the grade of lithium mica concentrate. Based on the technical scheme provided by this embodiment, there is no need to carry out desludging operation, effectively shortening the mineral processing process, and improving the recovery rate of lithium mica.
[0046] Furthermore, in some embodiments, the cationic collector is one of dodecylamine and octadecylamine, or a mixture of the two.
[0047] Furthermore, in some embodiments, the dosage of the combined collector is 300-550 g / t.
[0048] In the technical solution of the embodiment of the present application, the combined collector can efficiently float the lepidolite mineral. If the dosage of the combined collector is too low, the grade and recovery rate of the lepidolite concentrate will be reduced; if the dosage of the combined collector is too high, it will not only increase the reagent cost, but also affect the grade and recovery rate of the lepidolite concentrate.
[0049] Furthermore, in some embodiments, the pH value of the second slurry is 8-9.
[0050] In the technical solution of the embodiment of the present application, each component of the combined collector can give full play to the corresponding synergistic effect to improve the grade and recovery rate of the lithium mica concentrate. If the pH value of the second slurry is too high, it will corrode the equipment and the flotation process will be easy to run due to the large amount of foam, resulting in unstable operation, resulting in the lithium mica concentrate grade not meeting the standard; if the pH value of the second slurry is too low, strong acid will be used, which will not only corrode the equipment but also bring hidden dangers to production safety, and the lithium mica concentrate grade and recovery rate will be affected.
[0051] Furthermore, in some embodiments, the pH adjuster is sodium carbonate, and the addition amount of the pH adjuster is 1000-3000 g / t.
[0052] Furthermore, in some embodiments, the inhibitor is water glass, and the dosage of the inhibitor is 300-1000 g / t, so as to achieve a better inhibitory effect.
[0053] Furthermore, in some embodiments, the agent used in the desulfurization operation includes butyl xanthate, and the amount of butyl xanthate used is 30-100 g / t to achieve a better desulfurization effect.
[0054] Furthermore, in some embodiments, the slurry concentration during the grinding is 60% to 70%, and the grinding fineness is -0.074 mm particle size accounting for 50% to 60%; after the grinding, the slurry concentration needs to be adjusted so that the concentration of the first slurry is 30% to 40% to facilitate the smooth progress of subsequent processes.
[0055] Furthermore, in some embodiments, the number of selections of the selection operation is 2 to 4 times, and each selection is a blank selection.
[0056] In the technical solution of the embodiment of the present application, the beneficiation process does not require the addition of acid or other agents, which effectively avoids acid corrosion to equipment and its impact on the environment, while reducing the amount of agents used and effectively reducing the cost of mineral processing.
[0057] Some specific embodiments are listed below. It should be noted that the embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If specific techniques or conditions are not specified in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be obtained commercially.
[0058] Example 1
[0059] This embodiment provides a beneficiation process for recovering low-grade lithium mica, and recovers low-grade mica ore in Linwu County. 2 The content of O is 0.26%. The beneficiation process specifically includes the following steps:
[0060] S1. Put low-grade lithium mica ore into a ball mill for wet grinding, wherein the grinding concentration is 65%, the grinding fineness is 0.074 mm, and the particle size accounts for 50% to 60%. After grinding, the pulp concentration is adjusted to 35% to obtain the first pulp.
[0061] S2. Add 70 g / t of butyl xanthate to the first slurry, stir for 2 minutes, and then perform desulfurization. After 2 minutes of flotation, sulfide ore and desulfurized tailings are obtained.
[0062] S3. Add about 2000 g / t of sodium carbonate to the desulfurized tailings, adjust the pH value of the slurry to about 8.5, and obtain a second slurry.
[0063] S4. Add 500 g / t of water glass to the second slurry, stir for 3 minutes, then add 400 g / t of combined collector, stir for 3 minutes, and then perform lithium mica flotation operation. After 3 minutes of flotation, obtain flotation lithium rough concentrate and tailings.
[0064] The mass fractions of the components in the combined collector are: 75% of sodium sulfonated oleate, 15% of transformer oil, 1% of 12-hydroxystearic acid, 2% of diethylethanolamine and 7% of dodecylamine.
[0065] After testing, the test results obtained in the above manner are shown in Table 1.
[0066] Table 1 Test results obtained in steps S1 to S4 of Example 1
[0067]
[0068] S5. further performing three blank concentrations on the flotation lithium coarse concentrate to obtain lithium mica concentrate and concentrated tailings, and the concentrated tailings are returned to the previous flotation operation.
[0069] After the above three blank concentrations, the lithium mica concentrate obtained contains 2 The grade of O is 3.03% and the recovery rate is 58.42%.
[0070] Comparative Example 1
[0071] This comparative example provides a beneficiation process for recovering low-grade lepidolite. The low-grade lepidolite ore is consistent with that in Example 1. The beneficiation process specifically includes the following steps:
[0072] S1. Put low-grade lithium mica ore into a ball mill for wet grinding, wherein the grinding concentration is 65%, the grinding fineness is 0.074 mm, and the particle size accounts for 50% to 60%. After grinding, the pulp concentration is adjusted to 35% to obtain the first pulp.
[0073] S2. Desludging the first slurry to obtain desludging slurry.
[0074] S3. Add 50g / t of butyl xanthate to the deslimed slurry, stir for 2 minutes, and then perform desulfurization. After 2 minutes of flotation, sulfide ore and desulfurized tailings are obtained.
[0075] S4. Add about 1000 g / t of hydrochloric acid to the desulfurized tailings to adjust the pH value of the slurry to about 5 to obtain a second slurry.
[0076] S5. Add 100 g / t of water glass to the second slurry, stir for 3 minutes, then add 300 g / t of dodecylamine, stir for 3 minutes, and then perform lithium mica flotation operation. After 3 minutes of flotation, obtain a flotation lithium rough concentrate and tailings.
[0077] After testing, the test results obtained in the above manner are shown in Table 2.
[0078] Table 2 Test results obtained in steps S1 to S5 of comparative example 1
[0079]
[0080] S6. The flotation lithium rough concentrate is subjected to three concentrations. Acid is added before each concentration to adjust the pH value of the slurry to 3, so as to obtain lithium mica concentrate and concentrated tailings. The concentrated tailings are returned to the previous flotation operation.
[0081] After the above three rounds of concentration, the lithium mica concentrate obtained contains 2 The grade of O is 2.35% and the recovery rate is 31.29%.
[0082] Compared with Example 1, it can be seen that the method provided in this comparative example not only has a more complicated process, but also has lower grade and recovery rate, indicating that the low-grade lithium mica beneficiation process provided in Example 1 of the present application is shorter than the conventional lithium mica beneficiation process, and the concentrate grade and recovery rate are greatly improved.
[0083] Examples 2 to 3 and Comparative Examples 2 to 7
[0084] Examples 2 to 3 and Comparative Examples 2 to 7 respectively provide a beneficiation process for recovering low-grade lepidolite. Compared with Example 1, the only difference is that the mass fraction of each component in the combined collector is changed, and the remaining steps are consistent with Example 1, which will not be repeated here. The composition of the combined collector used in Examples 2 to 3 and Comparative Examples 2 to 7 is shown in Table 3.
[0085] Table 3 Mass fraction of each component in the combined collector of Examples 2 to 3 and Comparative Examples 2 to 7
[0086]
[0087] The Li in the lithium mica concentrate finally obtained in Examples 2 to 3 and Comparative Examples 2 to 7 2 The grade and recovery rate of O were tested, and the results are shown in Table 4.
[0088] Table 4 Test results of Examples 2 to 3 and Comparative Examples 2 to 7
[0089]
[0090]
[0091] It can be seen from Table 4 that the ratio of each component in the combined collector will have a great influence on the final concentrate grade and concentrate recovery rate. 2 The grade of O was increased to 2.8% to 3.6%, and the Li 2 The recovery rate of O is increased to 50% to 65%, achieving efficient recovery of low-grade lepidolite.
[0092] Examples 4-5 and Comparative Examples 8-9
[0093] Examples 4 to 5 and Comparative Examples 8 to 9 respectively provide a beneficiation process for recovering low-grade lepidolite. Compared with Example 1, the only difference is that the amount of the pH adjuster is changed, thereby changing the pH value of the second slurry. The remaining steps are consistent with Example 1 and are not repeated here. The pH values of the second slurry in Examples 4 to 5 and Comparative Examples 8 to 9 are shown in Table 5.
[0094] Table 5 pH value of the second slurry of Examples 4 to 5 and Comparative Examples 8 to 9
[0095] Example / Comparative Example pH value of the second slurry Example 4 8 Example 5 9 Comparative Example 8 7 Comparative Example 9 10
[0096] The Li in the lithium mica concentrate finally obtained in Examples 4 to 5 and Comparative Examples 8 to 9 2 The grade and recovery rate of O were tested, and the results are shown in Table 6.
[0097] Table 4 Test results of Examples 4 to 5 and Comparative Examples 8 to 9
[0098] Example / Comparative Example <![CDATA[Li 2 O grade (%)]]> <![CDATA[Li 2 O recovery rate (%)]]> Example 4 3.26 56.28 Example 5 2.89 62.15 Comparative Example 8 2.68 50.17 Comparative Example 9 2.54 58.38
[0099] It can be seen from Table 6 that too high or too low pH value will affect the concentrate grade and recovery rate of lithium mica. The present application can simultaneously improve the concentrate grade and recovery rate of lithium mica by accurately controlling the pH value of the second slurry.
[0100] In summary, the present application provides a mineral processing process for recovering low-grade lithium mica, which belongs to the field of lithium mica mineral processing, wherein the process includes: grinding low-grade lithium mica ore to obtain a first slurry; desulfurizing the first slurry to obtain sulfide ore and desulfurized tailings; adding a pH adjuster to the desulfurized tailings to obtain an alkaline second slurry; sequentially adding an inhibitor and a combined collector to the second slurry to perform lithium mica flotation operations to obtain a flotation rough concentrate and tailings; performing a beneficiation operation on the flotation rough concentrate to obtain a lithium mica concentrate and beneficiated tailings. Based on the mineral processing process provided by the present application, lithium mica can be selectively recovered in an alkaline environment, and the entire process does not require desludging operations, the process flow is shorter, the equipment is not susceptible to corrosion, the reagent system is simplified, and the flotation effect of lithium mica can be improved. Based on the method provided by the present application, Li 2 After the low-grade lithium mica with an O grade of less than 0.5% is beneficiated, the lithium mica concentrate obtained contains Li 2 The grade of O is 2.8% to 3.6%, and the Li content in lithium mica concentrate is 2 The recovery rate of O is 50% to 65%, and a higher recovery rate and higher grade are obtained at the same time, realizing the efficient recovery of low-grade lepidolite.
[0101] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A beneficiation process for recovering low-grade lepidolite, characterized in that: The steps include: Grinding low-grade lepidolite ore to obtain a first slurry; Desulfurizing the first slurry to obtain sulfide ore and desulfurized tailings; Adding a pH adjuster to the desulfurized tailings to obtain an alkaline second slurry; adding an inhibitor and a combined collector to the second slurry in sequence, performing a lepidolite flotation operation, and obtaining a flotation lithium coarse concentrate and tailings; The flotation lithium coarse concentrate is subjected to a beneficiation operation to obtain a lepidolite concentrate and beneficiated tailings.
2. The ore dressing process for recovering low-grade lepidolite according to claim 1, characterized in that: The combined collector includes the following components by mass fraction: 70% to 80% of sulfonated sodium oleate, 10% to 20% of transformer oil, 0.5% to 1% of 12-hydroxystearic acid, 0.5% to 2% of diethylethanolamine and 5% to 10% of cationic collector.
3. The ore dressing process for recovering low-grade lepidolite according to claim 2, characterized in that: The cationic collector is one of dodecylamine and octadecylamine or a mixture of the two.
4. The ore dressing process for recovering low-grade lepidolite according to claim 1, characterized in that: The dosage of the combined collector is 300-550 g / t.
5. The ore dressing process for recovering low-grade lepidolite according to claim 1, characterized in that: The pH value of the second slurry is 8-9.
6. The ore dressing process for recovering low-grade lepidolite according to claim 5, characterized in that: The pH adjuster is sodium carbonate, and the addition amount of the pH adjuster is 1000-3000 g / t.
7. The ore dressing process for recovering low-grade lepidolite according to claim 1, characterized in that: The inhibitor is water glass, and the dosage of the inhibitor is 300-1000 g / t.
8. The ore dressing process for recovering low-grade lepidolite according to claim 1, characterized in that: The reagent used in the desulfurization operation includes butyl xanthate, and the dosage of the butyl xanthate is 30-100 g / t.
9. The ore dressing process for recovering low-grade lepidolite according to claim 1, characterized in that: The ore pulp concentration during the grinding is 60% to 70%, and the grinding fineness is -0.074mm particle size accounting for 50% to 60%; after the grinding, the ore pulp concentration is adjusted to make the concentration of the first ore pulp 30% to 40%.
10. The ore dressing process for recovering low-grade lepidolite according to claim 1, characterized in that: The number of times of the selection operation is 2 to 4 times, and each selection is a blank selection.
Citation Information
Patent Citations
Method for extracting and preparing high-purity anhydrous lithium sulfate solid from byproduct mirabilite of lithium smelting enterprise
CN112850756A
Composite collecting agent, flotation reagent and method for low-grade lithium ore
CN115582223A
Non-desliming lepidolite flotation method
CN115608520A
Beneficiation method for comprehensively improving indexes of low-grade lepidolite concentrate
CN116371590A
Method for recovering lepidolite through short-process flotation
CN116727114A