Comprehensive recovery method of molybdenum, lead, sulfur and quartz in quartzite type molybdenum ore

Through the combination of physical ore dressing and chemical ore dressing, combined with specific agents and ceramic media, the efficient recovery of molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore is achieved, and the excess lead standard and the large tailings emissions in molybdenum concentrate are solved. The problem of this has improved resource utilization and recovery.

CN118874697APending Publication Date: 2024-11-01CHINA MOLYBDENUM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410851865.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The prior art is difficult to effectively separate molybdenum, lead and sulfur in quartzite-type molybdenum ore, resulting in high lead content in molybdenum concentrate, which is difficult to achieve the expected recovery effect, and the tailings emissions are large and resource utilization is insufficient.

Method used

Using the combination of physical ore dressing and chemical ore dressing, through crushing, wet ball milling, flotation and stirring leaching, multiple selections are performed using specific agents and ceramic media to achieve efficient recycling of molybdenum, lead, sulfur and quartz, reducing the efficiency of Molybdenum concentrates lead content and reduce tailings emissions.

Benefits of technology

It realizes efficient recycling of molybdenum, lead, sulfur and quartz, improves recovery and resource utilization, reduces tailings emissions, and has a simple and easy-to-operate process, which is environmentally friendly and efficient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874697A_ABST
    Figure CN118874697A_ABST
Patent Text Reader

Abstract

The invention discloses a comprehensive recovery method for molybdenum, lead, sulfur and quartz in quartzite type molybdenum ore, which comprises the following steps: S1, carrying out raw ore grinding operation, S2, carrying out molybdenum roughing I operation on ore pulp to obtain molybdenum rough concentrate and molybdenum roughing tailings; s3, blank concentration and regrinding are conducted on the molybdenum rough concentrate for molybdenum roughing II operation, a foam product II is obtained, molybdenum concentration is conducted on the foam product II, and molybdenum concentrate I is obtained; the molybdenum concentrate I is subjected to leaching operation to obtain pregnant solution and leaching residues, and the leaching residues are washed to obtain final qualified molybdenum concentrate; s5, carrying out blank concentration II operation on the lead-sulfur bulk concentrate to obtain a foam product III; the foam product III is subjected to lead and sulfur separation roughing operation; s6, lead scavenging is conducted on the lead roughing tailings to obtain lead scavenging concentrates and lead scavenging tailings, and quartz roughing operation is conducted on the tailings obtained through lead scavenging; and the quartz rough concentrate continues to be subjected to one-time concentration operation to obtain quartz concentrate and tailings II. The quartzite type molybdenum ore is treated in a physical ore dressing and chemical ore dressing combined mode, lead in molybdenum concentrate is reduced, and molybdenum, lead, sulfur and quartz in raw ore are efficiently recycled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ore dressing methods, and in particular to a comprehensive recovery method of molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore. Background Art

[0002] Molybdenum is an important strategic resource and plays an important role in industrial production. It is widely used in metallurgy, chemical industry, machinery manufacturing, electronics, aerospace, medical and other fields. my country's molybdenum mineral resources are widely distributed, but the grade is low. For example, quartzite-type molybdenum ore has a natural type close to primary ore, that is, molybdenum mainly exists in the form of molybdenite, which is often associated with sulfide minerals such as chalcopyrite and galena. In the flotation separation of complex polymetallic sulfide ores of molybdenum and lead, due to the complex intercalation relationship between molybdenite and galena, and their similar floatability, the separation of molybdenum and lead has always been a difficult problem. Therefore, molybdenum concentrate often contains high lead, making it difficult to achieve the expected recovery effect and product indicators. In addition, the useful minerals in the ore are encouraged to be comprehensively utilized to minimize the discharge of tailings.

[0003] Patent CN117206085A discloses a highly selective molybdenite flotation collector and its preparation method and use. The invention improves the collection capacity and the flotation recovery rate of molybdenite by designing the structure of the collector and realizing the selective adsorption of molybdenite under the action of different reagents; Patent CN115970851A discloses a grinding-flotation short-process separation method for treating fine-grained molybdenite. The invention reduces the over-grinding problem in the grinding process by using a tower mill to grind the ore, improves the mineral particle size composition of the flotation operation, and is a particle size composition The flotation column is used to replace the flotation machine, which reduces the circulation of the medium ore pulp and enhances the recovery of fine particles in the flotation process, thereby improving the flotation recovery rate. The above patent only improves the flotation recovery rate of molybdenite. For minerals with similar floatability such as lead and sulfur, it is not possible to effectively separate different minerals. Therefore, an efficient, stable and adaptable comprehensive recovery process is developed to achieve comprehensive recovery of sulfur and quartz while ensuring that the molybdenum and lead concentrates meet the standards. This is of great significance for the full utilization of resources of a difficult-to-select quartzite type molybdenum ore. Summary of the invention

[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a comprehensive recovery method for molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore, so as to realize the recovery of valuable metals molybdenum, lead, sulfur and high-purity quartz, solve the problems of difficult separation of molybdenum and lead and excessive lead in molybdenum concentrate, reduce the discharge of tailings, have high recovery rate, be stable, have strong adaptability, and be environmentally friendly and efficient.

[0005] The technical solution adopted by the present invention is: A comprehensive recovery method for molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore, comprising the following specific steps: S1: The raw ore is crushed and wet ball milled to grind the ore to a particle size of -0.074mm with a content of 60-70%; S2: The slurry ground in S1 is subjected to a molybdenum roughing I operation for suppressing lead and floating molybdenum to obtain a molybdenum rough concentrate and a molybdenum roughing tailings; S3: The molybdenum rough concentrate obtained from the molybdenum roughing operation I in S2 is stirred and slurried, and the foam product I obtained after 1-2 times of blank selection operation I in the flotation machine is subjected to a stirred mill re-grinding operation, and the re-grinded product is slurried for molybdenum roughing operation II to obtain a foam product II and a circulating product I, and the circulating product I is returned to the blank selection operation I, and the foam product II is subjected to 3-5 molybdenum selection operations to obtain a molybdenum concentrate I and a circulating product II, and the circulating product II is returned to the stirred mill before the re-grinding operation, and the molybdenum concentrate I is subjected to a stirring leaching operation to remove lead from the molybdenum concentrate, and then solid-liquid separation is performed to obtain a precious liquid and a leaching residue, and the leaching residue is then washed with water 3-4 times to obtain a final qualified molybdenum concentrate; S4: subjecting the molybdenum roughing tailings obtained from the molybdenum roughing I operation in S2 to a molybdenum scavenging operation to obtain a molybdenum scavenging concentrate, and returning the molybdenum scavenging concentrate and the tailings from the blank selection I operation in S3 to the front of the molybdenum roughing I operation; subjecting the tailings obtained from the molybdenum scavenging operation to a lead roughing operation, and obtaining a lead-sulfur mixed concentrate and a lead roughing tailings from the lead roughing operation; S5: The lead-sulfur mixed concentrate obtained from the lead roughing operation in S4 is subjected to blank selection II to obtain foam product III and intermediate product I, the foam product III is subjected to lead and sulfur separation roughing operation to obtain foam product IV and separation roughing tailings, the foam product IV is further subjected to separation and selection operation 2-3 times to obtain lead concentrate and intermediate product II, the separation roughing tailings are subjected to scavenging operation once to obtain sulfur concentrate and intermediate product III; the intermediate product II and the intermediate product III are returned together to the lead and sulfur separation roughing operation; S6: The lead roughing tailings obtained from the lead roughing operation in S4 are subjected to lead scavenging to obtain lead scavenging concentrate and lead scavenging tailings, and the lead scavenging concentrate and the intermediate product I in S5 are returned to the lead roughing operation; the tailings obtained from the lead scavenging are subjected to quartz roughing operation to obtain quartz rough concentrate and tailings I, and the quartz rough concentrate is further subjected to one quartz concentration operation to obtain quartz concentrate and tailings II; tailings I and tailings II are combined into the final tailings.

[0006] Specifically, in the S2, the reagent system of the molybdenum roughing I operation is: adding 30-60g / t of inhibitor Phosphok, 50-80g / t of collector kerosene, and 20-40g / t of foaming agent 2# oil; In S3, the reagent system of molybdenum roughing II operation is: adding 30-60g / t of inhibitor Phosphorus Knox, 50-80g / t of collector kerosene, 20-40g / t of foaming agent 2# oil, and 100-300g / t of dispersant water glass; the reagent system of molybdenum concentration single operation is: adding 100~300g / t of dispersant water glass, 30-80g / t of inhibitor Phosphorus Knox and 30-120g / t of sodium thioglycolate, 0-20g / t of collector kerosene, and 0-10g / t of foaming agent 2# oil; In S4, the molybdenum scavenging reagent system is: adding inhibitor Phosphok 20-40g / t, collector kerosene 15-30g / t, foaming agent 2# oil 10-20g / t.

[0007] Specifically, in S3, the leaching agents for the stirring leaching operation are sodium chloride and dilute hydrochloric acid; the solution is adjusted to a pH value of 1-1.5 using dilute hydrochloric acid with a mass fraction of 15%, and the amount of sodium chloride added is 270-320 g / L; the leaching operation conditions are: liquid-solid ratio of (3-4):1, leaching temperature of 80-100°C, and leaching time of 2-4h.

[0008] Specifically, the grinding medium used in the regrinding operation in S3 is a ceramic ball with an alumina content of ≥90%, and the grinding fineness requirement is -0.038mm particle size content of 90-95%, that is, the mass percentage of -0.038mm particle size material is 90-95%; the Fe content in the slurry after slurry adjustment of the regrinding product is 3+ The concentration is not more than 80mg / L; it makes the mineral surface more hydrophobic and has better floatability.

[0009] Specifically, in S3, when the foam product II undergoes 3-5 times of molybdenum selection, the selection equipment adopts a flotation machine + flotation column combined process, the first selection adopts a flotation machine, and the next two selections use flotation columns as flotation equipment.

[0010] Specifically, in the S4, the reagent system for lead roughing operation is: adding 15-30 g / t of collector sulfur and nitrogen and 15-30 g / t of foaming agent 2# oil.

[0011] Specifically, in S5, the reagent system for lead and sulfur separation roughing operation is: adding 500-700g / t of lime as an inhibitor and 10-20g / t of sulfur and nitrogen as a collector; the reagent system for separation and selection single operation is: adding 400-600g / t of lime as an inhibitor; adding 10-20g / t of sulfur and nitrogen as a collector and 5-15g / t of frother 2# oil as a scavenging separation operation.

[0012] Specifically, in the S6, the reagent system for lead scavenging operation is: adding 10-20 g / t of sulfur and nitrogen as collectors, and 5-20 g / t of 2# oil as foaming agent; the reagent system for quartz roughing operation is: adding 1500-2500 g / t of sulfuric acid as adjusting agent, adjusting to a pH value of 4; adding 150-250 g / t of dodecylamine as collector; the reagent system for quartz concentration operation is: adding 800-1200 g / t of sulfuric acid as adjusting agent, adjusting to a pH value of 4, and adding 80-150 g / t of dodecylamine as collector.

[0013] The final tailings discharge in S6 is relatively low, with a mass fraction of less than 40% of the original ore.

[0014] Due to the adoption of the above-mentioned technical solution, the present invention has the following advantages: The present invention adopts a combination of physical beneficiation and chemical beneficiation to process quartzite-type molybdenum ore, reduce the lead in the molybdenum concentrate, and realize efficient recovery of molybdenum, lead, sulfur and quartz in the original ore; the process structure and reagent system are simple, the on-site production is easy to operate, the flotation tail water is recycled, and the external tail water meets the discharge standards; the ceramic medium grinding is adopted to improve the floatability of the minerals, magnify the difference in floatability of different minerals, realize the efficient separation of polymetallic ores, and improve their respective recovery rates; the tailings quartz recovery not only obtains qualified quartz concentrate, but also greatly reduces the discharge of mine tailings, thereby increasing the economic benefits of the mine. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0016] The present invention will be further explained below in conjunction with the accompanying drawings and embodiments, which should not be used to limit the protection scope of the present invention. The purpose of disclosing the present invention is to protect all technical improvements within the scope of the present invention.

[0017] Taking a quartzite-type molybdenum ore in Henan as an example, the molybdenum content of the original ore is 0.089%, the sulfur grade is 1.28%, the lead grade is 0.18%, the SiO2 content in the ore is 85.14%, and the lead in the ore mainly exists as an independent mineral of galena. The oxidized lead phase is mainly lead alum, followed by cerussite. The metallic minerals in the ore are molybdenite, pyrite, galena, followed by lead alum, cerussite, etc. The non-metallic minerals are mainly quartz, followed by a small amount of chlorite, sericite, etc.

[0018] Combined with Figure 1 A comprehensive recovery method of molybdenum, lead, sulfur and quartz from a quartzite-type molybdenum ore is shown, and the specific steps are: S1: The raw ore is crushed and wet ball milled to grind the ore to a -0.074mm particle size content of 68.59%, that is, the mass percentage of the -0.074mm particle size material is 68.59%.

[0019] S2: The pulp ground in S1 is subjected to molybdenum roughing I operation for suppressing lead and floating molybdenum in the flotation machine to obtain molybdenum rough concentrate and molybdenum roughing tailings.

[0020] S3: The molybdenum rough concentrate obtained from the molybdenum roughing I operation in S2 is stirred and slurried, and the foam product I obtained after a blank selection I operation in the flotation machine is re-grinded in a stirred mill. The grinding medium used in the re-grinding operation is a ceramic ball with an alumina content of ≥90%, and the grinding fineness requirement is -0.038mm particle size content of 95%; Fe in the slurry after slurrying of the re-grinded product 3+ The concentration is 55 mg / L, and then the molybdenum roughing operation II is carried out to obtain foam product II and circulating product I, and the circulating product I is returned to the blank concentration operation I; the foam product II is subjected to three molybdenum concentration operations to obtain molybdenum concentrate I and circulating product II, and the circulating product II is returned to the stirred mill before the regrinding operation. The first molybdenum concentration adopts a flotation machine, and the next two molybdenum concentrations adopt flotation columns; the molybdenum concentrate I is subjected to a stirring leaching operation to remove the lead in the molybdenum concentrate, and then solid-liquid separation is carried out to obtain precious liquid and leaching residue, and the leaching residue is washed with water three times to obtain the final qualified molybdenum concentrate.

[0021] S4: The molybdenum roughing tailings obtained from the molybdenum roughing I operation in S2 are subjected to one molybdenum scavenging operation to obtain a molybdenum scavenging concentrate, and the molybdenum scavenging concentrate and the tailings from the blank concentration I operation in S3 are returned to the front of the molybdenum roughing I operation; the tailings products obtained from the molybdenum scavenging are subjected to lead roughing operation, and the lead roughing is performed to obtain a lead-sulfur mixed concentrate and lead roughing tailings.

[0022] S5: The lead-sulfur mixed concentrate obtained from the lead roughing operation in S4 is subjected to blank selection operation II to obtain foam product III and intermediate product I; the foam product III is subjected to lead and sulfur separation roughing operation to obtain foam product IV and separation roughing tailings; the foam product IV is further subjected to separation and selection operation twice to obtain lead concentrate and intermediate product II; the separation roughing tailings is subjected to scavenging operation once to obtain sulfur concentrate and intermediate product III; intermediate product II and intermediate product III are returned together to the lead and sulfur separation roughing operation.

[0023] S6: The lead roughing tailings obtained from the lead roughing operation in S4 are subjected to lead scavenging to obtain lead scavenging concentrate and lead scavenging tailings, and the lead scavenging concentrate and the intermediate product I in S5 are returned to the lead roughing operation; the tailings obtained from the lead scavenging are subjected to quartz roughing operation to obtain quartz rough concentrate and tailings I, and the quartz rough concentrate is further subjected to one quartz concentration operation to obtain quartz concentrate and tailings II; tailings I and tailings II are combined into the final tailings.

[0024] Preferably, in the S2, the reagent system of the molybdenum roughing I operation is: adding 40g / t of inhibitor Phosphok, 60g / t of collector kerosene, and 30g / t of foaming agent 2# oil; In S3, the reagent system of molybdenum roughing II operation is: adding dispersant water glass 200g / t, inhibitor phosphok 40g / t, collector kerosene 60g / t, foaming agent 2# oil 30g / t; dispersant water glass 200, 100, 100 g / t; inhibitor phosphok 70, 35, 35 g / t, inhibitor sodium thioglycolate 100, 50, 50 g / t, collector kerosene 10, 0, 0g / t, foaming agent 2# oil 5, 0, 0 g / t were added in the 3rd molybdenum concentration respectively; In S4, the molybdenum scavenging reagent system is: adding 20 g / t of inhibitor Phosphok, 20 g / t of collector kerosene, and 15 g / t of frother 2# oil.

[0025] Preferably, in S3, the leaching agents are sodium chloride and dilute hydrochloric acid; the solution is adjusted to a pH value of 1.2 using dilute hydrochloric acid with a mass fraction of 15%, and the amount of sodium chloride added is 290 g / L; the leaching conditions are: liquid-to-solid ratio of 4:1, leaching temperature of 90°C, and leaching time of 4 hours.

[0026] Preferably, in the S4, 20 g / t of collector sulfur and nitrogen and 20 g / t of foaming agent 2# oil are added in the lead roughing operation.

[0027] Preferably, in S5, 600 g / t of lime as an inhibitor and 10 g / t of sulfur and nitrogen as a collector are added in the rough separation operation of lead and sulfur; 500 and 400 g / t of lime as an inhibitor are added in the two separation and concentration operations respectively; 10 g / t of sulfur and nitrogen as a collector and 10 g / t of 2# oil as a foaming agent are added in the separation and scavenging operation.

[0028] Preferably, in the S6, 10 g / t of sulfur and nitrogen as a collector and 10 g / t of 2# oil as a foaming agent are added in the lead scavenging operation; 2100 g / t of sulfuric acid as an adjusting agent is added in the quartz roughing operation, the pH value is adjusted to 4, and 200 g / t of dodecylamine as a collector is added; 1000 g / t of sulfuric acid as an adjusting agent is added in the quartz concentrating operation, the pH value is adjusted to 4, and 100 g / t of dodecylamine as a collector is added.

[0029] The final tailings discharge in S6 is relatively low, with a mass fraction of 35.12% of the original ore.

[0030] The final technical indicators of each product are shown in Table 1.

[0031]

[0032] Note: “-” in Table 1 means items not tested.

[0033] Parts of the present invention not described in detail are prior art.

[0034] The embodiments selected herein for the purpose of disclosing the invention are currently considered to be suitable, but it should be understood that the invention is intended to include all changes and modifications of the embodiments that fall within the scope of the concept and invention.

Claims

1. A comprehensive recovery method for molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore, It is characterized in that The specific steps are: S1: The raw ore is crushed and wet ball milled to grind the ore to a particle size of -0.074mm with a content of 60-70%; S2: The ore pulp ground in S1 is subjected to a molybdenum roughing I operation for suppressing lead and floating molybdenum to obtain a molybdenum rough concentrate and a molybdenum roughing tailings; S3: stirring and slurrying the molybdenum rough concentrate obtained from the molybdenum roughing operation I in S2, carrying out 1-2 blank selection operations I in a flotation machine to obtain a foam product I, carrying out a stirred mill re-grinding operation, slurrying the re-grinded product to carry out a molybdenum roughing operation II to obtain a foam product II and a circulating product I, before the circulating product I is returned to the blank selection operation I, the foam product II is subjected to 3-5 molybdenum selection operations to obtain a molybdenum concentrate I and a circulating product II, the circulating product II is returned to the stirred mill re-grinding operation, the molybdenum concentrate I is subjected to a stirring leaching operation to remove lead from the molybdenum concentrate, and then solid-liquid separation is carried out to obtain a precious liquid and a leaching residue, and the leaching residue is then washed 3-4 times to obtain a final qualified molybdenum concentrate; S4: subjecting the molybdenum roughing tailings obtained from the molybdenum roughing I operation in S2 to a molybdenum scavenging operation to obtain a molybdenum scavenging concentrate, and returning the molybdenum scavenging concentrate and the tailings from the blank selection I operation in S3 to the front of the molybdenum roughing I operation; subjecting the tailings obtained from the molybdenum scavenging operation to a lead roughing operation, and obtaining a lead-sulfur mixed concentrate and a lead roughing tailings from the lead roughing operation; S5: The lead-sulfur mixed concentrate obtained from the lead roughing operation in S4 is subjected to blank selection II to obtain foam product III and intermediate product I, the foam product III is subjected to lead and sulfur separation roughing operation to obtain foam product IV and separation roughing tailings, the foam product IV is further subjected to separation and selection operation 2-3 times to obtain lead concentrate and intermediate product II, the separation roughing tailings are subjected to scavenging operation once to obtain sulfur concentrate and intermediate product III; the intermediate product II and the intermediate product III are returned together to the lead and sulfur separation roughing operation; S6: The lead roughing tailings obtained from the lead roughing operation in S4 are subjected to lead scavenging to obtain lead scavenging concentrate and lead scavenging tailings, and the lead scavenging concentrate and the intermediate product I in S5 are returned to the lead roughing operation; the tailings obtained from the lead scavenging are subjected to quartz roughing operation to obtain quartz rough concentrate and tailings I, and the quartz rough concentrate is further subjected to one quartz concentration operation to obtain quartz concentrate and tailings II; tailings I and tailings II are combined into the final tailings.

2. The comprehensive recovery method of molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore according to claim 1, Features: In the above-mentioned S2, the reagent system of the molybdenum roughing I operation is: adding 30-60g / t of inhibitor Phosphok, 50-80g / t of collector kerosene, and 20-40g / t of foaming agent 2# oil; In S3, the reagent system of molybdenum roughing II operation is: adding 30-60g / t of inhibitor Phosphorus Knox, 50-80g / t of collector kerosene, 20-40g / t of foaming agent 2# oil, and 100-300g / t of dispersant water glass; the reagent system of molybdenum concentration single operation is: adding 100~300g / t of dispersant water glass, 30-80g / t of inhibitor Phosphorus Knox and 30-120g / t of sodium thioglycolate, 0-20g / t of collector kerosene, and 0-10g / t of foaming agent 2# oil; In S4, the molybdenum scavenging reagent system is: adding inhibitor Phosphok 20-40g / t, collector kerosene 15-30g / t, foaming agent 2# oil 10-20g / t.

3. The comprehensive recovery method of molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore according to claim 1, Features: In S3, the leaching agents for the stirring leaching operation are sodium chloride and dilute hydrochloric acid; the solution is adjusted to a pH value of 1-1.5 using dilute hydrochloric acid with a mass fraction of 15%, and the amount of sodium chloride added is 270-320 g / L; the leaching operation conditions are: liquid-solid ratio is (3-4):1, leaching temperature is 80-100°C, and leaching time is 2-4h.

4. The comprehensive recovery method of molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore according to claim 1, Features: The grinding medium used in the regrinding operation in S3 is ceramic balls with an alumina content of ≥90%, and the grinding fineness requirement is 90-95% of the -0.038mm particle size, that is, the mass percentage of the -0.038mm particle size material is 90-95%; the Fe content in the slurry after slurry adjustment of the regrinding product 3+ The concentration is not more than 80mg / L.

5. The comprehensive recovery method of molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore according to claim 1, Features: In S3, when the foam product II is subjected to 3-5 times of molybdenum selection, the selection equipment adopts a flotation machine + flotation column combined process, the first selection adopts a flotation machine, and the latter two selections use flotation columns as flotation equipment.

6. The comprehensive recovery method of molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore according to claim 1, Features: In the S4, the reagent system for lead roughing operation is: adding 15-30g / t of collector sulfur and nitrogen and 15-30g / t of foaming agent 2# oil.

7. The comprehensive recovery method of molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore according to claim 1, Features: In the S5, the reagent system for lead and sulfur separation roughing operation is: adding 500-700g / t of lime as an inhibitor and 10-20g / t of sulfur and nitrogen as collectors; the reagent system for separation and selection single operation is: adding 400-600g / t of lime as an inhibitor; adding 10-20g / t of sulfur and nitrogen as collectors and 5-15g / t of frother 2# oil as a scavenging separation operation.

8. The comprehensive recovery method of molybdenum, lead, sulfur and quartz in quartzite-type molybdenum ore according to claim 1, Features: In the S6, the reagent system for lead scavenging operation is: adding 10-20 g / t of sulfur and nitrogen as collectors and 5-20 g / t of 2# oil as foaming agent; the reagent system for quartz roughing operation is: adding 1500-2500 g / t of sulfuric acid as adjusting agent, adjusting to a pH value of 4, and adding 150-250 g / t of dodecylamine as collector; the reagent system for quartz concentration operation is: adding 800-1200 g / t of sulfuric acid as adjusting agent, adjusting to a pH value of 4, and adding 80-150 g / t of dodecylamine as collector.