Ultrathin mirror molybdenum wafer and preparation method and application thereof
Through ultraviolet laser cutting, magnetic polishing and high-temperature equalization technologies, combined with double-sided grinding and polishing, the problems of thickness and shape changes in ultra-thin molybdenum wafer processing are solved, and high-precision and high-quality ultra-thin mirror molybdenum circles are achieved. Tablet preparation, suitable for semiconductor materials field.
Patent Information
- Application Number
- CN202410858589.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art is difficult to avoid changes in thickness and shape while ensuring the processing accuracy and surface quality of ultra-thin molybdenum wafers, especially under the requirements of flatness and roughness.
UV laser cutting, magnetic polishing, double-sided grinding and high-temperature leveling technology are adopted, combined with double-sided polishing, and through precise processing parameter control, the flatness and roughness of the molybdenum wafer reaches high precision.
The ultra-thin mirror molybdenum wafer preparation with high flatness (flatness ≦0.05mm) and low roughness (Ra≦10nm) is achieved, which meets the high requirements of semiconductor manufacturing, avoids thickness and shape changes, and is suitable for large-scale production.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of semiconductor material preparation, in particular to the technical field of high-precision preparation of ultra-thin mirror-surface molybdenum discs. Background Art
[0002] In the field of semiconductor material preparation technology, molybdenum is an important metal material and is widely used due to its good electrical and thermal conductivity and low expansion coefficient.
[0003] However, molybdenum has a high hardness and is difficult to process. Traditional molybdenum disc processing methods are mainly through mechanical cutting, grinding and stamping, but these methods often cannot meet the high requirements of modern semiconductor devices for the accuracy and surface quality of ultra-thin (thickness ≤ 0.1mm) mirror molybdenum discs.
[0004] In the field of precision grinding and polishing technology, double-sided grinding and polishing technology is an advanced processing method that can achieve simultaneous grinding and polishing of both sides of the workpiece, thereby improving processing efficiency and processing accuracy. However, this technology still faces some challenges when applied to the processing of ultra-thin molybdenum discs, and it is difficult to ensure the flatness and roughness during the processing.
[0005] In the field of high temperature heat treatment technology, high temperature leveling is a common heat treatment method that can be used to improve the flatness of workpieces and reduce internal stress. However, when this method is applied to the processing of ultra-thin molybdenum discs, the thickness and shape of the molybdenum discs may change, affecting their performance.
[0006] In order to solve the above problems, the existing technical solutions are mainly to improve the processing accuracy and surface quality of ultra-thin molybdenum discs by improving the grinding and polishing equipment and processes, and optimizing the heat treatment parameters. For example, some researchers have proposed the use of chemical mechanical polishing (CMP) method, which can effectively reduce the roughness of molybdenum discs by introducing chemical corrosive agents. In addition, some researchers have proposed the use of low-temperature heat treatment method, which can avoid deformation of molybdenum discs during heat treatment by controlling the heat treatment temperature and time. Although the existing technical solutions have improved the processing accuracy and surface quality of ultra-thin molybdenum discs to a certain extent, there are still some problems and limitations.
[0007] First, the existing grinding and polishing equipment and processes often cannot meet the processing requirements of ultra-thin molybdenum discs, especially when ensuring flatness and roughness while also ensuring that the thickness and shape of the molybdenum discs remain unchanged. Secondly, although the existing heat treatment method can improve the flatness of the molybdenum disc, it may cause the thickness and shape of the molybdenum disc to change, affecting its performance. Therefore, how to avoid changes in its thickness and shape while ensuring the processing accuracy and surface quality of ultra-thin molybdenum discs is an important challenge facing current technology. Summary of the invention
[0008] In order to solve the shortcomings of the prior art and avoid changes in the thickness and shape of the molybdenum disc while ensuring processing accuracy and surface quality, the present invention provides an ultra-thin mirror molybdenum disc and a preparation method and application thereof.
[0009] The present invention provides a method for preparing an ultra-thin mirror-surface molybdenum disc, the steps comprising: Use ultraviolet laser to cut the molybdenum plate to obtain molybdenum discs with preset diameters; The molybdenum disc is leveled at high temperature and then cooled to room temperature with the furnace; The molybdenum disc cooled to room temperature is double-sided ground; The double-sided ground molybdenum disc is double-sided polished to obtain an ultra-thin mirror-finished molybdenum disc.
[0010] In a preferred embodiment, the preparation method further includes: before high-temperature leveling, it also includes the step of removing micro burrs on the molybdenum disc using a magnetic polishing device.
[0011] More preferably, the roughness of the molybdenum disc subjected to high temperature leveling is Ra≦0.5 μm.
[0012] In a preferred embodiment, the purity of the molybdenum plate is >99.9%, preferably >99.99%, and more preferably >99.999%.
[0013] Preferably, the molybdenum plate is a cross-rolled molybdenum plate to reduce various anisotropies caused by texture.
[0014] Preferably, the cross-tying includes one or more of 45° cross-tying, 90° cross-tying, 45° and 90° alternating tying, and reversing cross-tying.
[0015] In a preferred embodiment, the frequency of the magnetic polishing is 5-35 Hz, preferably 8-30 Hz, and more preferably 10-25 Hz.
[0016] In a preferred embodiment, the magnetic polishing time is 5-100 min, preferably 8-70 min, and more preferably 10-60 min.
[0017] In a preferred embodiment, the heating rate of the high temperature leveling is <25°C / min, preferably <20°C / min, and more preferably <15°C / min.
[0018] In a preferred embodiment, the insulation temperature range of the high temperature leveling is 300-1000°C, preferably 500-950°C, and more preferably 700-950°C.
[0019] In a preferred embodiment, the insulation time of the high temperature leveling is 0.5-5h, preferably 0.8-4.5h, and more preferably 1-3h.
[0020] In a preferred embodiment, the double-sided grinding is performed 1-5 times, preferably 2-3 times.
[0021] In a preferred embodiment, the grinding medium for double-sided grinding includes one or more combinations of a grinding stone, a grinding wheel, sandpaper, a diamond abrasive wheel, an aluminum oxide abrasive wheel, and a silicon carbide abrasive wheel.
[0022] Preferably, the grinding media for double-sided grinding are 800-3000# specific structure aluminum oxide, rust-proof grinding fluid and pure water.
[0023] More preferably, the grinding media for double-sided grinding are 2000-3000# specific structure aluminum oxide, rust-proof grinding liquid and pure water.
[0024] In a preferred embodiment, the material of the double-sided grinding wheel includes one or more of blue steel, aluminum oxide, silicon carbide, cubic boron nitride, and diamond.
[0025] In a preferred embodiment, the double-sided grinding pressure is 200-1000N, preferably 300-950N, and more preferably 500-900N.
[0026] In a preferred embodiment, the rotation speed of the double-sided grinding is 3-25 rpm, preferably 5-20 rpm, and more preferably 8-17 rpm.
[0027] In a preferred embodiment, the double-sided grinding time is 1-10 hours, preferably 2-8 hours, and more preferably 3-5 hours.
[0028] In a preferred embodiment, the flatness of the double-sided ground molybdenum disc is ≦0.1 mm and the roughness is Ra ≦0.1 μm.
[0029] In a preferred embodiment, the preparation method of the present application further includes the step of ultrasonically cleaning the double-sided ground molybdenum disc after the double-sided grinding and before the double-sided polishing.
[0030] In a preferred embodiment, the double-sided polishing is performed 1-5 times, preferably 1-3 times.
[0031] In a preferred embodiment, the double-sided polishing includes mechanical polishing, chemical mechanical polishing, double-sided automatic polishing machine polishing or double-sided mirror polishing.
[0032] Preferably, the polishing materials used for the double-sided polishing include one or more of polishing paste (such as tungstic acid, aluminum oxide, silicon dioxide, zirconium oxide, cerium oxide), polishing cloth (such as damping cloth, velvet cloth, felt, fur, fabric), polishing wax (the main component is natural oil wax of animal, plant or mineral origin), polishing disc and polishing liquid.
[0033] In a preferred embodiment, the polishing medium for double-side polishing includes one or more combinations of silicon carbide, aluminum oxide, and silica gel.
[0034] Preferably, the polishing media for double-sided polishing are nano-SiO2 solution and deionized water.
[0035] In a preferred embodiment, the material of the double-sided polishing wheel includes one or more combinations of 304 stainless steel, nylon, polyester, and flannel.
[0036] In a preferred embodiment, the pressure of the double-sided polishing is 200-1200N, preferably 300-1000N, and more preferably 500-900N.
[0037] In a preferred embodiment, the rotation speed of the double-sided polishing is 3-30 rpm, preferably 5-25 rpm, and more preferably 8-20 rpm.
[0038] In a preferred embodiment, the double-sided polishing has a polishing time of 2-15 hours, preferably 2.5-8 hours, and more preferably 3-5 hours.
[0039] In a preferred embodiment, after the molybdenum disc is double-sided polished, the double-sided polished molybdenum disc is ultrasonically cleaned.
[0040] In a preferred embodiment, the preparation method described in the present application, after the molybdenum disc is double-sided polished, further includes the step of high-precision ceramic tooling to obtain the ultra-thin mirror-finished molybdenum disc.
[0041] The present invention also provides an ultra-thin mirror-surface molybdenum disc obtained by the preparation method, the flatness of which is ≤0.05 mm and the roughness Ra is ≤10 nm.
[0042] The present invention also provides an application of the ultra-thin mirror molybdenum disc, which can be applied in the field of semiconductor materials, especially in the application field of high-power LED chip substrates.
[0043] In this application specification, "cross rolling" refers to a technique of changing the rolling direction during the metal rolling process.
[0044] In the present application, "45° cross rolling" means that during the rolling process, the metal plate and strip are rolled along their length direction and then rotated 45° for rolling.
[0045] In the present application, "90° cross rolling" means that during the rolling process, the metal plate and strip are rolled along their length direction and then rotated 90° for rolling.
[0046] In the present application, "45° and 90° alternating rolling" means that during the rolling process, the metal sheet and strip is rolled along its length direction, then rotated 45° for rolling, and then rotated 90° for rolling.
[0047] In the present application, "reversing cross rolling" means that during the rolling process, the metal plate and strip are rolled along their length direction and then rotated 180 degrees for rolling.
[0048] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides an ultra-thin mirror molybdenum disc and a preparation method and application thereof, which can prepare ultra-thin mirror molybdenum discs with high flatness (flatness ≦0.05mm) and low roughness (Ra≦10nm), meeting the high requirements of semiconductor manufacturing for materials. The method combines a variety of technical means, adopts low-stress, low-deformation ultraviolet laser cold cutting technology, high-temperature leveling, double-sided grinding and polishing, and precise processing parameters; eliminates the influence of processing thermal stress and burrs on subsequent grinding and polishing, improves the grinding quality, and ensures that the molybdenum disc obtains high flatness while not causing changes in its thickness and shape. At the same time, the method of the present invention is simple and easy to implement, and is suitable for large-scale production. Compared with the existing chemical mechanical grinding, the present invention does not require special equipment and complex processes, only ordinary grinding and polishing equipment and high-temperature heat treatment equipment are needed to achieve high-precision processing of ultra-thin molybdenum discs, and has broad application prospects. DETAILED DESCRIPTION
[0049] The present invention provides an ultra-thin mirror molybdenum disc and a preparation method thereof and an application thereof. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail with examples below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0050] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged under appropriate circumstances. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0051] The following examples are not intended to limit the present invention in any way.
[0052] Embodiment 1: This embodiment provides a method for preparing an ultra-thin mirror-finish molybdenum wafer, the steps comprising: S1. UV laser cutting of molybdenum plates: Select molybdenum plates with purity > 99.99% and cross-rolled in alternating directions of 45° and 90° as raw materials, and cut them according to the preset diameter through high-precision UV laser cutting equipment to obtain initial molybdenum discs. This high-purity molybdenum plate ensures the basic performance of ultra-thin mirror molybdenum discs, while cross-rolling reduces the anisotropy caused by texture and improves the uniformity of the material.
[0053] S2, magnetic polishing to remove micro burrs: Place the initial molybdenum disc in S1 in the magnetic polishing equipment, set the frequency of magnetic polishing to 20Hz, and the polishing time to 30 minutes. Through the fine treatment of magnetic polishing, the micro burrs on the surface of the molybdenum disc are effectively removed, providing a good foundation for subsequent processing.
[0054] S3, high temperature leveling and furnace cooling: The molybdenum disc with micro-burrs removed in S2 is placed in a high temperature leveling furnace, and the heating rate is set to 10℃ / min, the holding temperature range is 800℃, and the holding time is 2 hours. Then, it is cooled to room temperature in the furnace. S3 improves the flatness of the molybdenum disc through high temperature leveling, and avoids internal stress concentration and deformation caused by rapid cooling through furnace cooling.
[0055] S4, graded double-sided grinding: The molybdenum disc cooled to room temperature in S3 is double-sided ground. The grinding medium for double-sided grinding is 2000-grade specific structure aluminum oxide, anti-rust grinding liquid and a certain proportion of pure water. The grinding wheel is made of aluminum oxide, the grinding pressure is set to 600N, the rotation speed is 15rpm, and the grinding time is 4 hours. The double-sided grinding is performed twice, and ultrasonic cleaning is performed after each grinding to remove debris and residues generated during the grinding process.
[0056] S5, double-sided polishing: Double-sided polishing of the molybdenum disc after double-sided grinding in S4. The number of polishing is 2 times, and the polishing time is adjusted according to the polishing effect. The polishing medium is nano-SiO2 solution and a certain amount of deionized water. The polishing wheel is made of 304 stainless steel, the pressure is 500N, the speed is 10rpm, the polishing time is 3h, and the ultrasonic cleaning and drying are performed after polishing. During the polishing process, the polishing pressure and speed are strictly controlled to ensure that the surface of the molybdenum disc reaches a mirror effect while maintaining the stability of its thickness and shape.
[0057] S6, tooling: the polished molybdenum disc obtained in S5 is subjected to high-precision ceramic tooling.
[0058] After the above steps, an ultra-thin mirror molybdenum disc is finally obtained, and its flatness is detected by white light interferometer and its roughness is detected by atomic force microscope. The molybdenum disc not only has excellent electrical conductivity and thermal conductivity, but also has high surface quality, high flatness (flatness ≦0.05mm), low roughness (Ra≦10nm), thickness of only 0.09mm, high uniformity, and stable shape, which meets the needs of modern semiconductor devices for high-precision and high-performance materials. In addition, by the method of this embodiment, an ultra-thin mirror molybdenum disc with a diameter of 50-150mm can be obtained.
[0059] Embodiment 2: This embodiment provides a method for preparing an ultra-thin mirror-finish molybdenum wafer, the steps comprising: S1. UV laser cutting of molybdenum plate: Select molybdenum plate with purity > 99.99% which is cross-rolled in alternating directions of 45° and 90° as raw material, and cut it according to the preset diameter through high-precision UV laser cutting equipment to obtain the initial molybdenum disc.
[0060] S2. Magnetic polishing to remove micro-burrs: Place the initial molybdenum disc in S1 into the magnetic polishing equipment, set the frequency of magnetic polishing to 25 Hz, and the polishing time to 60 minutes.
[0061] S3, high temperature leveling and furnace cooling: The molybdenum disc with micro-burrs removed in S2 is placed in a high temperature leveling furnace, and the heating rate is set to 15°C / min, the holding temperature range is 700°C, and the holding time is 2 hours. Then, it is cooled to room temperature in the furnace.
[0062] S4, graded double-sided grinding: The molybdenum disc cooled to room temperature in S3 is double-sided ground. The grinding medium for double-sided grinding is 1000# specific structure aluminum oxide, anti-rust grinding liquid and a certain proportion of pure water. The grinding wheel is made of aluminum oxide, the grinding pressure is set to 700N, the rotation speed is 15rpm, and the grinding time is 4 hours. The double-sided grinding is performed twice, and ultrasonic cleaning is performed after each grinding to remove debris and residues generated during the grinding process.
[0063] S5, double-sided polishing: Double-sided polishing of the molybdenum disc after double-sided grinding in S4. The number of polishing is 2 times, and the polishing time is adjusted according to the polishing effect. The polishing medium is nano-SiO2 solution and a certain amount of deionized water. The polishing wheel is made of 304 stainless steel, the pressure is 600N, the speed is 15rpm, the polishing time is 3h, and the ultrasonic cleaning and drying are performed after polishing. During the polishing process, the polishing pressure and speed are strictly controlled to ensure that the surface of the molybdenum disc reaches a mirror effect while maintaining the stability of its thickness and shape.
[0064] S6, tooling: the polished molybdenum disc obtained in S5 is subjected to high-precision ceramic tooling.
[0065] After the above steps, an ultra-thin mirror molybdenum disc is finally obtained, and its flatness is detected by white light interferometer and its roughness is detected by atomic force microscope. The molybdenum disc not only has excellent electrical conductivity and thermal conductivity, but also has high surface quality, high flatness (flatness ≦0.05mm), low roughness (Ra≦10nm), thickness of only 0.09mm, high uniformity, and stable shape, which meets the needs of modern semiconductor devices for high-precision and high-performance materials. In addition, by the method of this embodiment, an ultra-thin mirror molybdenum disc with a diameter of 50-150mm can be obtained.
[0066] Embodiment 3: This embodiment provides a method for preparing an ultra-thin mirror-finish molybdenum wafer, the steps comprising: S1. UV laser cutting of molybdenum plate: Select molybdenum plate with purity > 99.99% which is cross-rolled in alternating directions of 45° and 90° as raw material, and cut it according to the preset diameter through high-precision UV laser cutting equipment to obtain the initial molybdenum disc.
[0067] S2. Magnetic polishing to remove micro-burrs: Place the initial molybdenum disc in S1 into the magnetic polishing equipment, set the frequency of magnetic polishing to 20 Hz, and the polishing time to 50 minutes.
[0068] S3, high temperature leveling and furnace cooling: The molybdenum disc with micro-burrs removed in S2 is placed in a high temperature leveling furnace, and the heating rate is set to 15°C / min, the holding temperature range is 800°C, and the holding time is 3 hours. Then, it is cooled to room temperature in the furnace.
[0069] S4, graded double-sided grinding: The molybdenum disc cooled to room temperature in S3 is double-sided ground. The grinding medium for double-sided grinding is 2000 specific structure aluminum oxide, rust-proof grinding liquid and a certain proportion of pure water. The grinding wheel is made of aluminum oxide, the grinding pressure is set to 900N, the rotation speed is 15rpm, and the grinding time is 4 hours. The double-sided grinding is performed twice, and ultrasonic cleaning is performed after each grinding to remove debris and residues generated during the grinding process.
[0070] S5, double-sided polishing: Double-sided polishing of the molybdenum disc after double-sided grinding in S4. The number of polishing is 2 times, and the polishing time is adjusted according to the polishing effect. The polishing medium is nano-SiO2 solution and a certain amount of deionized water. The polishing wheel is made of 304 stainless steel, the pressure is 900N, the speed is 15rpm, the polishing time is 4h, and the ultrasonic cleaning and drying are performed after polishing. During the polishing process, the polishing pressure and speed are strictly controlled to ensure that the surface of the molybdenum disc reaches a mirror effect while maintaining the stability of its thickness and shape.
[0071] S6, tooling: the polished molybdenum disc obtained in S5 is subjected to high-precision ceramic tooling.
[0072] After the above steps, an ultra-thin mirror molybdenum disc is finally obtained, and its flatness is detected by white light interferometer and its roughness is detected by atomic force microscope. The molybdenum disc not only has excellent electrical conductivity and thermal conductivity, but also has high surface quality, high flatness (flatness ≦0.05mm), low roughness (Ra≦10nm), thickness of only 0.09mm, high uniformity, and stable shape, which meets the needs of modern semiconductor devices for high-precision and high-performance materials. In addition, by the method of this embodiment, an ultra-thin mirror molybdenum disc with a diameter of 50-150mm can be obtained.
[0073] Comparative Example 1: This comparative example provides a method for preparing a conventional molybdenum disc, the steps comprising: S1. Molybdenum plate stamping: Select unidirectional rolled molybdenum plate with purity > 99.99% as raw material, and obtain the initial molybdenum disc by mechanical cutting and stamping.
[0074] S2. The initial molybdenum disc of S1 is placed in a muffle furnace for annealing, and the heating rate is set to 15°C / min, the holding temperature range is 800°C, and the holding time is 2 hours. Then, the molybdenum disc is cooled to room temperature in the furnace.
[0075] S3, machining: The molybdenum discs of S2 are subjected to machining such as turning, milling, and grinding to further adjust the size and shape and remove surface burrs and defects.
[0076] S4, polishing: polishing the molybdenum disc obtained in S3, and precisely grinding the molybdenum disc to achieve a mirror effect.
[0077] The performance results of the molybdenum discs obtained in Examples 1-3 and Comparative Example 1 are recorded in Table 1.
[0078] Table 1. Performance results of molybdenum discs of Examples 1-3 and Comparative Example 1 In summary, compared with Comparative Example 1, Examples 1-3 of the present invention obtain ultra-thin mirror molybdenum discs with good electrical and thermal conductivity, high flatness (flatness ≦0.05mm) and low roughness (Ra≦10nm). By adopting cross-rolled molybdenum plate raw materials, the anisotropy caused by texture is reduced, which is convenient for subsequent processing. Secondly, the shape processing of the molybdenum disc of the present invention abandons the traditional stamping process and adopts low-stress, low-deformation ultraviolet laser cold cutting, which eliminates the influence of processing thermal stress and stamping burrs on subsequent grinding and polishing. In addition, the present invention uses magnetic polishing technology to eliminate surface defects and cut micro-burrs before double-sided grinding, which greatly improves the quality of grinding. The present invention also combines high-temperature leveling technology: after magnetic polishing, the ultra-thin molybdenum disc is subjected to high-temperature leveling treatment. By precisely controlling the leveling temperature, time and cooling rate, the ultra-thin molybdenum disc can obtain high flatness without causing changes in its thickness and shape. At the same time, the double-sided grinding and polishing technology adopted by the present invention performs graded double-sided grinding on the molybdenum disc to ensure the stability of its thickness and shape; then, by accurately controlling the grinding parameters, such as pressure, rotation speed, grinding time, etc., the processing accuracy and surface quality of the ultra-thin molybdenum disc are ensured. Finally, through polishing, the roughness of the ultra-thin molybdenum disc is further reduced and its flatness is improved. In addition, embodiments 1-3 of the present invention also use high-precision ceramic tooling, which also improves the flatness and accuracy of the molybdenum disc.
[0079] The specific embodiments of the present invention are described in detail above, but they are only examples, and the present invention is not limited to the specific embodiments described above. For those skilled in the art, any equivalent modifications and substitutions made to the present invention are also within the scope of the present invention. Therefore, the equalization changes and modifications made without departing from the spirit and scope of the present invention should be included in the scope of the present invention.
Claims
1. A method for preparing an ultra-thin mirror-finished molybdenum disc, characterized in that the steps include: Use ultraviolet laser to cut the molybdenum plate to obtain molybdenum discs with preset diameters; The molybdenum disc with the micro-burrs removed is leveled at high temperature and then cooled to room temperature in the furnace; The molybdenum disc cooled to room temperature is double-sided ground; The double-sided ground molybdenum disc is double-sided polished to obtain an ultra-thin mirror-finished molybdenum disc.
2. The method according to claim 1, characterized in that The preparation method further comprises: before high-temperature leveling, a step of removing micro-burrs on the molybdenum disc by using a magnetic polishing device.
3. The method according to claim 2, characterized in that The frequency of the magnetic polishing is 5-35 Hz, preferably 8-30 Hz, more preferably 10-25 Hz; and / or The magnetic polishing time is 5-100 min, preferably 8-70 min, more preferably 10-60 min.
4. The method according to claim 1, characterized in that: The heating rate of the high temperature leveling is less than 25°C / min, preferably less than 20°C / min, more preferably less than 15°C / min; and / or The high temperature leveling has a holding temperature range of 300-1000° C., preferably 500-950° C., more preferably 700-950° C.; and / or The insulation time of the high temperature leveling is 0.5-5h, preferably 0.8-4.5h, and more preferably 1-3h.
5. The method according to claim 1, characterized in that The double-sided grinding pressure is 200-1000N, preferably 300-950N, more preferably 500-900N; and / or The rotation speed of the double-sided grinding is 3-25 rpm, preferably 5-20 rpm, more preferably 8-17 rpm; The double-sided grinding time is 1-10 hours, preferably 2-8 hours, and more preferably 3-5 hours.
6. The method according to claim 1, characterized in that The polishing material used in the double-sided polishing includes one or more of a polishing disc, a polishing cloth, and a polishing liquid; and / or The polishing medium for double-sided polishing includes one or more combinations of silicon carbide, aluminum oxide, and silica gel; preferably, The polishing media for double-sided polishing are nano-SiO2 solution and deionized water.
7. The method according to claim 1, characterized in that The material of the double-sided polishing polishing wheel includes one or more combinations of 304 stainless steel, nylon, polyester, and flannel.
8. The method according to claim 1, characterized in that The double-sided polishing pressure is 200-1200N, preferably 300-1000N, more preferably 500-900N; and / or The rotation speed of the double-sided polishing is 3-30 rpm, preferably 5-25 rpm, more preferably 8-20 rpm; and / or The double-sided polishing has a polishing time of 2-15 hours, preferably 2.5-8 hours, and more preferably 3-5 hours.
9. An ultra-thin mirror-finished molybdenum disc obtained based on the method of claims 1-8, characterized in that: The flatness of the ultra-thin mirror-finished molybdenum disc is ≤ 0.05 mm; and / or Roughness Ra ≤ 10nm.
10. An application of the ultra-thin mirror-finished molybdenum disc according to claim 9, characterized in that: The ultra-thin mirror molybdenum disc is used in the field of semiconductor materials, especially in the application field of high-power LED chip substrates.
Citation Information
Patent Citations
Tungsten molybdenum alloy foil material polishing method and obtained product
CN109926907A
Grinding and polishing method for molybdenum wafer
CN111599673A
Precise and efficient cutting method for sheet molybdenum metal
CN112171189A
Double-sided polished molybdenum substrate and preparation method thereof as well as application thereof to LED light-emitting chips
CN112454160A
Ultraviolet laser machining system of diaphragm for scanning electron microscope
CN201154415Y
Cited By
Molybdenum wafer low-temperature preparation method and obtained molybdenum wafer
CN121042828A