Sand-containing colorful environment-friendly coating and preparation method thereof

By introducing cross-linking reaction between organic polymer suspension agent and special protective glue solution in water-based colorful coatings, the shortcomings in weather resistance and storage stability of existing coatings are solved, and better decorative effects and environmental protection are achieved.

CN118879141APending Publication Date: 2024-11-01HE BEI LAN TING SHI XIN XING JIAN CAI YOU XIAN GONG SI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411106654.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing water-based colorful paints ignore the overall weather resistance in the decorative effect, the product lacks coarse ore feel, insufficient storage stability, and the color points are easily gelatinized, which cannot truly reflect the effect of burnt stone.

Method used

The preparation method of sand-containing colorful environmentally friendly coatings, including pigment components, dispersion medium components and varnish components, and the use of organic polymer suspension agents and special protective glue solutions to improve the storage stability and construction stability of the coating through cross-linking reaction. , enhances the adhesion and water resistance of the dry film.

Benefits of technology

The stability, appearance effect and dry film performance of the paint are improved, ensuring the long-term storage stability of color points and the simplicity of construction, reducing transportation costs and energy consumption, and improving environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118879141A_ABST
    Figure CN118879141A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of coatings, and discloses a sand-containing colorful environment-friendly coating and a preparation method thereof, and the sand-containing colorful environment-friendly coating comprises a pigment component, a dispersion medium component and a varnish component; the pigment component is prepared from the following raw materials: water, natural white sand, cellulose, a dispersing agent, pigment filler, a defoaming agent, a coalescing agent, an emulsion, an anti-freezing solution, a protective glue solution, a pH regulator and a sterilizing agent; the dispersion medium component comprises the following raw materials: water, an organic polymer suspending agent, a protective glue solution and a coupling agent; the varnish component comprises the following raw materials: water, an emulsion, a pH regulator, a bactericide, a defoaming agent, a coalescing agent, an antifreezing agent and a thickening agent; wherein the organic polymer suspending agent is bentonite, the protective glue solution is a magnesium lithium silicate aqueous solution, and the coupling agent is a titanate coupling agent. According to the invention, single-component packaging is adopted, and a cross-linking reaction principle is introduced, so that the coating can achieve three purposes of strong stability, good aesthetic property and strong dry film property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coatings, and in particular to a sand-containing colorful environmentally friendly coating and a preparation method thereof. Background Art

[0002] Nowadays, the use of natural granite as a decorative material for the interior and exterior facades of buildings is gradually being phased out due to the difficulties in natural stone mining, the damage and pollution to the natural environment caused by mining, the natural color difference of stone source mines, and the poor safety of dry-hanging stone. Based on the above situation, color effect coatings that replace natural granite have emerged in the form of coatings.

[0003] In recent years, water-based multi-color paint has been a hot product in the field of building interior and exterior wall decorative paint. Due to its outstanding decorative effect, the product can be sprayed on the surface of latex paint or natural stone paint at one time. After drying, it can present a variety of color patterns at the same time, with realistic image effects, similar to the appearance of granite decorative effects. Compared with natural granite, it has a great price advantage and saves decoration costs. At the same time, the paint layer is thin and light, the construction process is simple, and the safety and environmental protection are greatly improved compared with natural dry-hanging stone. It is very suitable for the decoration of interior and exterior facades of high-end buildings such as office buildings, hotels, homes, hospitals, villas, etc., to enhance the image and grade of the buildings.

[0004] However, the quality of burnt noodle products on the market is mixed. Most of the existing technical solutions are single-component packaging, the materials are not flexible, and only the decorative effect is considered, resulting in the neglect of the overall weather resistance. The product lacks a rough mineral feel and cannot truly reflect the effect of the burnt noodle stone. The product is not stable enough in storage, and the colored dots are easily gelatinized due to the overall thickening. Summary of the invention

[0005] In view of this, in order to solve the above problems, the present invention proposes a sand-containing colorful environmentally friendly coating and a preparation method thereof.

[0006] The invention provides a sand-containing colorful environmentally friendly paint, which comprises the following raw materials in parts by weight: the sand-containing colorful environmentally friendly paint comprises a pigment component, a dispersion medium component and a varnish component;

[0007] The pigment components include the following raw materials: water, natural white sand, cellulose, dispersant, pigment filler, defoamer, film-forming aid, emulsion, antifreeze solution, protective glue solution, pH regulator and bactericide;

[0008] The dispersion medium components include the following raw materials: water, organic polymer suspension agent, protective colloid solution and coupling agent;

[0009] The varnish component includes the following raw materials: water, emulsion, pH regulator, bactericide, defoamer, film-forming aid, antifreeze agent and thickener;

[0010] Wherein, the organic polymer suspending agent is bentonite, the protective colloid solution is a lithium magnesium silicate aqueous solution, and the coupling agent is a titanate coupling agent.

[0011] Furthermore, the pigment component includes the following raw materials in parts by weight: 35.5 parts of water, 40 parts of natural white yarn, 0.7 parts of cellulose, 0.1 parts of dispersant, 1.1 parts of pigment filler, 0.2 parts of defoamer, 1 part of film-forming aid, 0.5 parts of emulsion, 0.8 parts of antifreeze, 5 parts of protective glue solution, 0.2 parts of pH regulator and 0.4 parts of fungicide;

[0012] The dispersion medium component includes the following raw materials in parts by weight: 48.8 parts of water, 0.2 parts of organic polymer suspending agent, 50 parts of protective colloid solution and 1 part of coupling agent;

[0013] The varnish component includes the following raw materials in parts by weight: 29.4 parts of water, 65 parts of emulsion, 0.2 parts of pH regulator, 0.3 parts of bactericide, 0.2 parts of defoamer, 3.3 parts of film-forming aid, 0.8 parts of antifreeze agent and 0.8 parts of thickener.

[0014] Furthermore, the emulsion is a mixture of one or more of water-based acrylic resin, silicone water-based acrylic resin, and water-based polyurethane resin; the cellulose is hydroxyethyl cellulose ether; the dispersant is a hydrophobic copolymer sodium salt dispersant; the defoaming agent is a mixture of one or more of modified polysiloxane and silicone modified mineral oil; the color filler is one or a mixture of calcined kaolin, heavy calcium, mica powder, talcum powder, and rutile titanium dioxide; the film-forming aid is dodecanol ester; the antifreeze agent is propylene glycol; the pH regulator is 2-amino-2-methyl-1-propanol; and the bactericide is a nitrogen-sulfur heterocyclic compound that does not contain organic volatiles.

[0015] Furthermore, the thickener is one or a mixture of hydrophobically modified alkali-soluble emulsion thickener and associative polyurethane thickener.

[0016] On the other hand, the present invention also proposes a method for preparing a sand-containing colorful environmentally friendly coating, which is applied to the above-mentioned sand-containing colorful environmentally friendly coating, comprising:

[0017] The pigment component is obtained by mixing water, natural white sand, cellulose, dispersant, pigment filler, defoamer, film-forming aid, emulsion, antifreeze solution, protective glue solution, pH regulator and bactericide;

[0018] Mixing water, organic polymer suspension agent, protective colloid solution and coupling agent to obtain a dispersion medium component;

[0019] The varnish component is obtained by mixing water, emulsion, pH regulator, bactericide, defoamer, film-forming aid, antifreeze agent and thickener.

[0020] Further, the preparation steps of the pigment component include:

[0021] Add water to the dispersion tank, add cellulose in sequence, disperse for 15-20 minutes, add dispersant, pigment filler, defoamer in sequence, disperse at high speed for 30 minutes and keep the dispersion speed at 1000-1200rpm;

[0022] Reduce the dispersion speed to 800-1000rpm, and add film-forming aid, antifreeze agent, emulsion, protective glue solution, PH regulator, fungicide, natural white sand, and thickener in sequence. After adding the thickener, increase the dispersion speed by 5-25%, stir at a constant speed for 5-15 minutes, obtain the pigment component and take it out for use.

[0023] Further, the preparation steps of the dispersion medium component are:

[0024] Add water into the dispersion tank, add organic polymer suspending agent in sequence, and disperse at high speed for 30-40 minutes at a dispersion speed of 1000-1200rpm;

[0025] Reduce the dispersion speed to 800-1000rpm, protect the colloid solution, increase the dispersion speed by 5-25% after adding the coupling agent, stir at a constant speed for 5-15 minutes, obtain the dispersion medium and take it out for use.

[0026] Further, the preparation steps of the varnish component:

[0027] Add water and emulsion into the dispersion tank, add pH regulator, bactericide, defoamer, antifreeze agent and film-forming aid in sequence while stirring, stirring speed is 500-800rpm, add thickener, increase the dispersion speed to 900-1200rpm, stir at a constant speed for 5-15min, test the viscosity and store for later use.

[0028] Furthermore, the water is RO water.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] For the protective liquid with lubricating and isolating functions, usually only inorganic gels such as silicate are used. However, the present invention develops a special organic polymer protective glue based on the inorganic gel to cooperate with it, so as to ensure that the storage stability and construction stability of the sand-containing colorful environmentally friendly coating are better, and the adhesion and water resistance of the dry film are better.

[0031] The present invention adopts a single-component packaging, which meets the requirements of transportation stability, is simple and convenient to construct, and is simple and error-prone to on-site operation. Compared with the two-component packaging, the single-component packaging saves transportation costs, reduces energy consumption, and is green and environmentally friendly.

[0032] The present invention can simultaneously achieve the three goals of stability, appearance and dry film performance, and introduces the cross-linking reaction principle into the dispersed phase and the continuous phase, making the formula and process of the whole sand-containing colorful environmentally friendly coating more rigorous and reliable in achieving the above three goals. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. Moreover, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0034] Figure 1 This is a test result diagram of a sand-containing colorful environmentally friendly coating according to an embodiment of the present invention. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] It should be noted that in the following embodiments, water refers to water obtained by purifying water using the RO reverse osmosis principle.

[0037] Example 1

[0038] Components and raw materials

[0039] Pigment components: R0 water, natural white sand, cellulose, dispersant, pigment filler, defoamer, film-forming aid, emulsion, antifreeze, protective glue solution, PH regulator and bactericide;

[0040] Dispersion medium components: water, organic polymer suspension agent, protective gel solution and coupling agent;

[0041] Varnish components: water, emulsion, pH regulator, bactericide, defoamer, film-forming aid, antifreeze agent and thickener;

[0042] Preparation process

[0043] 1. Preparation of pigment components

[0044] Add 35.5 parts of water into the dispersion tank.

[0045] Then, 0.7 parts of hydroxyethyl cellulose ether was added and dispersed for 15-20 minutes.

[0046] Add 0.1 parts of hydrophobic copolymer sodium salt dispersant, 1.1 parts of pigments and fillers, and 0.2 parts of modified polysiloxane defoamer in sequence, and disperse at high speed for 30 minutes, maintaining the dispersion speed at 1100 rpm.

[0047] Reduce the dispersion speed to 900 rpm, and add in sequence 1 part of dodecyl alcohol ester film-forming aid, 0.8 part of propylene glycol antifreeze agent, 0.5 part of aqueous acrylic resin emulsion, 5 parts of lithium magnesium silicate protective gel solution, 0.2 part of 2-amino-2-methyl-1-propanol pH regulator, 0.4 part of nitrogen and sulfur heterocyclic fungicide and 40 parts of natural white sand.

[0048] After adding the thickener, increase the dispersion speed by 25%, stir at a constant speed for 10 minutes, obtain the pigment component and take it out for use.

[0049] 2. Preparation of dispersion medium components

[0050] Add 48.8 parts of water into the dispersion tank.

[0051] 0.2 parts of bentonite organic polymer suspending agent were added in sequence and dispersed at high speed for 35 minutes at a dispersion speed of 1100 rpm.

[0052] The dispersion speed was reduced to 900 rpm, and after adding 50 parts of lithium magnesium silicate protective colloid solution and 1 part of titanate coupling agent, the dispersion speed was increased by 25%, and stirred at a constant speed for 10 minutes to obtain a dispersion medium, which was taken out for use.

[0053] 3. Preparation of varnish components

[0054] Add 29.4 parts of water and 65 parts of aqueous acrylic resin emulsion into a dispersion tank, and add 0.2 parts of 2-amino-2-methyl-1-propanol pH regulator, 0.3 parts of nitrogen and sulfur heterocyclic fungicide, 0.2 parts of modified polysiloxane defoamer, 0.8 parts of propylene glycol antifreeze and 3.3 parts of dodecyl alcohol ester film-forming aid in sequence while stirring at a stirring speed of 650 rpm.

[0055] Add 0.8 parts of hydrophobically modified alkali-soluble emulsion thickener, increase the dispersion speed to 1100 rpm, stir at a constant speed for 10 minutes, test the viscosity and store for later use.

[0056] Comparative Example 1

[0057] The difference between this comparative example and the embodiment is that:

[0058] The dispersion medium components were prepared according to the following weight proportions: 85 parts of RO water, 0.5 parts of film-forming aid, 0.5 parts of rheological agent, 10 parts of emulsion, 0.2 parts of defoaming agent, 5 parts of protective glue solution and 1 part of coupling agent.

[0059] The rheological agent in this comparative example is bentonite.

[0060] Comparative Example 2

[0061] The difference between this comparative example and the embodiment is that:

[0062] The dispersion medium components are prepared according to the following weight proportions: 65 parts of RO water, 0.5 parts of film-forming aid, 0.5 parts of rheological agent, 10 parts of emulsion, 20 parts of organic polymer protective colloid solution, 0.2 parts of defoamer, 5 parts of protective colloid solution and 1 part of coupling agent.

[0063] Comparative Example 3

[0064] The difference between this comparative example and the embodiment is that:

[0065] The dispersion medium components are prepared according to the following weight proportions: 20 parts of RO water, 0.5 parts of film-forming aid, 0.5 parts of rheological agent, 10 parts of emulsion, 30 parts of organic polymer protective colloid solution, 0.2 parts of defoaming agent, 40 parts of protective colloid solution and 1 part of coupling agent.

[0066] The coatings prepared in the examples and comparative examples 1-3 were sprayed by spraying equipment, and the effects on the materials were observed by naked eyes and graded and evaluated, and the storage stability of the materials was rated. The storage period was half a year (6 months). See Table 1: Data Record Table for details.

[0067] Table 1 Data record table

[0068]

[0069]

[0070] Note: A is the best; B is the middle; C is the worst.

[0071] The results of spraying by adding different proportions of special organic polymer protective glue in the dispersion medium show that the organic polymer protective glue does have a significant effect on the molding effect and storage stability of the color dots. This organic polymer protective glue cannot be molded without adding any material, and the color dots are in a paste state. As the amount of organic polymer protective glue increases, it significantly helps the molding of the color dots, but as the amount of addition increases, the color dots are obviously hard when it reaches 30%, and the overall effect is not good; for storage stability, this organic polymer protective glue cannot be molded without adding any material, and the color dots are in a paste state. As the amount of organic polymer protective glue increases, it significantly helps the storage of the color dots. After 6 months of storage, the material is taken out and sprayed evenly, and the color dots are clear and not gelatinized. However, as the amount of addition increases, when it reaches 30%, the color dots are complete after 6 months of storage, but slightly smaller and harder, and the overall effect is not good. Therefore, it can be seen that this organic polymer protective glue has a significant effect on the overall sand-containing colorful environmentally friendly coating.

[0072] The dispersed medium components of the embodiment were handed over to the National Building Materials Industry Building Materials and Structure Safety Quality Supervision and Inspection Center of Beijing National Testing Holding Group Co., Ltd. The test results are as follows: Figure 1 shown.

[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the specific implementation methods of the present invention can still be modified or replaced by equivalents. Any modification or equivalent replacement that does not depart from the spirit and scope of the present invention should be covered within the scope of protection of the claims of the present invention.

Claims

1. A sand-containing colorful environmentally friendly paint, characterized in that: The sand-containing colorful environmentally friendly paint comprises a pigment component, a dispersion medium component and a varnish component; The pigment components include the following raw materials: water, natural white sand, cellulose, dispersant, pigment filler, defoamer, film-forming aid, emulsion, antifreeze solution, protective glue solution, pH regulator and bactericide; The dispersion medium components include the following raw materials: water, organic polymer suspension agent, protective colloid solution and coupling agent; The varnish component includes the following raw materials: water, emulsion, pH regulator, bactericide, defoamer, film-forming aid, antifreeze agent and thickener; Wherein, the organic polymer suspending agent is bentonite, the protective colloid solution is a lithium magnesium silicate aqueous solution, and the coupling agent is a titanate coupling agent.

2. The sand-containing colorful environmentally friendly paint according to claim 1, characterized in that: The pigment component includes the following raw materials in parts by weight: 35.5 parts of water, 40 parts of natural white yarn, 0.7 parts of cellulose, 0.1 parts of dispersant, 1.1 parts of pigment filler, 0.2 parts of defoamer, 1 part of film-forming aid, 0.5 parts of emulsion, 0.8 parts of antifreeze, 5 parts of protective glue solution, 0.2 parts of pH regulator and 0.4 parts of bactericide; The dispersion medium component includes the following raw materials in parts by weight: 48.8 parts of water, 0.2 parts of organic polymer suspending agent, 50 parts of protective colloid solution and 1 part of coupling agent; The varnish component includes the following raw materials in parts by weight: 29.4 parts of water, 65 parts of emulsion, 0.2 parts of pH regulator, 0.3 parts of bactericide, 0.2 parts of defoamer, 3.3 parts of film-forming aid, 0.8 parts of antifreeze agent and 0.8 parts of thickener.

3. The sand-containing colorful environmentally friendly paint according to claim 2, characterized in that: The emulsion is a mixture of one or more of water-based acrylic resin, silicone water-based acrylic resin, and water-based polyurethane resin; the cellulose is hydroxyethyl cellulose ether; the dispersant is a hydrophobic copolymer sodium salt dispersant; the defoamer is a mixture of one or more of modified polysiloxane and silicone modified mineral oil; the color filler is one or a mixture of calcined kaolin, heavy calcium, mica powder, talcum powder, and rutile titanium dioxide; the film-forming aid is dodecanol ester; the antifreeze agent is propylene glycol; the pH regulator is 2-amino-2-methyl-1-propanol; and the bactericide is a nitrogen-sulfur heterocyclic compound that does not contain organic volatiles.

4. The sand-containing colorful environmentally friendly paint according to claim 2, characterized in that: The thickener is one or a mixture of hydrophobically modified alkali-soluble emulsion thickener and associative polyurethane thickener.

5. A method for preparing a sand-containing colorful environmentally friendly coating, applied to a sand-containing colorful environmentally friendly coating as claimed in any one of claims 1 to 4, characterized in that: include: The pigment component is obtained by mixing water, natural white sand, cellulose, dispersant, pigment filler, defoamer, film-forming aid, emulsion, antifreeze solution, protective glue solution, pH regulator and bactericide; Mixing water, organic polymer suspension agent, protective colloid solution and coupling agent to obtain a dispersion medium component; The varnish component is obtained by mixing water, emulsion, pH regulator, bactericide, defoamer, film-forming aid, antifreeze agent and thickener.

6. The method for preparing a sand-containing colorful environmentally friendly coating according to claim 5, characterized in that: The preparation steps of the pigment component include: Add water to the dispersion tank, add cellulose in sequence, disperse for 15-20 minutes, add dispersant, pigment filler, defoamer in sequence, disperse at high speed for 30 minutes and keep the dispersion speed at 1000-1200rpm; Reduce the dispersion speed to 800-1000rpm, and add film-forming aid, antifreeze agent, emulsion, protective glue solution, PH regulator, fungicide, natural white sand, and thickener in sequence. After adding the thickener, increase the dispersion speed by 5-25%, stir at a constant speed for 5-15 minutes, obtain the pigment component and take it out for use.

7. The method for preparing a sand-containing colorful environmentally friendly coating according to claim 5, characterized in that: Preparation steps of dispersion medium components: Add water into the dispersion tank, add organic polymer suspending agent in sequence, and disperse at high speed for 30-40 minutes at a dispersion speed of 1000-1200rpm; Reduce the dispersion speed to 800-1000rpm, protect the colloid solution, increase the dispersion speed by 5-25% after adding the coupling agent, stir at a constant speed for 5-15 minutes, obtain the dispersion medium and take it out for use.

8. The method for preparing a sand-containing colorful environmentally friendly coating according to claim 5, characterized in that: Steps for making varnish components: Add water and emulsion into the dispersion tank, add pH regulator, bactericide, defoamer, antifreeze agent and film-forming aid in sequence while stirring, stirring speed is 500-800rpm, add thickener, increase the dispersion speed to 900-1200rpm, stir at a constant speed for 5-15min, and then store for later use.

9. The method for preparing a sand-containing colorful environmentally friendly coating according to claim 5, characterized in that: The water is RO water.

Citation Information

Patent Citations

  • High-solid-content interior and exterior crosslinked type water-in-water colorful granite paint and preparation method thereof

    CN102391767A

  • Sand-in-water colorful imitation stone paint

    CN104312351A

  • Sand-containing colorful environment-friendly coating and preparation method of same

    CN106366814A

  • Hemp sand coating and preparation method thereof

    CN115124898A