Wear-resistant water-based road marking paint and preparation method thereof

By using composite resin and wear-resistant components in water-based road marking coatings, the problem of insufficient wear resistance and service life of water-based marking coatings is solved, and the wear resistance and dirt resistance of marking coatings is achieved. The improvement of reflectivity extends the service life and meets the needs of green environmental protection and traffic safety.

CN118879162APending Publication Date: 2024-11-01BAODING KESHUNDA TRAFFIC FACILITY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411308256.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-19
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The existing water-based road marking coatings have short wear resistance and service life, which are prone to sticking and dirty, making them difficult to meet the needs of green environmental protection and traffic safety.

Method used

Using a combination of composite resin, wear-resistant components, cellulose, dispersant, wetting agent, defoaming agent and additives, wear-resistant water-resistant road marking coatings are prepared through agitation and dispersion process to improve the wear resistance and reflectivity of the coatings. .

Benefits of technology

It significantly improves the wear resistance, dirt resistance and reflectivity of the marking coating, extends its service life, and meets the requirements of green environmental protection and traffic safety.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of road marking coatings, in particular to a wear-resistant water-based road marking coating and a preparation method thereof.The wear-resistant water-based road marking coating is prepared from, by mass, 80-100 parts of composite resin, 120-300 parts of wear-resistant component, 1-10 parts of cellulose, 0.1-5 parts of dispersing agent, 0.1-5 parts of wetting agent, 0.1-5 parts of defoaming agent, 0.1-5 parts of additive and 100-150 parts of solvent. According to the wear-resistant water-based road marking coating adopting the components and the preparation method thereof, the marking coating provided by the invention has excellent wear resistance, dirt resistance and light reflection, and the service life of the marking coating is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road marking paints, and in particular to a wear-resistant water-based road marking paint and a preparation method thereof. Background Art

[0002] Road marking is an important part of traffic safety facilities. It can provide the required information visually, guide road traffic and ensure the safety of drivers and pedestrians. Road marking paints are divided into four categories: solvent-based, hot-melt, two-component and water-based road marking paints. Solvent-based road marking paints use organic substances as solvents, and emit a large amount of organic compounds (VOCs) during construction, which will pollute the surrounding environment and harm the health of construction workers. Hot-melt road marking paints use natural resins or petroleum resin synthetic materials as film-forming materials. The heating process is complicated during construction, and toxic gases are also released during the heating process. At the same time, it is easy to stick to dust and dirt during use. Under the background of the concept of green highway construction and the promotion of the realization of dual carbon goals, new green, environmentally friendly, energy-saving and material-saving water-based road marking products have been widely promoted and used.

[0003] Water-based road markings are road markings that use water as a solvent and water-soluble or water-emulsified resins as film-forming materials. Because the coating of water-based road markings is thinner, its wear resistance is relatively weaker than that of solvent-based road markings. In the later stages of use, water-based road marking paints have problems such as short life, poor wear resistance, and easy sticking and dirtiness. Summary of the invention

[0004] The purpose of the present invention is to provide a wear-resistant water-based road marking paint and a preparation method thereof. The provided road marking paint has excellent wear resistance, dirt resistance and reflectivity, and improves the service life of the road marking paint.

[0005] To achieve the above purpose, the present invention provides a wear-resistant water-based road marking paint, wherein the components are calculated by weight: 80-100 parts of composite resin, 120-300 parts of wear-resistant components, 1-10 parts of cellulose, 0.1-5 parts of dispersant, 0.1-5 parts of wetting agent, 0.1-5 parts of defoaming agent, 0.1-5 parts of additives, and 100-150 parts of solvent.

[0006] Preferably, the composite resin includes one or more of polyurethane resin, modified acrylic resin and epoxy resin.

[0007] Preferably, the modified acrylic resin includes one or more of dodecafluoroheptyl methacrylate, polydimethylsiloxy methacrylate and POSS modified acrylic resin.

[0008] Preferably, the wear-resistant component includes one or more of rutile titanium dioxide, heavy calcium, titanium dioxide-supported mesoporous carbon, glass microspheres and modified nano-alumina.

[0009] Preferably, the dispersant includes one or more of an inorganic dispersant, an organic dispersant and an amphoteric dispersant;

[0010] The wetting agent includes one or more of polyethylene glycol ether, ethylene glycol monobutyl ether, alcohol ester and modified silicone.

[0011] Preferably, the additive includes one or more of a leveling agent, ammonia, triethylamine and a silane coupling agent.

[0012] Preferably, the defoaming agent includes one or more of polysiloxane defoaming agents, fatty acid ester defoaming agents, polyether defoaming agents and modified silicone defoaming agents.

[0013] Preferably, the solvent includes one or more of methanol and deionized water.

[0014] The preparation method of the above-mentioned wear-resistant water-based road marking paint comprises the following steps:

[0015] S1. Weigh 80-100 parts of composite resin, 120-300 parts of wear-resistant components, 1-10 parts of cellulose, 0.1-5 parts of dispersant, 0.1-5 parts of wetting agent, 0.1-5 parts of defoaming agent, 0.1-5 parts of additives, and 100-150 parts of solvent by mass;

[0016] S2, putting the composite resin, part of the additives and part of the solvent into a reaction kettle, stirring at 300-400 rpm, and adding the remaining additives, wetting agent, dispersant and defoaming agent in sequence to obtain a mixed system;

[0017] S3, adding the wear-resistant component to the mixed system in S2 in small amounts and multiple times, stirring and dispersing at 1000-1500 rpm to obtain a dispersed system;

[0018] S4. Slowly add the remaining solvent to the dispersed system in S3, stir and mix at 800-1000 rpm, stir and disperse at 1000-1200 rpm, and obtain the road marking paint after sieving.

[0019] Preferably, in S3, the mass ratio of the wear-resistant component to the composite resin is 1-5:1.

[0020] Preferably, in S4, the sieved particle size is 100-150 mesh.

[0021] Therefore, the present invention adopts a wear-resistant water-based road marking paint with the above-mentioned components, and its beneficial effects are as follows: 1. The road marking paint provided by the present invention adopts a composite resin as a coating matrix, and the composite resin is obtained by grafting modified acrylic resin and epoxy resin. The composite resin obtained after grafting contains epoxy resin, modified acrylic resin-epoxy resin and acrylic copolymer resin, and obtains a micellar structure after being dispersed in water. The epoxy group and the epoxy resin are located inside the micelle, and the carboxyl group outside the micelle is neutralized with triethylamine to form a salt. The obtained composite resin water dispersion has high stability and uniform particle size;

[0022] 2. In the titanium dioxide-loaded mesoporous carbon used in the present invention, silicon dioxide is doped in the pores of the mesoporous carbon, and then the titanium dioxide-loaded mesoporous carbon is doped into the composite resin matrix, which enhances the wear resistance of the road marking paint and can also decompose harmful substances in the gas under light conditions. The high specific surface area of ​​the titanium dioxide-loaded mesoporous carbon helps to disperse and increase the effective contact between the composite resin and the curing agent. At the same time, the presence of the loaded titanium dioxide and rutile titanium dioxide cooperates with the glass microbeads to improve the reflectivity of the road marking paint and the visibility of the road marking paint at night or in low light environments;

[0023] 3. The silicon-modified nano-alumina used in the present invention increases the wear resistance and hydrophobicity of the road marking paint, prevents dust and the like from adhering to the marking line, and improves the service life and dirt resistance of the road marking paint;

[0024] 4. The road marking paint provided by the present invention has excellent wear resistance, dirt resistance and light reflection, thereby improving the service life of the road marking paint.

[0025] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION

[0026] The present invention is further described below in conjunction with embodiments. Unless otherwise defined, the technical terms or scientific terms used in the present invention should be the common meanings understood by people with ordinary skills in the field to which the present invention belongs. The above-mentioned features or features mentioned in the specific examples mentioned in the present invention can be combined arbitrarily, and these specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0027] Example 1

[0028] The preparation of modified acrylic resin-epoxy resin composite resin comprises the following steps:

[0029] S1, weighing 90 g of modified acrylic resin (dodecafluoroheptyl methacrylate) and 6 g of initiator (TAPA), mixing them evenly to obtain a first solution for standby use;

[0030] S2, weighing 12% of the mass of the modified acrylic resin E-44 epoxy resin and an appropriate amount of chain transfer agent, dissolving them in a solvent, stirring at 60-90° C. under nitrogen protection, to obtain a second solution;

[0031] S3. Slowly add the first solution to the second solution at 125°C, keep the temperature for 1.5 hours after the addition is completed, add 2 g of initiator (TAPA) and continue to keep the temperature at 125°C for 3 hours to obtain dodecafluoroheptyl methacrylate-epoxy composite resin.

[0032] In S3, the amount of epoxy resin added is 12% of the mass of dodecafluoroheptyl methacrylate, and the initiator (TAPA) attacks the aH and H on the tertiary carbon on the epoxy resin molecular chain to become grafting active sites, further generating free radicals to initiate grafting copolymerization.

[0033] Example 2

[0034] The preparation of titanium dioxide-supported mesoporous carbon comprises the following steps:

[0035] S1, dissolving 1.3 g of zinc nitrate hexahydrate and 50 mL of ruthenium acetylacetonate in methanol to obtain a first solution;

[0036] S2, dispersing 3 g of titanium dioxide in methanol to obtain a second dispersion;

[0037] S3, adding the second dispersion in S2 to the first solution in S1, stirring magnetically for 28 hours, washing, centrifuging, and freeze-drying to obtain an intermediate;

[0038] S4. The intermediate in S3 is placed in a tubular furnace, and carbonized and hot-joined at 1000° C. under nitrogen protection to obtain titanium dioxide-supported mesoporous carbon.

[0039] Example 3

[0040] S1. Weigh 90 parts of dodecafluoroheptyl methacrylate-epoxy composite resin, 162 parts of rutile titanium dioxide, glass microspheres and modified nano-alumina, 5 parts of carboxymethyl cellulose, 2 parts of inorganic dispersant, 2 parts of wetting agent polyethylene glycol ether, 2 parts of polysiloxane defoamer, 5 parts of titanium dioxide-loaded mesoporous carbon, 5 parts of additives, and 120 parts of solvent, by mass.

[0041] S2. Put dodecafluoroheptyl methacrylate-epoxy composite resin, triethylamine and deionized water into a reaction kettle, stir at 350 rpm, and add ammonia water, wetting agent polyethylene glycol ether, inorganic dispersant and polysiloxane defoaming agent in sequence to obtain a mixed system.

[0042] S3. Add rutile titanium dioxide, glass microbeads, silicon-modified nano-alumina and titanium dioxide-loaded mesoporous carbon to the mixed system in S2 in small amounts and multiple times, and stir and disperse at 1300 rpm to obtain a dispersed system.

[0043] The mass ratio of the total mass of rutile titanium dioxide, glass microspheres, silicon-modified nano-alumina and titanium dioxide-supported mesoporous carbon to the dodecafluoroheptyl methacrylate-epoxy composite resin is 1.8:1.

[0044] S4. Slowly add deionized water to the dispersed system in S3, stir and mix at 900 rpm, stir and disperse at 1200 rpm, and obtain the road marking paint after sieving.

[0045] When in use, add curing agent XP-2655 (Bayer) with 1.8 times the mass of dodecafluoroheptyl methacrylate-epoxy composite resin, mix and apply it on the road surface, and let it stand to cure.

[0046] Example 4

[0047] S1. Weigh 100 parts of polydimethylsiloxy methacrylate-epoxy composite resin, 200 parts of rutile titanium dioxide, heavy calcium, glass microspheres and modified nano-alumina, 8 parts of carboxymethyl cellulose, 3 parts of amphoteric dispersant, 3 parts of ethylene glycol monobutyl ether, 2 parts of modified silicone defoamer, 3 parts of titanium dioxide-loaded mesoporous carbon, 5 parts of additives, and 150 parts of deionized water, by mass.

[0048] S2. Put polydimethylsiloxy methacrylate-epoxy composite resin, triethylamine and deionized water into a reaction kettle, stir at 350 rpm, and add ammonia water, ethylene glycol monobutyl ether, amphoteric dispersant and modified silicone defoaming agent in sequence to obtain a mixed system.

[0049] S3. Add rutile titanium dioxide, heavy calcium, glass microspheres, silicon-modified nano-alumina and titanium dioxide-loaded mesoporous carbon to the mixed system in S2 in small amounts and in multiple times, and stir and disperse at 1300 rpm to obtain a dispersed system.

[0050] The mass ratio of the total mass of rutile titanium dioxide, heavy calcium, glass microspheres, silicon-modified nano-alumina and titanium dioxide-supported mesoporous carbon to the mass ratio of polydimethylsiloxyalkyl methacrylate-epoxy composite resin is 2:1.

[0051] S4. Slowly add deionized water to the dispersed system in S3, stir and mix at 1000 rpm, stir and disperse at 1200 rpm, and obtain the road marking paint after sieving.

[0052] When in use, add curing agent XP-2655 (Bayer) with 1.8 times the mass of polydimethylsiloxy methacrylate-epoxy composite resin, mix and apply it on the road surface, and let it stand to cure.

[0053] Example 5

[0054] S1. Weigh 80 parts of dodecafluoroheptyl methacrylate-epoxy composite resin, 160 parts of rutile titanium dioxide, heavy calcium, glass microspheres and modified nano-alumina, 5 parts of carboxymethyl cellulose, 1 part of inorganic dispersant, 1 part of polyethylene glycol ether, 1 part of polysiloxane defoamer, 2 parts of titanium dioxide-loaded mesoporous carbon, 5 parts of additives, and 100 parts of deionized water, by mass.

[0055] S2. Put dodecafluoroheptyl methacrylate-epoxy composite resin, triethylamine and deionized water into a reaction kettle, stir at 350 rpm, and add ammonia water, polyethylene glycol ether, inorganic dispersant and polysiloxane defoaming agent in sequence to obtain a mixed system.

[0056] S3. Add rutile titanium dioxide, heavy calcium, glass microspheres, silicon-modified nano-alumina and titanium dioxide-loaded mesoporous carbon to the mixed system in S2 in small amounts and in multiple times, and stir and disperse at 1300 rpm to obtain a dispersed system.

[0057] The mass ratio of the total mass of rutile titanium dioxide, heavy calcium, glass microspheres, silicon-modified nano-alumina and titanium dioxide-supported mesoporous carbon to the mass of dodecafluoroheptyl methacrylate-epoxy composite resin is 2:1.

[0058] S4. Slowly add deionized water to the dispersed system in S3, stir and mix at 1000 rpm, stir and disperse at 1200 rpm, and obtain the road marking paint after sieving.

[0059] When in use, add curing agent XP-2655 (Bayer) with 1.8 times the mass of dodecafluoroheptyl methacrylate-epoxy composite resin, mix and apply it on the road surface, and let it stand to cure.

[0060] Example 6

[0061] S1. Weigh 100 parts of dodecafluoroheptyl methacrylate-epoxy composite resin, 300 parts of rutile titanium dioxide and heavy calcium, 8 parts of carboxymethyl cellulose, 3 parts of amphoteric dispersant, 3 parts of ethylene glycol monobutyl ether, 2 parts of modified silicone defoamer, 3 parts of titanium dioxide-loaded mesoporous carbon, 5 parts of additives, and 150 parts of deionized water by mass.

[0062] S2. Put dodecafluoroheptyl methacrylate-epoxy composite resin, triethylamine and deionized water into a reaction kettle, stir at 350 rpm, and add ammonia water, ethylene glycol monobutyl ether, amphoteric dispersant and modified silicone defoaming agent in sequence to obtain a mixed system.

[0063] S3. Add rutile titanium dioxide, heavy calcium, glass microspheres, silicon-modified nano-alumina and titanium dioxide-loaded mesoporous carbon to the mixed system in S2 in small amounts and in multiple times, and stir and disperse at 1300 rpm to obtain a dispersed system.

[0064] The mass ratio of the total mass of rutile titanium dioxide, heavy calcium, glass microspheres, silicon-modified nano-alumina and titanium dioxide-supported mesoporous carbon to the mass of dodecafluoroheptyl methacrylate-epoxy composite resin is 3:1.

[0065] S4. Slowly add deionized water to the dispersed system in S3, stir and mix at 1000 rpm, stir and disperse at 1200 rpm, and obtain the road marking paint after sieving.

[0066] When in use, add curing agent XP-2655 (Bayer) with 1.8 times the mass of dodecafluoroheptyl methacrylate-epoxy composite resin, mix and apply it on the road surface, and let it stand to cure.

[0067] Comparative Example 1

[0068] S1. Weigh 100 parts of water-based acrylic resin, 200 parts of rutile titanium dioxide, heavy calcium and glass beads, 8 parts of carboxymethyl cellulose, 3 parts of amphoteric dispersant, 3 parts of ethylene glycol monobutyl ether, 2 parts of modified silicone defoamer, and 150 parts of deionized water by mass.

[0069] S2. Put water-based acrylic resin and deionized water into a reaction kettle, stir at 350 rpm, and add ammonia water, ethylene glycol monobutyl ether, amphoteric dispersant and modified silicone defoamer in sequence to obtain a mixed system.

[0070] S3. Add rutile titanium dioxide, heavy calcium and glass beads to the mixed system in S2 in small amounts and in multiple times, and stir and disperse at 1300 rpm to obtain a dispersed system.

[0071] The mass ratio of the total mass of rutile titanium dioxide, heavy calcium and glass microspheres to the water-based acrylic resin is 2:1.

[0072] S4. Slowly add deionized water to the dispersed system in S3, stir and mix at 1000 rpm, stir and disperse at 1200 rpm, and obtain the road marking paint after sieving.

[0073] When using, add curing agent XP-2655 (Bayer) with a mass 1.8 times that of the water-based acrylic resin, mix well, apply on the road surface, and let stand to cure.

[0074] Test Example 1

[0075] The road marking coatings in Examples 3-6 and Comparative Example 1 were respectively applied on the surface of cement-based test blocks, and the road marking coatings obtained after curing were tested.

[0076] a. Wear resistance test

[0077] The wear resistance test was carried out according to GB / T 1768 "Determination of wear resistance of paint film". The wear resistance test of the marking coatings in Examples 3-6 and Comparative Example 1 was carried out using an abrasion tester. The load was set to 1000 g, and the wear value was measured after the rubber grinding wheel reached 200 revolutions. The results are shown in Table 1.

[0078] b. Stain resistance test

[0079] According to GB / T 9780-2013, the stain resistance test of the road marking coating was carried out. Fly ash was selected as the pollution source to prepare a fly ash suspension. The fly ash suspension was applied equally on the road marking coatings in Examples 3-6 and Comparative Example 1. The obtained stain resistance data are shown in Table 1.

[0080] Table 1, Performance data of road marking coating in Examples 3-6 and Comparative Example 1

[0081] Example 3 Example 4 Example 5 Example 6 Comparative Example 1 Wear value mg 8.5 5.6 6.3 4.2 12.7 Stain resistance % 1.8 1.3 3.7 0.9 10.9

[0082] Therefore, the present invention adopts a wear-resistant water-based road marking paint with the above structure and a preparation method thereof, and provides a marking paint with excellent wear resistance, dirt resistance and reflectivity, thereby improving the service life of the marking paint.

[0083] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A wear-resistant water-based road marking paint, characterized in that: The components are calculated by weight as follows: 80-100 parts of composite resin, 120-300 parts of wear-resistant components, 1-10 parts of cellulose, 0.1-5 parts of dispersant, 0.1-5 parts of wetting agent, 0.1-5 parts of defoaming agent, 0.1-5 parts of additives and 100-150 parts of solvent.

2. The wear-resistant water-based road marking paint according to claim 1, characterized in that: The composite resin includes one or more of a polyurethane resin, a modified acrylic resin, and an epoxy resin.

3. The wear-resistant water-based road marking paint according to claim 2, characterized in that: The modified acrylic resin includes one or more of dodecafluoroheptyl methacrylate, polydimethylsiloxy methacrylate and POSS modified acrylic resin.

4. The wear-resistant water-based road marking paint according to claim 1, characterized in that: The wear-resistant component comprises one or more of rutile titanium dioxide, heavy calcium, titanium dioxide-loaded mesoporous carbon, glass microspheres and modified nano-alumina.

5. The wear-resistant water-based road marking paint according to claim 1, characterized in that: The dispersant includes one or more of an inorganic dispersant, an organic dispersant and an amphoteric dispersant; The wetting agent includes one or more of polyethylene glycol ether, ethylene glycol monobutyl ether, alcohol ester and modified silicone.

6. The wear-resistant water-based road marking paint according to claim 1, characterized in that: The additives include one or more of a leveling agent, ammonia water, triethylamine and a silane coupling agent.

7. The wear-resistant water-based road marking paint according to claim 1, characterized in that: The defoaming agent includes one or more of polysiloxane defoaming agents, fatty acid ester defoaming agents, polyether defoaming agents and modified silicone defoaming agents.

8. The wear-resistant water-based road marking paint according to claim 1, characterized in that: The solvent includes one or more of methanol and deionized water.

9. A method for preparing the wear-resistant water-based road marking paint according to any one of claims 1 to 8, characterized in that: The following steps are included: S1. Weigh 80-100 parts of composite resin, 120-300 parts of wear-resistant components, 1-10 parts of cellulose, 0.1-5 parts of dispersant, 0.1-5 parts of wetting agent, 0.1-5 parts of defoaming agent, 0.1-5 parts of additives, and 100-150 parts of solvent by mass; S2, putting the composite resin, part of the additives and part of the solvent into a reaction kettle, stirring at 300-400 rpm, and adding the remaining additives, wetting agent, dispersant and defoaming agent in sequence to obtain a mixed system; S3, adding the wear-resistant component to the mixed system in S2 in small amounts and multiple times, stirring and dispersing at 1000-1500 rpm to obtain a dispersed system; S4. Slowly add the remaining solvent to the dispersed system in S3, stir and mix at 800-1000 rpm, stir and disperse at 1000-1200 rpm, and obtain the road marking paint after sieving.

10. The method for preparing a wear-resistant water-based road marking paint according to claim 9, characterized in that: In S3, the mass ratio of the wear-resistant component to the composite resin is 1-5:1.

Citation Information

Patent Citations

  • POSS (Polyhedral Oligomeric Silsesquioxane) fluorosilicone acrylate-polyurethane blood compatible coating and preparation method thereof

    CN103468120A

  • Long-side-chain fluorine-containing acrylic epoxy resin and coating prepared from resin as raw material

    CN103951773A

  • Electromagnetic shielding composite coating use composition and coating and method

    CN104059464A

  • Low surface energy coating and preparation method thereof

    CN108841322A

  • Quick-drying reflective modified acrylic road marking paint, and preparation method and application thereof

    CN110093083A