Integrated fracturing fluid system and preparation method thereof
By slowly releasing hydrogen ions in the integrated fracturing fluid system, the hydrogen ions are released under high temperatures, the problem of limited use of acid fracturing fluid is solved, the efficiency of oil well mining is improved, and the Reuse of resources.
Patent Information
- Application Number
- CN202410912721.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing acid fracturing fluid has limited depth of use in high-temperature wells, and the chemical acid binding effect is poor, resulting in a reduced oil well mining efficiency.
Adopt an integrated fracturing liquid system, including acid liquid, hydrogen ion sustained-release particles, polyvinyl alcohol, acrylamide and other components. The hydrogen ion sustained-release particles slowly release hydrogen ions at high temperatures, and combine polyvinyl alcohol and other components to form Stable fracturing liquid and the recycling of cation exchange resin is achieved through nano iron powder.
It extends the depth of use of acid fracturing fluid, improves the oil well mining efficiency, saves the use of hydrogen ion sustained-release particles, and realizes the reuse of resources, ensuring the normal fracturing operation in the deep oil well.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of petroleum exploitation fracturing fluid, in particular to an integrated fracturing fluid system and a preparation method thereof. Background Art
[0002] Oil is the "blood" of modern industry, and its processed products are indispensable energy or raw materials in modern industrial production and daily life. However, during the oil well exploitation process, the exploitation efficiency will continue to decrease with the continuous increase of exploitation time. At present, in order to improve the oil production efficiency of oil wells, acid fracturing fluid is used to improve the oil production efficiency. However, due to the high downhole temperature during the long-term drilling and oil production process of oil wells, the reaction rate of acid fracturing fluid and carbonate rock is greatly accelerated, resulting in the current limited use depth of acid fracturing fluid. At the same time, the current "acid binding" operation of hydrogen ions by chemical means is also in general effect at the highest downhole temperature of nearly 200°C. Summary of the invention
[0003] The present invention provides an integrated fracturing fluid system and a preparation method thereof, so as to solve the defects in the prior art.
[0004] The present invention is achieved through the following technical solutions:
[0005] The integrated fracturing fluid system comprises the following substances in parts by weight: 50-60 parts of acid solution; 0-30 parts of hydrogen ion slow-release particles; 0.4-0.8 parts of polyvinyl alcohol; 0.2-0.4 parts of acrylamide; 0.3-0.7 parts of tetraisopropyl titanate; 0.2-0.4 parts of ethylenediaminetetraacetic acid; 0.3-0.5 parts of diethylenetriaminepentaacetic acid; 0.1-0.3 parts of polymaleic anhydride; 0.5-0.9 parts of aramid fiber particles; 0.2-0.4 parts of copper lactate; 0.2-0.4 parts of triethylammonium chloride; 0.2-0.4 parts of dodecyldimethylammonium chloride; and 0.1-0.2 parts of alkylphenol polyoxyethylene ether.
[0006] In the integrated fracturing fluid system as described above, the acid liquid is a hydrochloric acid solution with a concentration of 15-25%.
[0007] In the integrated fracturing fluid system as described above, the molecular weight of the polyvinyl alcohol is 30,000-50,000.
[0008] In the integrated fracturing fluid system as described above, the aramid fiber particles are sieved through a 200-mesh sieve for later use.
[0009] In the integrated fracturing fluid system as described above, the hydrogen ion slow-release particles include the following substances by weight: 60-80 parts of cation exchange resin particles that adsorb hydrogen ions; and 100-120 parts of waterborne polyurethane resin.
[0010] In the integrated fracturing fluid system as described above, the cation exchange resin is a hydroxy type cation exchange resin.
[0011] In the integrated fracturing fluid system as described above, the waterborne polyurethane resin is a polyether polyurethane, and the molecular weight of the polyether polyurethane is 1000-4000.
[0012] The integrated fracturing fluid system as described above, the method for preparing the hydrogen ion slow-release particles comprises the following steps:
[0013] Step 1: soak the cation exchange resin particles in a hydrochloric acid solution with a concentration of 35%, fully stir and mix at a stirring speed of 100-120 r / min for 3-5 hours, and then filter out the cation exchange resin particles that adsorb hydrogen ions for use;
[0014] Step 2: The cation exchange resin particles for hydrogen ion absorption obtained in step 1 are weighed and sealed for storage, then the waterborne polyurethane resin is weighed according to the ratio, and then the waterborne polyurethane resin is sent to a sealed mixer for heating and melting, and then the cation exchange resin particles for hydrogen ion absorption are added and sealed and mixed for 3-5 minutes at a stirring speed of 200-250r / min, and then sent to an extruder for granulation and cooled to room temperature;
[0015] Step 3: The granules obtained in step 2 are crushed and passed through a 50-mesh sieve to obtain hydrogen ion sustained-release granules, which are quickly sealed and stored.
[0016] In the integrated fracturing fluid system as described above, the particle size of the cation exchange resin in step 1 is 10-50 μm.
[0017] In the integrated fracturing fluid system as described above, the mass volume ratio of the cation exchange resin to the 35% hydrochloric acid solution in step 1 is 1:1.
[0018] In the integrated fracturing fluid system as described above, the cation exchange resin particles in step 1 contain 10-15% of nano-scale iron powder.
[0019] The preparation method of the integrated fracturing fluid system comprises the following steps:
[0020] Step 1: weigh hydrochloric acid solution, polyvinyl alcohol, acrylamide, tetraisopropyl titanate, ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, polymaleic anhydride, aramid fiber particles, copper lactate, triethylammonium chloride, dodecyldimethylammonium chloride, and alkylphenol polyoxyethylene ether according to the ratio;
[0021] Step 2: Add hydrochloric acid solution, polyvinyl alcohol, acrylamide, tetraisopropyl titanate, ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, polymaleic anhydride, aramid fiber particles, copper lactate, triethylammonium chloride, dodecyldimethylammonium chloride, and alkylphenol polyoxyethylene ether into a sealed reactor, heat to 40-60° C., stir at a stirring speed of 140-160 r / min for 1-2 hours, mix thoroughly, and then seal and store;
[0022] Step 3: When using, weigh the hydrogen ion slow-release particles according to the ratio and add them to the mixed solution in step 2. Stir for 30-50 minutes at a stirring speed of 140-160 r / min and then send it into the oil well for use as a fracturing fluid.
[0023] The advantages of the present invention are:
[0024] The present invention selects the amount of hydrogen ion slow-release particles added in the fracturing fluid system according to the actual production depth of the oil well, thereby ensuring the use depth of the acid fracturing fluid and effectively saving the use amount of hydrogen ion slow-release particles;
[0025] The hydrogen ion slow-release particles in the present invention include cation exchange resin particles that absorb hydrogen ions and water-based polyurethane resin. The cation exchange resin particles that absorb hydrogen ions can absorb calcium ions and release hydrogen ions after entering the solution, thereby reacting with carbonate rocks to achieve fracturing operations. At the same time, the water-based polyurethane resin can be slowly hydrolyzed at a higher temperature so that it can be hydrolyzed and released only after reaching the depth of the oil well. The cation exchange resin particles that absorb hydrogen ions absorb calcium ions in the solution and release hydrogen ions. At the same time, the molecular weight of the water-based polyurethane resin can be selected according to the depth of the oil well. The molecular weight will affect the hydrolysis rate of the water-based polyurethane resin. The larger the molecular weight, the slower the hydrolysis rate of the water-based polyurethane resin, thereby ensuring the normal fracturing operation in the deep of the oil well.
[0026] The cation exchange resin particles of the present invention contain a certain amount of nano iron powder, which can be recycled by magnetic attraction in subsequent operations, thereby realizing the recovery of the cation exchange resin particles, and then can be reused after eluting to remove calcium ions, thereby effectively saving resources and realizing the reuse of resources. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] The method for preparing the integrated fracturing fluid system comprises the following steps:
[0030] Step 1: Weigh 600g of 15% hydrochloric acid solution; 4g of polyvinyl alcohol with a molecular weight of 30000-35000; 2g of acrylamide; 3g of tetraisopropyl titanate; 2g of ethylenediaminetetraacetic acid; 3g of diethylenetriaminepentaacetic acid; 1g of polymaleic anhydride; 5g of aramid fiber particles (sieved through a 200-mesh sieve for later use); 2g of copper lactate; 2g of triethylammonium chloride; 2g of dodecyldimethylammonium chloride; 1g of alkylphenol polyoxyethylene ether;
[0031] Step 2: Add 15% hydrochloric acid solution, polyvinyl alcohol with a molecular weight of 30,000-35,000, acrylamide, tetraisopropyl titanate, ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, polymaleic anhydride, aramid fiber particles (sieved through a 200-mesh sieve for later use), copper lactate, triethylammonium chloride, dodecyldimethylammonium chloride, and alkylphenol polyoxyethylene ether into a sealed reactor, heat to 40°C, stir at a stirring speed of 140 r / min for 2 hours, mix thoroughly, and then seal and store.
[0032] Example 2
[0033] The method for preparing hydrogen ion sustained-release particles comprises the following steps:
[0034] Step 1: soaking hydroxyl cation exchange resin particles (particle size of 10-20 μm, containing 10% nano-iron powder) in a 35% hydrochloric acid solution, stirring and mixing at a stirring speed of 100 r / min for 3.5 hours, and then filtering out the cation exchange resin particles that adsorb hydrogen ions for use;
[0035] Step 2: The hydroxyl type cation exchange resin particles for hydrogen ion absorption obtained in step 1 are weighed to 600 g and then sealed and stored; then, 1000 g of polyether polyurethane with a molecular weight of 1000-1500 is weighed according to the ratio, and then the polyether polyurethane is sent into a sealed mixer for heating and melting, and then the cation exchange resin particles for hydrogen ion absorption are added and sealed and mixed for 5 minutes at a stirring speed of 200 r / min, and then sent into an extruder for granulation and cooled to room temperature;
[0036] Step 3: The granules obtained in step 2 are crushed and passed through a 50-mesh sieve to obtain hydrogen ion sustained-release granules, which are quickly sealed and stored.
[0037] The method for preparing the integrated fracturing fluid system comprises the following steps:
[0038] Step 1: Weigh 600g of 15% hydrochloric acid solution; 4g of polyvinyl alcohol with a molecular weight of 30000-35000; 2g of acrylamide; 3g of tetraisopropyl titanate; 2g of ethylenediaminetetraacetic acid; 3g of diethylenetriaminepentaacetic acid; 1g of polymaleic anhydride; 5g of aramid fiber particles (sieved through a 200-mesh sieve for later use); 2g of copper lactate; 2g of triethylammonium chloride; 2g of dodecyldimethylammonium chloride; 1g of alkylphenol polyoxyethylene ether;
[0039] Step 2: Add 15% hydrochloric acid solution, polyvinyl alcohol with a molecular weight of 30,000-35,000, acrylamide, tetraisopropyl titanate, ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, polymaleic anhydride, aramid fiber particles (sieved through a 200 mesh sieve for later use), copper lactate, triethylammonium chloride, dodecyldimethylammonium chloride, and alkylphenol polyoxyethylene ether into a sealed reactor, heat to 45°C, stir at a stirring speed of 145 r / min for 1.8 hours, mix thoroughly, and then seal and store.
[0040] Step 3: Weigh 100 g of hydrogen ion sustained-release particles and add them to the mixed solution in step 2. Stir for 50 minutes at a stirring speed of 140 r / min, then seal and store for later use.
[0041] Example 3
[0042] The method for preparing hydrogen ion sustained-release particles comprises the following steps:
[0043] Step 1: Soak hydroxyl cation exchange resin particles (particle size of 40-50 μm, containing 15% nano-grade iron powder) in a 35% hydrochloric acid solution, fully stir and mix at a stirring speed of 120 r / min for 3 hours, and then filter out the cation exchange resin particles that adsorb hydrogen ions for later use;
[0044] Step 2: 800 g of the hydroxyl type cation exchange resin particles for hydrogen ion absorption obtained in step 1 are weighed and sealed for storage, and then 1200 g of polyether polyurethane with a molecular weight of 3000-4000 is weighed, and then the polyether polyurethane is sent into a sealed mixer for heating and melting, and then the cation exchange resin particles for hydrogen ion absorption are added and sealed and mixed for 3 minutes at a stirring speed of 250 r / min, and then sent into an extruder for granulation and cooled to room temperature;
[0045] Step 3: The granules obtained in step 2 are crushed and passed through a 50-mesh sieve to obtain hydrogen ion sustained-release granules, which are quickly sealed and stored.
[0046] The method for preparing the integrated fracturing fluid system comprises the following steps:
[0047] Step 1: according to the ratio, weigh 500g of 25% hydrochloric acid solution; 8g of polyvinyl alcohol with a molecular weight of 40000-50000; 4g of acrylamide; 7g of tetraisopropyl titanate; 4g of ethylenediaminetetraacetic acid; 5g of diethylenetriaminepentaacetic acid; 3g of polymaleic anhydride; 9g of aramid fiber particles (sieved through a 200-mesh sieve for later use); 4g of copper lactate; 4g of triethylammonium chloride; 4g of dodecyldimethylammonium chloride; 2g of alkylphenol polyoxyethylene ether;
[0048] Step 2: Add 25% hydrochloric acid solution, polyvinyl alcohol with a molecular weight of 40,000-50,000, acrylamide, tetraisopropyl titanate, ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, polymaleic anhydride, aramid fiber particles (passed through a 200 mesh sieve for standby use), copper lactate, triethylammonium chloride, dodecyldimethylammonium chloride, and alkylphenol polyoxyethylene ether into a sealed reactor, heat to 60° C., stir at a stirring speed of 160 r / min for 1 h, mix thoroughly, and then seal and store;
[0049] Step 3: Weigh 300 g of hydrogen ion sustained-release particles and add them to the mixed solution in step 2. Stir for 30 minutes at a stirring speed of 160 r / min, then seal and store for later use.
[0050] Example 4
[0051] The method for preparing hydrogen ion sustained-release particles comprises the following steps:
[0052] Step 1: Soak hydroxyl cation exchange resin particles (particle size of 20-30 μm, containing 13% nano-iron powder) in a 35% hydrochloric acid solution, fully stir and mix at a stirring speed of 110 r / min for 4 hours, and then filter out the cation exchange resin particles that adsorb hydrogen ions for later use;
[0053] Step 2: Weigh 700 g of the hydroxyl type cation exchange resin particles for hydrogen ion absorption obtained in step 1 and seal them for storage, then weigh 1100 g of polyether polyurethane with a molecular weight of 2000-3000, then send the polyether polyurethane into a sealed mixer for heating and melting, then add the cation exchange resin particles for hydrogen ion absorption and seal and mix them at a stirring speed of 230 r / min for 4 minutes, then send them into an extruder for granulation and cool them to room temperature;
[0054] Step 3: The granules obtained in step 2 are crushed and passed through a 50-mesh sieve to obtain hydrogen ion sustained-release granules, which are quickly sealed and stored.
[0055] The method for preparing the integrated fracturing fluid system comprises the following steps:
[0056] Step 1: weigh 550g of 20% hydrochloric acid solution; 6g of polyvinyl alcohol with a molecular weight of 35000-40000; 3g of acrylamide; 5g of tetraisopropyl titanate; 3g of ethylenediaminetetraacetic acid; 4g of diethylenetriaminepentaacetic acid; 2g of polymaleic anhydride; 7g of aramid fiber particles (sieved through a 200-mesh sieve for later use); 3g of copper lactate; 3g of triethylammonium chloride; 3g of dodecyldimethylammonium chloride; 1.5g of alkylphenol polyoxyethylene ether;
[0057] Step 2: Add 20% hydrochloric acid solution, polyvinyl alcohol with a molecular weight of 35000-40000, acrylamide, tetraisopropyl titanate, ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, polymaleic anhydride, aramid fiber particles (sieved through a 200 mesh sieve for standby use), copper lactate, triethylammonium chloride, dodecyldimethylammonium chloride, and alkylphenol polyoxyethylene ether into a sealed reactor, heat to 50° C., stir at a stirring speed of 150 r / min for 1.5 h, mix thoroughly, and then seal and store;
[0058] Step 3: Weigh 200 g of hydrogen ion sustained-release particles and add them to the mixed solution in step 2. Stir for 40 minutes at a stirring speed of 150 r / min, then seal and store for later use.
[0059] The hydrogen ion slow-release particles prepared in Examples 2-4 were respectively added into boiling water at 100°C, and then the hydrolysis of the polyether polyurethane was observed. The results were as follows: the hydrogen ion slow-release particles prepared in Example 2 had hydroxyl cation exchange resin particles that adsorbed hydrogen ions released after 2.4 hours of heating, and the hydroxyl cation exchange resin particles that adsorbed hydrogen ions were completely released after 18.7 hours; the hydrogen ion slow-release particles prepared in Example 3 had hydroxyl cation exchange resin particles that adsorbed hydrogen ions released after 4.2 hours of heating, and the hydroxyl cation exchange resin particles that adsorbed hydrogen ions were completely released after 26.3 hours; the hydrogen ion slow-release particles prepared in Example 4 had hydroxyl cation exchange resin particles that adsorbed hydrogen ions released after 3.7 hours of heating, and the hydroxyl cation exchange resin particles that adsorbed hydrogen ions were completely released after 21.2 hours.
[0060] From the above test results, it can be known that the hydrogen ion slow-release particles in the present invention can slowly release hydroxyl type cation exchange resin particles over a long period of time and then release hydrogen ions by absorbing calcium ions, thereby being able to conveniently complete the fracturing operation deep underground, and the density of the hydrogen ion slow-release particles is greater than the density of water, thereby being able to penetrate deep into the oil well to ensure the normal fracturing operation deep in the oil well, and at the same time, whether to add hydrogen ion slow-release particles, and the amount of hydrogen ion slow-release particles added and the corresponding molecular weight of polyether polyurethane can be selected according to the depth of the oil well and other factors to ensure the normal fracturing operation deep in the oil well.
[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. An integrated fracturing fluid system, characterized in that: The invention comprises the following substances in parts by weight: 50-60 parts of acid solution; 0-30 parts of hydrogen ion sustained-release particles; 0.4-0.8 parts of polyvinyl alcohol; 0.2-0.4 parts of acrylamide; 0.3-0.7 parts of tetraisopropyl titanate; 0.2-0.4 parts of ethylenediaminetetraacetic acid; 0.3-0.5 parts of diethylenetriaminepentaacetic acid; 0.1-0.3 parts of polymaleic anhydride; 0.5-0.9 parts of aramid fiber particles; 0.2-0.4 parts of copper lactate; 0.2-0.4 parts of triethylammonium chloride; 0.2-0.4 parts of dodecyldimethylammonium chloride; and 0.1-0.2 parts of alkylphenol polyoxyethylene ether.
2. The integrated fracturing fluid system according to claim 1, characterized in that: The acid solution is a hydrochloric acid solution with a concentration of 15-25%.
3. The integrated fracturing fluid system according to claim 1, characterized in that: The molecular weight of the polyvinyl alcohol is 30,000-50,000.
4. The integrated fracturing fluid system according to claim 1, characterized in that: The aramid fiber particles are sieved through a 200-mesh sieve for later use.
5. The integrated fracturing fluid system according to claim 1, characterized in that: The hydrogen ion slow-release particles include the following substances by weight: 60-80 parts of cation exchange resin particles for adsorbing hydrogen ions; and 100-120 parts of waterborne polyurethane resin.
6. The integrated fracturing fluid system according to claim 5, characterized in that: The cation exchange resin is a hydroxy type cation exchange resin.
7. The integrated fracturing fluid system according to claim 5, characterized in that: The waterborne polyurethane resin is a polyether polyurethane, and the molecular weight of the polyether polyurethane is 1000-4000.
8. The integrated fracturing fluid system according to claim 5, characterized in that: The preparation method of the hydrogen ion sustained-release particles comprises the following steps: Step 1: soak the cation exchange resin particles in a hydrochloric acid solution with a concentration of 35%, fully stir and mix at a stirring speed of 100-120 r / min for 3-5 hours, and then filter out the cation exchange resin particles that adsorb hydrogen ions for use; Step 2: The cation exchange resin particles for hydrogen ion absorption obtained in step 1 are weighed and sealed for storage, then the waterborne polyurethane resin is weighed according to the ratio, and then the waterborne polyurethane resin is sent to a sealed mixer for heating and melting, and then the cation exchange resin particles for hydrogen ion absorption are added and sealed and mixed for 3-5 minutes at a stirring speed of 200-250r / min, and then sent to an extruder for granulation and cooled to room temperature; Step 3: The granules obtained in step 2 are crushed and passed through a 50-mesh sieve to obtain hydrogen ion sustained-release granules, which are quickly sealed and stored.
9. The integrated fracturing fluid system according to claim 8, characterized in that: The particle size of the cation exchange resin in step 1 is 10-50 μm; In the step 1, the mass volume ratio of the cation exchange resin to the 35% hydrochloric acid solution is 1:1; The cation exchange resin particles in step 1 contain 10-15% of nano-scale iron powder.
10. A method for preparing an integrated fracturing fluid system, characterized in that: The steps include: Step 1: weigh hydrochloric acid solution, polyvinyl alcohol, acrylamide, tetraisopropyl titanate, ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, polymaleic anhydride, aramid fiber particles, copper lactate, triethylammonium chloride, dodecyldimethylammonium chloride, and alkylphenol polyoxyethylene ether according to the ratio; Step 2: Add hydrochloric acid solution, polyvinyl alcohol, acrylamide, tetraisopropyl titanate, ethylenediaminetetraacetic acid, diethylenetriaminepentaacetic acid, polymaleic anhydride, aramid fiber particles, copper lactate, triethylammonium chloride, dodecyldimethylammonium chloride, and alkylphenol polyoxyethylene ether into a sealed reactor, heat to 40-60° C., stir at a stirring speed of 140-160 r / min for 1-2 hours, mix thoroughly, and then seal and store; Step 3: When using, weigh the hydrogen ion slow-release particles according to the ratio and add them to the mixed solution in step 2. Stir for 30-50 minutes at a stirring speed of 140-160 r / min and then send it into the oil well for use as a fracturing fluid.